A quick-drying magnetic ink and its preparation method and application in chip production
By surface modification of nano iron tetraoxide and combining it with modified polyurethane acrylate, a multiple curing system is formed, which solves the problems of poor dispersion and low curing rate of iron tetraoxide, and improves the dispersion and curing speed of magnetic inks , improves the separation and screening efficiency and the comprehensive performance of ink in chip production.
Patent Information
- Application Number
- CN202411223149.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-09-03
AI Technical Summary
The poor dispersion of iron tetroxide in existing magnetic inks leads to layering and low curing rate, which limits its application and separation and screening efficiency in chip production.
By surface modification of nano iron tritetroxide, grafting vinyl silane coupling agent and trimethylolpropane tris(3-mercaptopropionate), and combining with modified polyurethane acrylate, photoinitiator, etc., Form a multiple curing system to improve dispersion and curing speed.
It significantly improves the dispersion and compatibility of nano iron tetroxide in ink, shortens the curing time of ink, improves the efficiency of chip separation and screening and the comprehensive performance of ink.
Smart Images

Figure CN118725640B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of inks, and in particular to a quick-drying magnetic ink and a preparation method thereof and application thereof in chip production. Background Art
[0002] Magnetic ink is a type of functional ink. By adding magnetic fillers to the ink matrix, the ink becomes magnetic. Ferroferric oxide, as a substance with good magnetic properties, is often added to the ink matrix as a magnetic filler to give the ink magnetism. However, as an inorganic filler, ferroferric oxide has poor dispersibility in organic polymer resins, and the resulting magnetic ink is prone to stratification. In addition, due to the presence of ferroferric oxide particles, the curing rate of the light-shielding part of the magnetic ink is low during UV curing.
[0003] During the chip manufacturing process, defective products may appear due to operational problems or the characteristics of the material itself. It is usually necessary to mark the defective products for separation and screening. The separation and screening technology used in the prior art is time-consuming and labor-intensive, and is not conducive to mass production.
[0004] Prior art, such as Chinese patent application CN111808472A, discloses a fast-curing UV water-based magnetic ink and a preparation method thereof, wherein a polyacrylic acid polymer is prepared, and the polyacrylic acid polymer is reacted with at least one of hydroxyethyl methacrylate, glycidyl methacrylate and acrylic acid under the action of triethylamine under the action of phenol inhibition to obtain a prepolymer, and ferroferric oxide is added as a magnetic filler to obtain a magnetic ink, and the curing speed of the ink is accelerated due to the multiple effects of the olefinic bonds of the polyene functional monomer and the olefinic bonds of the prepolymer, the cross-linking reaction of the amino group with the carboxyl group, and the cross-linking reaction of the amino group with the epoxy group. However, the magnetic filler ferroferric oxide used has not been subjected to surface modification treatment, and the ferroferric oxide has poor dispersibility in the ink, is easy to agglomerate, and the ink is prone to stratification, which limits the application of the material. Summary of the invention
[0005] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a quick-drying magnetic ink and a preparation method thereof and an application in chip production. The magnetic ink can be quickly cured and has excellent comprehensive performance and magnetic separation performance. After printing it on a chip, it is beneficial to the separation and screening of the chip.
[0006] In order to achieve the above object, the technical solution adopted by the present invention is as follows: a method for preparing a quick-drying magnetic ink, comprising the following steps:
[0007] Step 1, preparing mercapto nano-iron tetroxide and silane-modified epoxy resin; wherein the preparation of mercapto nano-iron tetroxide comprises the following steps: step (1), mixing vinyl trimethoxysilane, nano-iron tetroxide, and ethanol aqueous solution, ultrasonically dispersing, adding a regulator to adjust the pH value, reacting, filtering, washing, and drying after the reaction is completed to obtain alkenyl nano-iron tetroxide; step (2), mixing alkenyl nano-iron tetroxide, trimethylolpropane tris (3-mercaptopropionate), and toluene, ultrasonically dispersing, reacting, filtering, washing, and drying after the reaction is completed to obtain mercapto nano-iron tetroxide; wherein the silane-modified epoxy resin The preparation of the resin comprises the following steps: step (1), mixing phenol, phosphotungstic acid and thioglycolic acid evenly, adding acrolein dropwise, reacting after the addition is complete, adding a regulator to adjust the pH value after the reaction is complete, removing excess phenol by rotary evaporation to obtain a bisphenol intermediate; step (2), mixing the bisphenol intermediate, epichlorohydrin and tetrabutylammonium chloride, reacting, cooling after the reaction is complete, adding potassium hydroxide aqueous solution dropwise, continuing the reaction after the addition is complete, purifying after the reaction is complete, and obtaining an alkenyl epoxy resin; mixing cyclohexylaminopropyltrimethoxysilane, an alkenyl epoxy resin and lithium bromide, reacting, and obtaining a silane-modified epoxy resin after the reaction is complete;
[0008] Step 2: Mix silane-modified epoxy resin, 1,4-butanediol, isophorone diisocyanate, dibutyltin dilaurate and acetone, react, add alkenyl polyether and bisphenol fluorene after the reaction, continue the reaction, add hydroxyethyl methacrylate after the reaction, react again, and remove the solvent acetone by rotary evaporation after the reaction to obtain modified polyurethane acrylate; the preparation of alkenyl polyether includes the following steps: mix polytetrahydrofuran ether glycol and dichloroethane, add trifluoroacetic acid and tin tetrachloride in sequence, add a mixture of glycidyl methacrylate and p-methoxyphenol dropwise, react after the addition is complete, purify after the reaction to obtain alkenyl polyether; mix modified polyurethane acrylate, mercapto nano-ferric tetroxide, trimethylolpropane triacrylate, additives and photoinitiator, stir to obtain quick-drying magnetic ink.
[0009] Preferably, when preparing mercapto nano-ferroferric oxide in step 1, in step (1), the mass ratio of vinyltrimethoxysilane, nano-ferroferric oxide and ethanol aqueous solution is 10: (0.8-1): (180-200), and the ethanol aqueous solution is 50 vol% ethanol aqueous solution; the reaction conditions are: reacting at a pH value of 9.5-10 and a temperature of 40-50° C. for 3-4 hours.
[0010] Preferably, the conditioning agent comprises 28 wt % ammonia water.
[0011] Preferably, when preparing the mercapto nano-ferroferric oxide in step 1, in step (2), the mass ratio of alkenyl nano-ferroferric oxide, trimethylolpropane tris(3-mercaptopropionate) and toluene is 10:(50-55):(180-200); and the reaction conditions are: reacting for 16-20 hours at room temperature under ultraviolet light irradiation with a wavelength of 365 nm.
[0012] Preferably, when preparing the silane-modified epoxy resin in step 1, in step (1), the mass ratio of phenol, acrolein, phosphotungstic acid and thioglycolic acid is (26-26.5): (2.2-2.3): (0.15-0.16): (0.15-0.16); the dripping condition of acrolein is: dripping at a temperature of 45-50°C for 20-30min; the reaction conditions are: reacting at a temperature of 50-60°C for 6-8h.
[0013] Preferably, the regulator includes 0.1 mol / L sodium hydroxide aqueous solution, and the pH value after adjustment is neutral.
[0014] Preferably, when preparing the silane-modified epoxy resin in step 1, in step (2), the mass ratio of the bisphenol intermediate, epichlorohydrin, tetrabutylammonium chloride and potassium hydroxide aqueous solution is 25: (90-95): (1.5-1.6): (77-80), the potassium hydroxide aqueous solution is a 40wt% potassium hydroxide aqueous solution; the reaction conditions are: reacting at a temperature of 100-120°C for 24-26h; the potassium hydroxide aqueous solution is added dropwise at a temperature of 0°C for 30-40min; and the reaction is continued at a temperature of 0-2°C for 30-40min.
[0015] Preferably, the purification operation includes: liquid separation, taking the organic phase, adding dichloromethane 4-6 times the mass of the organic phase to dissolve and dilute, then adding water 4-6 times the mass of the organic phase to wash, liquid separation to obtain the washed organic phase, and rotary evaporation at 30-35°C to remove the solvent dichloromethane.
[0016] Preferably, when preparing the silane-modified epoxy resin in step 1, in step (2), the mass ratio of cyclohexylaminopropyltrimethoxysilane, alkenyl epoxy resin and lithium bromide is (9-9.5):15:(0.4-0.5); when preparing the silane-modified epoxy resin, the reaction conditions are: stirring the reaction at room temperature in a nitrogen atmosphere for 48-50 hours.
[0017] Preferably, in the step 2, the mass ratio of silane-modified epoxy resin, 1,4-butanediol, isophorone diisocyanate, alkenyl polyether, bisphenol fluorene, hydroxyethyl methacrylate, dibutyltin dilaurate and acetone is (20-22): (20-30): 80: (110-120): (5-6): (22-25): (0.04-0.05): (100-120); the reaction conditions are: reacting for 3-4 hours at a temperature of 70-80°C in a nitrogen atmosphere; continuing the reaction conditions are: continuing the reaction for 5-6 hours at a temperature of 55-65°C in a nitrogen atmosphere; and re-reacting for 1-2 hours in a nitrogen atmosphere at a temperature of 55-65°C.
[0018] Preferably, in the step 2 for preparing alkenyl polyether, the mass ratio of polytetramethylene glycol, glycidyl methacrylate, ethylene dichloride, trifluoroacetic acid, tin tetrachloride and p-methoxyphenol is 290: (28-30): (320-350): (0.28-0.3): (0.28-0.3): 0.02; the dripping conditions of the mixture of glycidyl methacrylate and p-methoxyphenol are: dripping at a temperature of 70-80°C for 0.5-1h; the reaction conditions are: reacting at a temperature of 70-80°C for 1-2h in a nitrogen atmosphere.
[0019] Preferably, the purification operation comprises: adding water in an amount 2-3 times the mass of the crude reaction product to the crude reaction product obtained after the reaction, then adding a 0.1 mol / L potassium hydroxide aqueous solution to adjust the pH value to neutral, filtering, taking the filtrate, adding acetone and water in an amount 3-4 times the mass of the filtrate in turn for washing, separating the liquids, taking the organic phase, and removing the solvent by rotary evaporation at a temperature of 70-80°C.
[0020] Preferably, in step 2, the mass ratio of modified polyurethane acrylate, mercapto nano-ferric oxide, trimethylolpropane triacrylate, additive and photoinitiator is 80: (30-35): (35-40): (2-3): (5-6), and the additive is prepared by mixing a defoamer and a leveling agent in a mass ratio of 1:1.
[0021] Preferably, a quick-drying magnetic ink is prepared by the method for preparing the quick-drying magnetic ink as described above.
[0022] Preferably, an application of the quick-drying magnetic ink as described above in chip production.
[0023] Compared with the prior art, the invention has the following beneficial effects: in the quick-drying magnetic ink prepared by the invention, the surface of nano-ferroferric oxide is modified to obtain mercapto nano-ferroferric oxide, which is mixed with modified polyurethane acrylate, photoinitiator, additives, etc., thereby improving the dispersibility and compatibility of the nano-ferroferric oxide in the ink, improving the magnetic properties of the ink, and facilitating the separation and screening of the chip after printing on the chip.
[0024] The invention uses vinyl trimethoxysilane to modify the surface of nano ferroferric oxide to obtain alkenyl nano ferroferric oxide, and the vinyl groups on the surface of the nano ferroferric oxide undergo a mercapto-ene click chemical reaction with mercapto groups under light conditions, so that trimethylolpropane tris(3-mercaptopropionate) is grafted on the surface of the nano ferroferric oxide, thereby improving the dispersibility of the nano ferroferric oxide in ink. Moreover, since trimethylolpropane tris(3-mercaptopropionate) has a multi-mercapto functional group structure, the surface of the obtained mercapto nano ferroferric oxide has a large number of mercapto functional groups. The mercapto nano ferroferric oxide is added to the ink as a magnetic filler, and the mercapto functional groups can participate in the ultraviolet curing process of the ink and interact with organic polymer resins in the ink. The carbon-carbon double bonds in the lipid-modified polyurethane acrylate undergo click chemical reaction, which reduces the oxygen inhibition effect in the ink light curing process, accelerates the curing speed of the ink, and further improves the dispersibility and compatibility of nano-ferroferric oxide in the ink; the present invention utilizes phenol and acrolein to undergo a condensation reaction under catalyst conditions to obtain a bisphenol intermediate with a carbon-carbon double bond in the side chain, which is reacted with epichlorohydrin to obtain a bisphenol-type alkenyl epoxy resin with a carbon-carbon double bond in the side chain, and a secondary amine group of cyclohexylaminopropyltrimethoxysilane undergoes a ring-opening reaction with an epoxy group of the alkenyl epoxy resin to graft a siloxane segment into the alkenyl epoxy resin. The obtained silane-modified epoxy resin can be used as a polyol. Hydroxyl compounds are introduced into the polyurethane acrylate system, and the active groups in the silane-modified epoxy resin can react with the isocyanate groups of the polyurethane, thereby introducing siloxane segments, carbon-carbon double bonds, and epoxy resin structures into the polyurethane acrylate resin, thereby increasing the crosslinking degree of the resin and improving the comprehensive properties of the ink; the present invention mixes polytetramethylene ether diol with glycidyl methacrylate, and introduces carbon-carbon double bonds into the side chains of polytetramethylene ether diol through a ring-opening reaction between hydroxyl groups and epoxy groups to obtain alkenyl polyether; reacts the silane-modified epoxy resin, alkenyl polyether, bisphenol fluorene, 1,4-butanediol, and isophorone diisocyanate under catalyst conditions, and reacts the methyl acrylate through a ring-opening reaction between methyl acrylate and polytetramethylene ether diol; The modified polyurethane acrylate is capped with hydroxyethyl olefinate to obtain modified polyurethane acrylate; the modified polyurethane acrylate is mixed with mercapto nano-ferroferric oxide, a photoinitiator, an additive, etc. to obtain a quick-drying magnetic ink; wherein, the siloxane segment in the silane-modified epoxy resin can improve the water resistance of the ink, and the epoxy resin structure can improve the comprehensive performance of the ink; both the alkenyl polyether and the silane-modified epoxy resin contain carbon-carbon double bonds as side chain groups, which can not only undergo free radical polymerization during the photocuring process, but also undergo click chemical reaction with the mercapto group of the mercapto nano-ferroferric oxide, so that the prepared quick-drying magnetic ink has a multiple curing system, thereby improving the curing speed and comprehensive performance of the ink. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 It is a process flow chart for preparing quick-drying magnetic ink in the present invention;
[0026] Figure 2It is a bar graph of actual drying time of Examples 1-5 and Comparative Examples 1-2 in the comprehensive performance test of the present invention. DETAILED DESCRIPTION
[0027] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0028] Example 1
[0029] This embodiment discloses a method for preparing a quick-drying magnetic ink, comprising the following steps:
[0030] Step 1, preparing mercapto nano-ferroferric oxide and silane-modified epoxy resin; wherein the preparation of mercapto nano-ferroferric oxide comprises the following steps: step (1), mixing vinyl trimethoxysilane, nano-ferroferric oxide, and 50 vol% ethanol aqueous solution in a mass ratio of 10:0.9:190, ultrasonically dispersing for 25 minutes, adding 28 wt% ammonia water to adjust the pH value to 9.5, reacting at 45°C for 3.5 hours, filtering after the reaction, taking the filter cake, adding ethanol 6 times the mass of the filter cake for washing, and drying at 55°C for 14 hours to obtain alkenyl nano-ferroferric oxide; step (2), mixing alkenyl nano-ferroferric oxide with 1% ethanol and 0.1% ethanol. Ferroferric oxide, trimethylolpropane tris(3-mercaptopropionate) and toluene are mixed in a mass ratio of 10:50:180, ultrasonically dispersed for 10 minutes, and reacted at room temperature for 16 hours under ultraviolet light irradiation with a wavelength of 365nm. After the reaction is completed, filter and take the filter cake, add toluene 5 times the mass of the filter cake to wash three times, and dry at 90°C for 26 hours to obtain mercapto nano-ferroferric oxide; wherein the preparation of silane-modified epoxy resin comprises the following steps: step (1), mixing phenol, phosphotungstic acid and thioglycolic acid at 45°C, adding acrolein, and the mass of phenol, acrolein, phosphotungstic acid and thioglycolic acid is 50%. The ratio is 26:2.2:0.15:0.15, the addition time is 20 minutes, after the addition is completed, the reaction is carried out at 50°C for 8 hours, after the reaction is completed, 0.1 mol / L sodium hydroxide aqueous solution is added to adjust the pH value to neutral, and excess phenol is removed by rotary evaporation at 150°C to obtain a bisphenol intermediate; step (2), the bisphenol intermediate, epichlorohydrin, and tetrabutylammonium chloride are mixed, and the reaction is carried out at 100°C for 26 hours. After the reaction is completed, the mixture is cooled to 0°C, and a 40wt% potassium hydroxide aqueous solution is added dropwise for 30 minutes. The bisphenol intermediate, epichlorohydrin, tetrabutylammonium chloride, and 40wt% The mass ratio of potassium hydroxide aqueous solution is 25:90:1.5:77. After the addition is completed, the reaction is continued at 0°C for 40 minutes. After the reaction is completed, the liquid is separated, the organic phase is taken, and dichloromethane 4 times the mass of the organic phase is added to dissolve and dilute, and then water 4 times the mass of the organic phase is added to wash, and the liquid is separated to obtain the washed organic phase. The solvent dichloromethane is removed by rotary evaporation at 30°C to obtain an alkenyl epoxy resin; cyclohexylaminopropyltrimethoxysilane, alkenyl epoxy resin, and lithium bromide are mixed in a mass ratio of 9:15:0.4, and stirred for reaction at room temperature in a nitrogen atmosphere for 48 hours. After the reaction is completed, a silane-modified epoxy resin is obtained;
[0031] Step 2: Mix silane-modified epoxy resin, 1,4-butanediol, isophorone diisocyanate, dibutyltin dilaurate, and acetone, and react them in a nitrogen atmosphere at 70°C for 4 hours. After the reaction, add alkenyl polyether and bisphenol fluorene, and continue to react for 6 hours in a nitrogen atmosphere at 55°C. After the reaction, add hydroxyethyl methacrylate, and react again at 55°C for 2 hours. After the reaction, remove the solvent acetone by rotary evaporation at 30°C to obtain modified polyurethane acrylate; The mass ratio of silane-modified epoxy resin, 1,4-butanediol, isophorone diisocyanate, alkenyl polyether, bisphenol fluorene, hydroxyethyl methacrylate, dibutyltin dilaurate and acetone is 20:30:80:110:5:22:0.04:100; the preparation of alkenyl polyether includes the following steps: mixing polytetrahydrofuran ether glycol and dichloroethane, adding trifluoroacetic acid and tin tetrachloride in sequence, and dropping a mixture of glycidyl methacrylate and p-methoxyphenol at a temperature of 70°C. The dropping time is 1h, and the mass ratio of polytetrahydrofuran ether glycol, glycidyl methacrylate, dichloroethane, trifluoroacetic acid, tin tetrachloride, and p-methoxyphenol is 290:28:320:0.28:0.28:0.02. After the dropping is completed, the reaction is carried out in a nitrogen atmosphere at 70°C for 2h. After the reaction is completed, a crude reaction product is obtained, and water with a mass of 2 times that of the crude reaction product is added, and then a 0.1 mol / L potassium hydroxide aqueous solution is added to adjust the pH value to neutral, and the filtrate is taken according to the reaction mixture. Add acetone and water 3 times the mass of the filtrate for washing, separate the liquids, take the organic phase, and remove the solvent by rotary evaporation at 70°C to obtain alkenyl polyether; mix modified polyurethane acrylate, mercapto nano-ferric oxide, trimethylolpropane triacrylate, additives, and photoinitiator in a mass ratio of 80:30:35:2:5 in a light-proof environment, the additive is prepared by mixing a defoamer and a leveling agent in a mass ratio of 1:1, and stir at a speed of 350 r / min and room temperature for 1 hour to obtain quick-drying magnetic ink.
[0032] Example 2
[0033] This embodiment discloses a method for preparing a quick-drying magnetic ink, comprising the following steps:
[0034] Step 1, prepare mercapto nano ferroferric oxide and silane-modified epoxy resin; wherein, the preparation of mercapto nano ferroferric oxide comprises the following steps: alkenyl nano ferroferric oxide, trimethylolpropane tris (3-mercaptopropionate), and toluene are mixed in a mass ratio of 10:52:185, the preparation of alkenyl nano ferroferric oxide is the same as that in Example 1, ultrasonically dispersed for 15 minutes, reacted at room temperature for 18 hours in an environment of ultraviolet light irradiation with a wavelength of 365nm, after the reaction is completed, filtered, the filter cake is taken, and toluene 6 times the mass of the filter cake is added The mixture was washed three times and dried at 95°C for 25 hours to obtain thiol nano-iron tetroxide; wherein the preparation of silane-modified epoxy resin comprises the following steps: step (1), phenol, phosphotungstic acid and thioglycolic acid were mixed evenly at 45°C, acrolein was added dropwise, the mass ratio of phenol, acrolein, phosphotungstic acid and thioglycolic acid was 26.2:2.23:0.15:0.15, the addition time was 25 minutes, after the addition was completed, the mixture was reacted at 55°C for 7 hours, after the reaction was completed, 0.1 mol / L sodium hydroxide solution was added The solution is adjusted to a neutral pH value, and excess phenol is removed by rotary evaporation at 155°C to obtain a bisphenol intermediate; step (2), mixing the bisphenol intermediate, epichlorohydrin, and tetrabutylammonium chloride, reacting at 110°C for 25 hours, cooling to 0°C after the reaction, and dripping a 40 wt% potassium hydroxide aqueous solution for 30 minutes, wherein the mass ratio of the bisphenol intermediate, epichlorohydrin, tetrabutylammonium chloride, and 40 wt% potassium hydroxide aqueous solution is 25:92:1.53:77, and after the dripping is completed, heating at 0°C. The reaction was continued at room temperature for 35 minutes. After the reaction was completed, the liquid was separated, the organic phase was taken, dichloromethane 4 times the mass of the organic phase was added to dissolve and dilute, and then water 4 times the mass of the organic phase was added to wash, and the washed organic phase was obtained. The solvent dichloromethane was removed by rotary evaporation at a temperature of 30°C to obtain an alkenyl epoxy resin; cyclohexylaminopropyltrimethoxysilane, alkenyl epoxy resin, and lithium bromide were mixed in a mass ratio of 9.2:15:0.45, and stirred for reaction at room temperature in a nitrogen atmosphere for 49 hours. After the reaction was completed, a silane-modified epoxy resin was obtained;
[0035] Step 2: Mix silane-modified epoxy resin, 1,4-butanediol, isophorone diisocyanate, dibutyltin dilaurate, and acetone, and react them in a nitrogen atmosphere at 70°C for 3.5 hours. After the reaction, add alkenyl polyether and bisphenol fluorene, and continue to react in a nitrogen atmosphere at 55°C for 6 hours. After the reaction, add hydroxyethyl methacrylate, and react again at 60°C for 1.5 hours. After the reaction, remove the solvent acetone by rotary evaporation at 30°C to obtain modified polyurethane acrylate; wherein The mass ratio of silane-modified epoxy resin, 1,4-butanediol, isophorone diisocyanate, alkenyl polyether, bisphenol fluorene, hydroxyethyl methacrylate, dibutyltin dilaurate, and acetone is 20.5:28:80:112:5.2:23:0.04:110; the preparation of alkenyl polyether includes the following steps: mixing polytetrahydrofuran ether glycol and dichloroethane, adding trifluoroacetic acid and tin tetrachloride in sequence, adding a mixture of glycidyl methacrylate and p-methoxyphenol dropwise at a temperature of 75°C, and the addition time is 2:1. The reaction mixture was stirred for 0.5 h, and the mass ratio of polytetrahydrofuran ether glycol, glycidyl methacrylate, dichloroethane, trifluoroacetic acid, tin tetrachloride and p-methoxyphenol was 290:28.5:330:0.285:0.285:0.02. After the addition was completed, the mixture was reacted for 1.5 h at 75 ° C in a nitrogen atmosphere. After the reaction was completed, a crude reaction product was obtained, and water with a mass of 2 times that of the crude reaction product was added. Then, a 0.1 mol / L potassium hydroxide aqueous solution was added to adjust the pH value to neutral. The mixture was filtered and the filtrate was taken. Add acetone and water 3 times the mass of the filtrate for washing, separate the liquids, take the organic phase, and remove the solvent by rotary evaporation at 75°C to obtain alkenyl polyether; mix modified polyurethane acrylate, mercapto nano-ferric oxide, trimethylolpropane triacrylate, additives, and photoinitiator in a mass ratio of 80:32:36:2.5:5.5 in a light-proof environment, the additive is prepared by mixing a defoamer and a leveling agent in a mass ratio of 1:1, and stir at a speed of 360 r / min and room temperature for 0.5 h to obtain quick-drying magnetic ink.
[0036] Example 3
[0037] This embodiment discloses a method for preparing a quick-drying magnetic ink, comprising the following steps:
[0038] Step 1, preparing mercapto nano-ferroferric tetroxide and silane-modified epoxy resin; wherein the preparation of mercapto nano-ferroferric tetroxide comprises the following steps: mixing alkenyl nano-ferroferric tetroxide, trimethylolpropane tris (3-mercaptopropionate), and toluene in a mass ratio of 10:53:190, the preparation of alkenyl nano-ferroferric tetroxide is the same as that in Example 1, ultrasonically dispersed for 15 minutes, reacted at room temperature for 18 hours in an environment of ultraviolet light irradiation with a wavelength of 365nm, after the reaction is completed, filtered, the filter cake is taken, and toluene 6 times the mass of the filter cake is added The mixture was washed three times and dried at 95°C for 25 hours to obtain thiol nano-iron tetroxide; wherein the preparation of silane-modified epoxy resin comprises the following steps: step (1), phenol, phosphotungstic acid and thioglycolic acid were mixed evenly at 48°C, acrolein was added dropwise, the mass ratio of phenol, acrolein, phosphotungstic acid and thioglycolic acid was 26.3:2.25:0.15:0.15, the addition time was 25 minutes, after the addition was completed, the mixture was reacted at 55°C for 7 hours, after the reaction was completed, 0.1 mol / L sodium hydroxide solution was added The solution is adjusted to a neutral pH value, and excess phenol is removed by rotary evaporation at 155°C to obtain a bisphenol intermediate; step (2), mixing the bisphenol intermediate, epichlorohydrin, and tetrabutylammonium chloride, reacting at 110°C for 25 hours, cooling to 0°C after the reaction, and dripping a 40 wt% potassium hydroxide aqueous solution for 35 minutes, wherein the mass ratio of the bisphenol intermediate, epichlorohydrin, tetrabutylammonium chloride, and 40 wt% potassium hydroxide aqueous solution is 25:93:1.55:78, and after the dripping is completed, stirring at 1°C The reaction was continued at 33°C for 35 minutes. After the reaction was completed, the organic phase was separated, and dichloromethane 5 times the mass of the organic phase was added to dissolve and dilute it. Then, water 5 times the mass of the organic phase was added for washing. The organic phase after washing was separated to obtain the washed organic phase. The solvent dichloromethane was removed by rotary evaporation at 33°C to obtain an alkenyl epoxy resin. Cyclohexylaminopropyltrimethoxysilane, alkenyl epoxy resin, and lithium bromide were mixed in a mass ratio of 9.3:15:0.45, and stirred for reaction at room temperature in a nitrogen atmosphere for 49 hours. After the reaction was completed, a silane-modified epoxy resin was obtained.
[0039] Step 2: Mix silane-modified epoxy resin, 1,4-butanediol, isophorone diisocyanate, dibutyltin dilaurate, and acetone, and react them in a nitrogen atmosphere at 75°C for 3.5 hours. After the reaction, add alkenyl polyether and bisphenol fluorene, and continue to react for 5.5 hours in a nitrogen atmosphere at 60°C. After the reaction, add hydroxyethyl methacrylate, and react again at 60°C for 1.5 hours. After the reaction, remove the solvent acetone by rotary evaporation at 30°C to obtain modified polyurethane acrylate; The mass ratio of silane-modified epoxy resin, 1,4-butanediol, isophorone diisocyanate, alkenyl polyether, bisphenol fluorene, hydroxyethyl methacrylate, dibutyltin dilaurate and acetone is 21:25:80:115:5.5:23.5:0.04:110; the preparation of alkenyl polyether includes the following steps: mixing polytetrahydrofuran ether glycol and dichloroethane, adding trifluoroacetic acid and tin tetrachloride in sequence, adding a mixture of glycidyl methacrylate and p-methoxyphenol dropwise at a temperature of 75°C, and adding The reaction time was 0.8h, and the mass ratio of polytetrahydrofuran ether glycol, glycidyl methacrylate, dichloroethane, trifluoroacetic acid, tin tetrachloride, and p-methoxyphenol was 290:29:340:0.29:0.29:0.02. After the addition was completed, the reaction was carried out in a nitrogen atmosphere at a temperature of 75°C for 1.5h. After the reaction was completed, a crude reaction product was obtained, and water 2.5 times the mass of the crude reaction product was added, and then a 0.1 mol / L potassium hydroxide aqueous solution was added to adjust the pH value to neutral, and the filtrate was taken and added in sequence. The mixture was washed with acetone and water (3.5 times the mass of the filtrate), separated, and the organic phase was taken. The solvent was removed by rotary evaporation at 75°C to obtain alkenyl polyether. Modified polyurethane acrylate, mercapto nano-ferric oxide, trimethylolpropane triacrylate, additives, and photoinitiator were mixed in a mass ratio of 80:33:38:2.5:5.5 in a light-proof environment. The additive was prepared by mixing a defoamer and a leveling agent in a mass ratio of 1:1. The mixture was stirred at a speed of 380 r / min and room temperature for 0.8 h to obtain a quick-drying magnetic ink.
[0040] Example 4
[0041] This embodiment discloses a method for preparing a quick-drying magnetic ink, comprising the following steps:
[0042] Step 1, prepare mercapto nano ferroferric oxide and silane-modified epoxy resin; wherein, the preparation of mercapto nano ferroferric oxide comprises the following steps: alkenyl nano ferroferric oxide, trimethylolpropane tris (3-mercaptopropionate), and toluene are mixed in a mass ratio of 10:54:190, the preparation of alkenyl nano ferroferric oxide is the same as that in Example 1, ultrasonically dispersed for 15 minutes, reacted at room temperature for 18 hours in an environment of ultraviolet light irradiation with a wavelength of 365nm, after the reaction is completed, filtered, the filter cake is taken, and toluene 8 times the mass of the filter cake is added The mixture was washed three times and dried at 95°C for 25 hours to obtain mercapto nano-iron tetroxide; wherein the preparation of the silane-modified epoxy resin comprises the following steps: step (1), phenol, phosphotungstic acid and thioglycolic acid were mixed uniformly at 50°C, acrolein was added dropwise, the mass ratio of phenol, acrolein, phosphotungstic acid and thioglycolic acid was 26.4:2.28:0.16:0.16, the addition time was 30 minutes, after the addition was completed, the mixture was reacted at 60°C for 7 hours, after the reaction was completed, 0.1 mol / L sodium hydroxide was added The aqueous solution is adjusted to a neutral pH value, and excess phenol is removed by rotary evaporation at a temperature of 155° C. to obtain a bisphenol intermediate; step (2), the bisphenol intermediate, epichlorohydrin, and tetrabutylammonium chloride are mixed, reacted at a temperature of 110° C. for 25 hours, after the reaction is completed, cooled to 0° C., and a 40 wt % potassium hydroxide aqueous solution is added dropwise for 40 minutes, and the mass ratio of the bisphenol intermediate, epichlorohydrin, tetrabutylammonium chloride, and 40 wt % potassium hydroxide aqueous solution is 25:94:1.58:79. After the addition is completed, The reaction was continued at ℃ for 35 minutes. After the reaction was completed, the liquid was separated, the organic phase was taken, dichloromethane 6 times the mass of the organic phase was added to dissolve and dilute, and then water 6 times the mass of the organic phase was added to wash, and the washed organic phase was obtained. The solvent dichloromethane was removed by rotary evaporation at 35℃ to obtain an alkenyl epoxy resin; cyclohexylaminopropyltrimethoxysilane, alkenyl epoxy resin, and lithium bromide were mixed in a mass ratio of 9.4:15:0.5, and stirred for reaction at room temperature in a nitrogen atmosphere for 49 hours. After the reaction was completed, a silane-modified epoxy resin was obtained;
[0043] Step 2: Mix silane-modified epoxy resin, 1,4-butanediol, isophorone diisocyanate, dibutyltin dilaurate, and acetone, and react them in a nitrogen atmosphere at 75°C for 3.5 hours. After the reaction, add alkenyl polyether and bisphenol fluorene, and continue to react for 5 hours in a nitrogen atmosphere at 65°C. After the reaction, add hydroxyethyl methacrylate, and react again at 65°C for 1 hour. After the reaction, remove the solvent acetone by rotary evaporation at 30°C to obtain modified polyurethane acrylate; wherein The mass ratio of silane-modified epoxy resin, 1,4-butanediol, isophorone diisocyanate, alkenyl polyether, bisphenol fluorene, hydroxyethyl methacrylate, dibutyltin dilaurate, and acetone is 21.5:23:80:118:5.8:24:0.05:120; the preparation of alkenyl polyether includes the following steps: mixing polytetrahydrofuran ether glycol and dichloroethane, adding trifluoroacetic acid and tin tetrachloride in sequence, adding a mixture of glycidyl methacrylate and p-methoxyphenol dropwise at a temperature of 80°C, and dropping The addition time is 1 hour, and the mass ratio of polytetrahydrofuran ether glycol, glycidyl methacrylate, dichloroethane, trifluoroacetic acid, tin tetrachloride, and p-methoxyphenol is 290:29.5:350:0.295:0.295:0.02. After the addition is completed, the reaction is carried out in a nitrogen atmosphere at a temperature of 75°C for 2 hours. After the reaction is completed, a crude reaction product is obtained, and water 3 times the mass of the crude reaction product is added, and then a 0.1 mol / L potassium hydroxide aqueous solution is added to adjust the pH value to neutral, and the filtrate is taken according to the reaction mixture. Add acetone and water in an amount 4 times the mass of the filtrate for washing, separate the liquids, take the organic phase, and remove the solvent by rotary evaporation at 75°C to obtain alkenyl polyether; mix modified polyurethane acrylate, mercapto nano-ferric oxide, trimethylolpropane triacrylate, additives, and photoinitiator in a mass ratio of 80:34:39:2.5:5.5 in a light-proof environment, the additive is prepared by mixing a defoamer and a leveling agent in a mass ratio of 1:1, and stir at a speed of 390 r / min and room temperature for 1 hour to obtain quick-drying magnetic ink.
[0044] Example 5
[0045] This embodiment discloses a method for preparing a quick-drying magnetic ink, comprising the following steps:
[0046] Step 1, preparing mercapto nano-ferroferric tetroxide and silane-modified epoxy resin; wherein the preparation of mercapto nano-ferroferric tetroxide comprises the following steps: mixing alkenyl nano-ferroferric tetroxide, trimethylolpropane tris(3-mercaptopropionate), and toluene in a mass ratio of 10:55:200, the preparation of alkenyl nano-ferroferric tetroxide is the same as that in Example 1, ultrasonically dispersed for 20 minutes, reacted at room temperature for 20 hours in an environment of ultraviolet light irradiation with a wavelength of 365nm, and after the reaction is completed, filtered, the filter cake is taken, and toluene 8 times the mass of the filter cake is added The mixture was washed three times and dried at 100°C for 24 hours to obtain mercapto nano-iron tetroxide; wherein the preparation of silane-modified epoxy resin comprises the following steps: step (1), phenol, phosphotungstic acid and thioglycolic acid were mixed evenly at 50°C, acrolein was added dropwise, the mass ratio of phenol, acrolein, phosphotungstic acid and thioglycolic acid was 26.5:2.3:0.16:0.16, the addition time was 30 minutes, after the addition was completed, the mixture was reacted at 60°C for 6 hours, after the reaction was completed, 0.1 mol / L sodium hydroxide was added The aqueous solution is adjusted to a neutral pH value, and excess phenol is removed by rotary evaporation at a temperature of 160° C. to obtain a bisphenol intermediate; step (2), the bisphenol intermediate, epichlorohydrin, and tetrabutylammonium chloride are mixed, reacted at a temperature of 120° C. for 24 hours, after the reaction is completed, cooled to 0° C., and a 40 wt % potassium hydroxide aqueous solution is added dropwise for 40 minutes, and the mass ratio of the bisphenol intermediate, epichlorohydrin, tetrabutylammonium chloride, and 40 wt % potassium hydroxide aqueous solution is 25:95:1.6:80. After the addition is completed, the mixture is stirred at 2° C. The reaction was continued at 35°C for 30 minutes. After the reaction was completed, the organic phase was separated, and dichloromethane 6 times the mass of the organic phase was added to dissolve and dilute it. Then, water 6 times the mass of the organic phase was added for washing. The organic phase after washing was separated to obtain the washed organic phase. The solvent dichloromethane was removed by rotary evaporation at 35°C to obtain an alkenyl epoxy resin. Cyclohexylaminopropyltrimethoxysilane, alkenyl epoxy resin, and lithium bromide were mixed in a mass ratio of 9.5:15:0.5, and stirred for reaction at room temperature in a nitrogen atmosphere for 50 hours. After the reaction was completed, a silane-modified epoxy resin was obtained.
[0047] Step 2: Mix silane-modified epoxy resin, 1,4-butanediol, isophorone diisocyanate, dibutyltin dilaurate, and acetone, and react them in a nitrogen atmosphere at 80°C for 3 hours. After the reaction, add alkenyl polyether and bisphenol fluorene, and continue to react for 5 hours in a nitrogen atmosphere at 65°C. After the reaction, add hydroxyethyl methacrylate, and react again at 65°C for 1 hour. After the reaction, remove the solvent acetone by rotary evaporation at 30°C to obtain modified polyurethane acrylate; The mass ratio of silane-modified epoxy resin, 1,4-butanediol, isophorone diisocyanate, alkenyl polyether, bisphenol fluorene, hydroxyethyl methacrylate, dibutyltin dilaurate and acetone is 22:20:80:120:6:25:0.05:120; the preparation of alkenyl polyether comprises the following steps: polytetrahydrofuran ether glycol and ethylene dichloride are mixed, trifluoroacetic acid and tin tetrachloride are added in sequence, a mixture of glycidyl methacrylate and p-methoxyphenol is added dropwise at a temperature of 80°C, and The addition time is 0.5h, and the mass ratio of polytetrahydrofuran ether glycol, glycidyl methacrylate, dichloroethane, trifluoroacetic acid, tin tetrachloride, and p-methoxyphenol is 290:30:350:0.3:0.3:0.02. After the addition is completed, the reaction is carried out in a nitrogen atmosphere at 80°C for 1h. After the reaction is completed, a crude reaction product is obtained, and water 3 times the mass of the crude reaction product is added, and then a 0.1 mol / L potassium hydroxide aqueous solution is added to adjust the pH value to neutral, and the filtrate is taken and filtered. Add acetone and water in an amount 4 times the mass of the filtrate for washing, separate the liquids, take the organic phase, and remove the solvent by rotary evaporation at 80°C to obtain alkenyl polyether; mix modified polyurethane acrylate, mercapto nano-ferric oxide, trimethylolpropane triacrylate, additives, and photoinitiator in a mass ratio of 80:35:40:3:6 in a light-proof environment, and the additive is prepared by mixing a defoamer and a leveling agent in a mass ratio of 1:1. Stir at a speed of 400 r / min and room temperature for 0.5 h to obtain quick-drying magnetic ink.
[0048] Comparative Example 1
[0049] This comparative example discloses a method for preparing magnetic ink, comprising the following steps:
[0050] Step 1, preparing silane modified epoxy resin; Step (1), mixing phenol, phosphotungstic acid and thioglycolic acid at 45°C, adding acrolein dropwise, the mass ratio of phenol, acrolein, phosphotungstic acid and thioglycolic acid is 26:2.2:0.15:0.15, the adding time is 20min, after the adding is completed, reacting at 50°C for 8h, after the reaction is completed, adding 0.1mol / L sodium hydroxide aqueous solution to adjust the pH value to neutral, and removing excess phenol by rotary evaporation at 150°C to obtain a bisphenol intermediate; Step (2), mixing the bisphenol intermediate, epichlorohydrin and tetrabutylammonium chloride, reacting at 100°C for 26h, after the reaction is completed, cooling to 0°C, and adding 40wt% potassium hydroxide aqueous solution. , the dropping time is 30min, the mass ratio of bisphenol intermediate, epichlorohydrin, tetrabutylammonium chloride and 40wt% potassium hydroxide aqueous solution is 25:90:1.5:77, after the dropping is completed, the reaction is continued at 0℃ for 40min, after the reaction is completed, the liquid is separated, the organic phase is taken, dichloromethane 4 times the mass of the organic phase is added to dissolve and dilute, and then water 4 times the mass of the organic phase is added to wash, the liquid is separated, the washed organic phase is obtained, and the solvent dichloromethane is removed by rotary evaporation at 30℃ to obtain alkenyl epoxy resin; cyclohexylaminopropyltrimethoxysilane, alkenyl epoxy resin and lithium bromide are mixed in a mass ratio of 9:15:0.4, stirred and reacted in a nitrogen atmosphere at room temperature for 48h, after the reaction is completed, a silane-modified epoxy resin is obtained;
[0051] Step 2: Mix silane-modified epoxy resin, 1,4-butanediol, isophorone diisocyanate, dibutyltin dilaurate, and acetone, and react them in a nitrogen atmosphere at 70°C for 4 hours. After the reaction, add alkenyl polyether and bisphenol fluorene, and continue to react for 6 hours in a nitrogen atmosphere at 55°C. After the reaction, add hydroxyethyl methacrylate and react again at 55°C for 2 hours. After the reaction, remove the solvent acetone by rotary evaporation at 30°C to obtain modified polyurethane acrylate. ; wherein the mass ratio of silane-modified epoxy resin, 1,4-butanediol, isophorone diisocyanate, alkenyl polyether, bisphenol fluorene, hydroxyethyl methacrylate, dibutyltin dilaurate, and acetone is 20:30:80:110:5:22:0.04:100; the preparation of alkenyl polyether comprises the following steps: mixing polytetrahydrofuran ether glycol and dichloroethane, adding trifluoroacetic acid and tin tetrachloride in sequence, and dropping a mixture of glycidyl methacrylate and p-methoxyphenol at a temperature of 70°C; The addition time is 1h, the mass ratio of polytetrahydrofuran ether glycol, glycidyl methacrylate, dichloroethane, trifluoroacetic acid, tin tetrachloride, and p-methoxyphenol is 290:28:320:0.28:0.28:0.02. After the addition is completed, the reaction is carried out in a nitrogen atmosphere at a temperature of 70°C for 2h. After the reaction is completed, a crude reaction product is obtained, and water with a mass of 2 times that of the crude reaction product is added, and then a 0.1 mol / L potassium hydroxide aqueous solution is added to adjust the pH value to neutral, and the filtrate is taken. The mixture was stirred for 1 h at a speed of 350 r / min and room temperature for 1 h to obtain magnetic ink.
[0052] Comparative Example 2
[0053] This comparative example discloses a method for preparing magnetic ink, comprising the following steps:
[0054] Step 1, preparing mercapto nano-ferroferric oxide; alkenyl nano-ferroferric oxide, trimethylolpropane tris (3-mercaptopropionate), and toluene are mixed in a mass ratio of 10:50:180. The preparation of alkenyl nano-ferroferric oxide is the same as that in Example 1. Ultrasonic dispersion is performed for 10 minutes. The reaction is carried out at room temperature under an ultraviolet lamp irradiation environment with a wavelength of 365 nm for 16 hours. After the reaction is completed, the filter is filtered, and the filter cake is taken. Toluene with a mass of 5 times that of the filter cake is added for washing three times, and the mixture is dried at 90° C. for 26 hours to obtain mercapto nano-ferroferric oxide;
[0055] Step 2: Mix 1,4-butanediol, isophorone diisocyanate, dibutyltin dilaurate and acetone, react in a nitrogen atmosphere at 70°C for 4 hours, add polytetramethylene glycol and bisphenol fluorene after the reaction, continue to react in a nitrogen atmosphere at 55°C for 6 hours, add hydroxyethyl methacrylate after the reaction, react again at 55°C for 2 hours, and remove the solvent acetone by rotary evaporation at 30°C to obtain modified polyurethane acrylate; wherein, 1,4-butanediol and isophorone diisocyanate , polytetramethylene ether diol, bisphenol fluorene, hydroxyethyl methacrylate, dibutyltin dilaurate, and acetone in a mass ratio of 50:80:110:5:22:0.04:100; modified polyurethane acrylate, mercapto nano-ferric oxide, trimethylolpropane triacrylate, additives, and photoinitiator are mixed in a mass ratio of 80:30:35:2:5 in a light-proof environment. The additive is prepared by mixing a defoamer and a leveling agent in a mass ratio of 1:1. The mixture is stirred at a speed of 350 r / min and room temperature for 1 hour to obtain magnetic ink.
[0056] In the above embodiments and comparative examples: nano-iron tetroxide comes from Shanghai MacLean Biochemical Technology Co., Ltd., with a particle size of 20 nm and CAS number: 1317-61-9; trimethylolpropane tris(3-mercaptopropionate) comes from Shanghai Aladdin Biochemical Technology Co., Ltd., with CAS number: 33007-83-9; phosphotungstic acid comes from Shanghai Shaoyuan Reagent Co., Ltd., with CAS number: 12067-99-1; epichlorohydrin comes from Shanghai Aladdin Biochemical Technology Co., Ltd., with a model of analytical grade and CAS number: 106-89-8; cyclohexylaminopropyl trimethoxysilane comes from Shanghai MacLean Biochemical Technology Co., Ltd., with a product number of N924015 and a CAS number of 3068-78-8; bisphenol fluorene comes from Alfa Aesar Company, CAS number: 3236-71-3; hydroxyethyl methacrylate comes from Guangdong Wengjiang Chemical Reagent Co., Ltd., CAS number: 868-77-9; polytetramethylene ether glycol comes from Shanghai Aladdin Biochemical Technology Co., Ltd., Mn=2900, CAS number: 25190-06-1; glycidyl methacrylate comes from Shanghai McLean Biochemical Technology Co., Ltd., CAS number: 106-91-2; trimethylolpropane triacrylate comes from Guangdong Wengjiang Chemical Reagent Co., Ltd., CAS number: 15625-89-5; photoinitiator comes from Shanghai Aladdin Biochemical Technology Co., Ltd., model photoinitiator 1173, CAS number: 7374-98-5; defoamer comes from BASF, model EfkaPB2001; leveling agent comes from Dow Corning, model DC-57.
[0057] Test example
[0058] The comprehensive performance of the magnetic inks prepared in Examples 1-5 and Comparative Examples 1-2 was tested; the magnetic inks prepared in Examples 1-5 and Comparative Examples 1-2 were printed on the surface of a 3.2 mm × 2.4 mm × 0.5 mm glass sheet, respectively, and cured at 140° C. for 3 seconds under UV-LED ultraviolet light to obtain samples 1-7; 100 samples 1-7 were taken, respectively, blended with 900 3.2 mm × 2.4 mm × 0.5 mm glass sheets, and separated under the action of an external magnetic field, and the magnetic separation performance was tested; the specific test results are shown in Tables 1 and 2:
[0059] ;
[0060]
[0061] The testing of each indicator in the table is based on the following standards: the actual drying time is determined by referring to GB / T 1728-2020 "Determination of drying time of paint film and putty film"; the water resistance is determined by referring to GB / T 1733-1993 "Determination of water resistance of paint film"; the adhesion is determined by referring to GB∕T 13217.7-2023 "Ink adhesion test method"; the hardness is determined by referring to GB / T 6739-2006 "Determination of paint film hardness by pencil method for paints and varnishes".
[0062] It can be seen from the test results in Table 1 and Table 2 that the magnetic ink prepared by the present invention can be quickly cured and has excellent comprehensive performance and magnetic separation performance.
[0063] The invention performs surface modification on nano ferroferric oxide, and sequentially grafts a vinyl silane coupling agent and trimethylolpropane tris(3-mercaptopropionate), thereby improving the dispersibility of the nano ferroferric oxide in ink. Moreover, since trimethylolpropane tris(3-mercaptopropionate) has a multi-mercapto functional group structure, the surface of the obtained mercapto nano ferroferric oxide has a large number of mercapto functional groups. When the mercapto nano ferroferric oxide is added into the ink as a magnetic filler, the mercapto functional groups can participate in the ultraviolet light curing process of the ink, and generate a click chemical reaction with the carbon-carbon double bonds of the organic polymer resin in the ink, thereby reducing the oxygen inhibition effect in the light curing process of the ink. The curing speed of the ink is accelerated, the dispersibility and compatibility of the nano-iron tetroxide in the ink are further improved, so that the prepared quick-drying magnetic ink has a multiple curing system, and the curing speed and comprehensive performance of the ink are improved; in Comparative Example 1, the surface of the nano-iron tetroxide is not modified, and trimethylolpropane tris (3-mercaptopropionate) with a multi-thiol functional group structure is not grafted on the surface of the nano-iron tetroxide, so the nano-iron tetroxide cannot be connected to the polymer resin matrix of the ink through a chemical bond during the photocuring process, the dispersibility of the nano-iron tetroxide is reduced, it is easy to agglomerate, and the lack of the thiol functional group is not conducive to the curing of the nano-iron tetroxide. The improvement effect of oxygen inhibition effect is achieved, so the curing speed of the magnetic ink in comparative example 1 is reduced and the comprehensive performance is reduced; the silane-modified epoxy resin, alkenyl polyether, bisphenol fluorene, 1,4-butanediol and isophorone diisocyanate of the present invention react under catalyst conditions and are capped by hydroxyethyl methacrylate to obtain modified polyurethane acrylate; wherein the siloxane segment in the silane-modified epoxy resin can improve the water resistance of the ink, and the epoxy resin structure can improve the comprehensive performance of the ink; both the alkenyl polyether and the silane-modified epoxy resin contain carbon-carbon double bonds as side chain groups, which can not only generate Free radical polymerization can be generated, and click chemical reaction can occur with the thiol group of thiol nano-ferroferric oxide, so that the prepared quick-drying magnetic ink has a multiple curing system, which improves the curing speed and comprehensive performance of the ink; in comparative example 2, silane-modified epoxy resin is not added, and polytetrahydrofuran ether diol is not modified. The epoxy resin structure is lacking to improve the comprehensive performance of the ink and the siloxane structure is lacking to improve the water resistance of the ink. At the same time, the side chain carbon-carbon double bond content in the ink system is reduced. In the light curing process, the cross-linking speed of the resin is reduced, so the curing speed of the magnetic ink in comparative example 2 is reduced, and the comprehensive performance is reduced.
[0064] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing a quick-drying magnetic ink, characterized in that: The following steps are involved: Step 1, preparing mercapto nano-ferroferric oxide and silane-modified epoxy resin; Wherein, the preparation of mercapto nano-ferroferric oxide comprises the following steps: Mixing alkenyl nano-ferrosilicate, trimethylolpropane tris(3-mercaptopropionate) and toluene, dispersing by ultrasonication, reacting, filtering, washing and drying after the reaction is completed to obtain mercapto nano-ferrosilicate; The mass ratio of alkenyl nano-iron tetroxide, trimethylolpropane tris(3-mercaptopropionate) and toluene is 10:(50-55):(180-200); wherein the alkenyl nano-iron tetroxide is prepared by reacting vinyl trimethoxysilane, nano-iron tetroxide and ethanol aqueous solution in a mass ratio of 10:(0.8-1):(180-200), and the ethanol aqueous solution is 50 vol% ethanol aqueous solution; The preparation of silane-modified epoxy resin comprises the following steps: Step (1), mixing a bisphenol intermediate, epichlorohydrin and tetrabutylammonium chloride, reacting, cooling after the reaction is completed, dropping a potassium hydroxide aqueous solution, continuing the reaction after the dropwise addition is completed, and purifying after the reaction is completed to obtain an olefin epoxy resin; The mass ratio of bisphenol intermediate, epichlorohydrin, tetrabutylammonium chloride and potassium hydroxide aqueous solution is 25: (90-95): (1.5-1.6): (77-80), and the potassium hydroxide aqueous solution is a 40wt% potassium hydroxide aqueous solution; wherein the bisphenol intermediate is prepared by reacting phenol, acrolein, phosphotungstic acid and thioglycolic acid in a mass ratio of (26-26.5): (2.2-2.3): (0.15-0.16): (0.15-0.16); Step (2), mixing cyclohexylaminopropyltrimethoxysilane, alkenyl epoxy resin and lithium bromide, and reacting them. After the reaction is completed, a silane-modified epoxy resin is obtained; The mass ratio of cyclohexylaminopropyltrimethoxysilane, alkenyl epoxy resin and lithium bromide is (9-9.5):15:(0.4-0.5); Step 2: Mix silane-modified epoxy resin, 1,4-butanediol, isophorone diisocyanate, dibutyltin dilaurate, and acetone, and react. After the reaction is completed, add alkenyl polyether and bisphenol fluorene, and continue to react. After the reaction is completed, add hydroxyethyl methacrylate, and react again. After the reaction is completed, remove the solvent acetone by rotary evaporation to obtain modified polyurethane acrylate; The mass ratio of silane-modified epoxy resin, 1,4-butanediol, isophorone diisocyanate, alkenyl polyether, bisphenol fluorene, hydroxyethyl methacrylate, dibutyltin dilaurate and acetone is (20-22): (20-30): 80: (110-120): (5-6): (22-25): (0.04-0.05): (100-120); wherein the alkenyl polyether is prepared by reacting polytetramethylene glycol, glycidyl methacrylate, ethylene dichloride, trifluoroacetic acid, tin tetrachloride and p-methoxyphenol in a mass ratio of 290: (28-30): (320-350): (0.28-0.3): (0.28-0.3): 0.02; Modified polyurethane acrylate, mercapto nano-ferroferric oxide, trimethylolpropane triacrylate, acetone, additives and photoinitiator are mixed and stirred to obtain a quick-drying magnetic ink; The mass ratio of modified polyurethane acrylate, mercapto nano-ferric oxide, trimethylolpropane triacrylate, additive and photoinitiator is 80: (30-35): (35-40): (2-3): (5-6), and the additive is prepared by mixing a defoamer and a leveling agent in a mass ratio of 1:
1.
2. The method for preparing a quick-drying magnetic ink according to claim 1, characterized in that: When preparing the mercapto nano-ferroferric oxide in step 1, the olefin nano-ferroferric oxide is prepared by the following steps: Vinyl trimethoxysilane, nano-ferroferric oxide and ethanol aqueous solution are mixed, ultrasonically dispersed, a regulator is added to adjust the pH value, reacted, filtered, washed and dried after the reaction is completed to obtain vinyl nano-ferroferric oxide; The reaction conditions are as follows: react at a pH of 9.5-10 and a temperature of 40-50° C. for 3-4 hours.
3. The method for preparing a quick-drying magnetic ink according to claim 1, characterized in that: In the step 1, when preparing the mercapto nano-ferroferric oxide, the reaction conditions are: reacting for 16-20 hours at room temperature under the irradiation environment of an ultraviolet lamp with a wavelength of 365nm.
4. The method for preparing a quick-drying magnetic ink according to claim 1, characterized in that: When the silane-modified epoxy resin is prepared in step 1, the bisphenol intermediate in step (1) is prepared by the following steps: Phenol, phosphotungstic acid and thioglycolic acid are uniformly mixed, acrolein is added dropwise, and after the addition is complete, a reaction is carried out. After the reaction is completed, a regulator is added to adjust the pH value, and excess phenol is removed by rotary evaporation to obtain a bisphenol intermediate; The conditions for dropping acrolein are: dropping at 45-50°C for 20-30 minutes; and the reaction conditions are: reacting at 50-60°C for 6-8 hours.
5. The method for preparing a quick-drying magnetic ink according to claim 1, characterized in that: When preparing the silane-modified epoxy resin in step 1, the reaction conditions in step (1) are: reacting at a temperature of 100-120° C. for 24-26 hours; the dropping conditions of the potassium hydroxide aqueous solution are: dropping at a temperature of 0° C. for 30-40 minutes; and the continued reaction conditions are: continuing the reaction at a temperature of 0-2° C. for 30-40 minutes; When preparing the silane-modified epoxy resin in step 1, the reaction conditions in step (2) are: stirring the reaction at room temperature in a nitrogen atmosphere for 48-50 hours.
6. The method for preparing a quick-drying magnetic ink according to claim 1, characterized in that: The alkenyl polyether in step 2 is prepared by the following steps: The polytetrahydrofuran ether glycol and dichloroethane are mixed, trifluoroacetic acid and tin tetrachloride are added in sequence, a mixture of glycidyl methacrylate and p-methoxyphenol is added dropwise, after the addition is complete, the mixture is reacted, and after the reaction is complete, the mixture is purified to obtain an alkenyl polyether; The dripping condition of the mixture of glycidyl methacrylate and p-methoxyphenol is: dripping at 70-80° C. for 0.5-1 h; the reaction condition is: reacting at 70-80° C. for 1-2 h in a nitrogen atmosphere.
7. The method for preparing a quick-drying magnetic ink according to claim 1, characterized in that: In the step 2, the reaction conditions are: reacting for 3-4 hours at 70-80°C in a nitrogen atmosphere; continuing the reaction conditions are: continuing the reaction for 5-6 hours at 55-65°C in a nitrogen atmosphere; and reacting again for 1-2 hours at 55-65°C in a nitrogen atmosphere.
8. A quick-drying magnetic ink prepared by the method for preparing a quick-drying magnetic ink as claimed in any one of claims 1 to 7.
9. Use of the quick-drying magnetic ink as claimed in claim 8 in chip production.