Wear-resistant super-hydrophobic coating with drag reduction performance and preparation method of wear-resistant super-hydrophobic coating
Through the combination of hydrophobic nano-silica and micron mesoporous silica and epoxy resin, an embedded micro-nano particle structure is formed, which solves the shortcomings of super-hydrophobic coating in drag reduction and wear resistance, and achieves high-speed fluid environment Highly efficient drag reduction and wear resistance, suitable for large-scale construction.
Patent Information
- Application Number
- CN202410995108.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-10-01
AI Technical Summary
Existing superhydrophobic coatings are ineffective in drag reduction applications and lack wear resistance, making them unable to effectively reduce drag and maintain surface properties in high-speed fluid environments.
A combination of hydrophobic nano-silica and hydrophobic micron mesoporous silica and epoxy resin is used to form an embedded micro-nano particle structure through modification treatment. The super-hydrophobic coating is prepared by spraying to ensure low surface roughness and high wear resistance. .
A wear-resistant coating that significantly reduces resistance in fluids and maintains a superhydrophobic state is achieved. It is suitable for high-speed moving objects such as boats, simplifying the large-scale preparation process and reducing costs.
Smart Images

Figure CN118725691A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of super-hydrophobic nanomaterials, and in particular to a wear-resistant super-hydrophobic coating with drag reduction performance and a preparation method thereof. Background Art
[0002] In nature, the surface of plants and animals such as lotus leaves, water chestnuts, and pufferfish often repel water, which provides a basic theoretical basis and design ideas for researchers to study super-hydrophobic surfaces. In recent years, super-hydrophobic surfaces with a contact angle greater than 150° and a rolling angle less than 10° have attracted widespread attention and have shown broad prospects in the fields of anti-fouling, anti-icing, flow control, and drag reduction.
[0003] Super-hydrophobic surface is composed of surface roughness and low surface energy material. The construction of surface roughness is usually related to the preparation method. It can be realized on the substrate surface by plasma, photolithography technology, etc., or it can be coated on the substrate surface by nanomaterials. Common nanomaterials include nanoparticles such as silicon dioxide, aluminum oxide, and zinc oxide; low surface energy material is usually fluorine material or silane material, and polymers with fluorine groups are usually used for surface modification, and can also be mixed in nanopowders. Common preparation methods for super-hydrophobic surface include sol-gel method, etching method, self-assembly method, template method, etc., but the chemical composition used in the above method is relatively complex, the preparation process is often overly dependent on precision instruments, the operating environment and time control are strict, and there are certain requirements for the substrate, resulting in limited substrates that can be used. In addition, the preparation cost is high, the process operation steps are complicated, and large-scale preparation is difficult, which also limits the application of super-hydrophobic surface.
[0004] Super hydrophobic surface can reduce the surface friction of objects in laminar and turbulent flow. Using super hydrophobic surface can change the no-slip condition to the slip condition, thereby reducing the object wall velocity gradient and wall shear stress, so the energy required for the object to move in the fluid or the fluid to flow in the pipeline will be reduced, and the corresponding resistance will also be reduced. At present, although excellent anti-fouling, self-cleaning, transparent and other super hydrophobic surfaces can be obtained by some methods, they may not be suitable for the drag reduction application of objects, because the drag reduction effect of super hydrophobic surface is affected by surface roughness: the smaller the surface roughness under the super hydrophobic surface air film is covered, the stronger the drag reduction effect is, if you want to play a drag reduction effect, you need to prepare a super hydrophobic coating with low surface roughness. In addition, as the object moving speed increases, the shearing of the fluid to the super hydrophobic surface increases, and people have certain requirements for the impact resistance of the super hydrophobic surface according to actual application needs, so it is necessary to develop a wear-resistant super hydrophobic coating with excellent drag reduction performance and a preparation method of this coating. Summary of the invention
[0005] In order to solve the problem that existing super-hydrophobic coatings are not suitable for applications in drag reduction, and to meet people's further high requirements for the wear resistance of super-hydrophobic coatings, the present invention provides a wear-resistant super-hydrophobic coating with drag reduction performance and a preparation method thereof. The prepared super-hydrophobic coating has both excellent drag reduction performance and wear resistance.
[0006] To achieve the above objectives, the following technical solutions are adopted:
[0007] A wear-resistant super-hydrophobic coating with drag-reducing performance, wherein the raw materials for making the coating are hydrophobic nano-silicon dioxide, hydrophobic micron-mesoporous silica and epoxy resin;
[0008] The mass ratio of hydrophobic micro-mesoporous silica, hydrophobic nano-silica and epoxy resin is 10:3:17;
[0009] The hydrophobic nano-silica is obtained by modifying nano-silica, and the hydrophobic micron-mesoporous silica is obtained by modifying micron-mesoporous silica.
[0010] It is further defined that the particle size of nano-silicon dioxide is 5 to 15 nm.
[0011] It is further defined that the particle size of micron mesoporous silica is 1 to 10 μm.
[0012] It is further defined that the epoxy resin is bisphenol A epoxy resin, polyacrylate epoxy resin, FEVE fluorocarbon resin or water-based polyurethane.
[0013] A method for preparing a wear-resistant super-hydrophobic coating with drag reduction performance comprises the following steps:
[0014] Step 1: respectively adding nano-silica and micro-mesoporous silica to a solution consisting of anhydrous ethanol, deionized water and ammonium hydroxide and heating the solution, then respectively adding silane to obtain two sets of mixed solutions, centrifuging and drying the mixed solutions to obtain hydrophobic nano-silica and hydrophobic micro-mesoporous silica;
[0015] Step 2: Dispersing hydrophobic nano-silica and hydrophobic micron mesoporous silica in a polar solvent and stirring to obtain a mixed solution, and adding epoxy resin to the mixed solution to obtain a coating solution;
[0016] Step 3: Spray the coating liquid onto the treated substrate, and dry the substrate after the polar solvent in the coating liquid is completely evaporated to obtain a super hydrophobic coating.
[0017] It is further defined that the silane in step 1 is octyltriethoxysilane, γ-aminopropyltriethoxysilane, γ-methacryloxypropyltrimethoxysilane or perfluorodecyltriethoxysilane.
[0018] It is further defined that in step 1, the mass ratio of nano-silica to silane is 7:1, and the mass ratio of micron-mesoporous silica to silane is 7:1.
[0019] It is further defined that in step 1, the mass ratio of anhydrous ethanol, deionized water and ammonium hydroxide is 10:2:1.
[0020] It is further defined that the heating temperature in step 1 is 50°C.
[0021] It is further defined that the centrifugal speed in step 1 is 8000 r / min and the time is 15 min.
[0022] It is further defined that in step 1, the proportion of nano-silica in the mixed solution is 5wt%, and the proportion of micron-mesoporous silica in the mixed solution is 5wt%.
[0023] It is further defined that in step 2, the stirring speed is 600 r / min and the stirring time is 10 min.
[0024] It is further defined that the sum of the mass of the hydrophobic nano-silica and the hydrophobic micron-mesoporous silica in the coating liquid in step 2 accounts for 10 wt % to 15 wt %.
[0025] It is further defined that the polar solvent in step 2 is one of ethyl acetate, butyl acetate and cyclohexane.
[0026] It is further defined that in step three, after spraying the coating liquid onto the substrate, wait for 3 to 5 minutes.
[0027] It is further defined that the drying process in step three is: drying at 80° C. for 1 hour in a constant temperature drying oven.
[0028] It is further defined that in step three, the substrate is one of acrylic, glass, ABS board, etc.
[0029] The beneficial effects of the present invention are:
[0030] Super-hydrophobic coating of the present invention can carry out dehydration condensation in the environment of absolute ethanol, deionized water and ammonium hydroxide using hydrophilic nano-silicon and micron mesoporous silica particles, then hydrophobically modified using silane, by the stirring of two kinds of hydrophobically modified particles in polar solvents, hydrophobic nano-silicon (i.e. forming a kind of micro-nano particle structure) is loaded with hydrophobic micron mesoporous silica, substrate plane and micro-nano particles are fixed with epoxy resin, and a kind of wear-resistant super-hydrophobic coating with drag reduction performance is obtained.Because the hole of hydrophobically modified micron mesoporous silica is filled by hydrophobic nano-silicon, when super-hydrophobic coating is destroyed by external force, hydrophobic micron mesoporous silica is first destroyed, but the hydrophobic nano-silicon in mesoporous silica can continue to form roughness and low surface energy on the surface, so that coating continues to reach super-hydrophobic state, improves the wear resistance of coating. In addition, the unmodified hydroxyl groups on the surface of micro-mesoporous silica and nano-silica can form covalent bonds with functional groups in epoxy resin, such as epoxy groups, further enhancing the wear resistance of the superhydrophobic coating.
[0031] When water flows in a pipe, it will produce pressure difference at different positions due to the friction loss along the wall. The pressure difference data ΔP of the smooth surface is measured through a high-speed circulating water tunnel. smooth , under the same conditions, the pressure difference data ΔP of the super hydrophobic surface was measured SHS , through the drag reduction formula: The drag reduction rate of the super-hydrophobic coating is obtained, and the results obtained therefrom show that the lower the surface roughness, the better the drag reduction performance, which explains why not all super-hydrophobic coatings have good drag reduction performance, because their roughness is not very low. The present invention is to stir hydrophobic micron mesoporous silica and hydrophobic nano silica in a polar solvent so that the two form an "embedded" micro-nano particle combination, and this combination form has a lower surface roughness, so that the super-hydrophobic coating has a good drag reduction effect, and can be used on surfaces such as boats to reduce navigation resistance. The present invention adopts a spraying method, and a super-hydrophobic coating can be prepared under most substrate shapes and materials, which is convenient for large-scale construction. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 This is the SEM image of the nano-silicon dioxide in Example 1;
[0033] Figure 2 is a SEM image of the micron mesoporous silica in Example 1;
[0034] Figure 3 Schematic diagram of the contact angle of the super-hydrophobic coating obtained in Example 1, wherein CA is the contact angle;
[0035] Figure 4 This is a friction resistance test diagram of the super hydrophobic coating obtained in Example 1;
[0036] Figure 5 This is a test graph of the drag reduction rate of the super hydrophobic coating obtained in Example 1;
[0037] Figure 6 This is a friction resistance test diagram of the super hydrophobic coating obtained in Example 2;
[0038] Figure 7 This is a test graph of the drag reduction rate of the super-hydrophobic coating obtained in Example 2;
[0039] Figure 8 This is a test chart of the drag reduction rate of the super-hydrophobic coating obtained in Comparative Example 1. DETAILED DESCRIPTION
[0040] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the present invention. The following embodiments are only used to more clearly illustrate the technical solutions of the present invention, and cannot be used to limit the protection scope of the present invention.
[0041] Unless otherwise specified, the experimental materials, reagents, methods and instruments used in the following embodiments and comparative examples are conventional materials, reagents, methods and instruments in the art and can be obtained through commercial channels by those skilled in the art.
[0042] Example 1
[0043] (1) 9 g of hydrophilic nano-silica with a particle size of 5 nm was added to a mixed solution consisting of 200 ml of anhydrous ethanol, 20 ml of deionized water, and 10 ml of ammonium hydroxide, and the mixture was uniformly dispersed and heated to 50° C. 1.2 mL of octyltriethoxysilane was added and stirred for 24 h to obtain a mixed solution. The mixed solution was centrifuged at a speed of 8000 r / min in a centrifuge for 15 min, and the hydrophobic nano-silica was obtained after drying. Figure 1 This is the microstructure of the raw material nano-silicon dioxide.
[0044] The hydrophobic modification of micron-mesoporous silica is the same as that of nano-silica. Except that the raw material is micron-mesoporous silica with a particle size of 3 μm, the types, amounts and experimental parameters of other chemical substances are the same as those of the hydrophobic modification process of nano-silica. Figure 2 This is the microstructure of the raw material micron-mesoporous silica.
[0045] (2) 1.2 g of hydrophobic nano-silica and 4 g of hydrophobic micron mesoporous silica were added to 30 g of butyl acetate, placed in a magnetic stirrer and stirred at a speed of 600 r / min for 10 min, and then 6.8 g of bisphenol A epoxy resin was added, and the solution was evenly dispersed to obtain a coating liquid.
[0046] (3) After wiping the acrylic plate with butyl acetate, place it in a drying oven to dry. Use an air compressor and a 1 mm caliber spray gun to evenly spray the coating liquid onto the acrylic plate at a pressure of 2 to 2.4 MPa. Wait for 3 to 5 minutes. After the polar solvent is completely evaporated, place the acrylic plate in a constant temperature drying oven and dry it at 80° C. for 1 hour to obtain a super hydrophobic coating.
[0047] The super-hydrophobic coating obtained in this example was subjected to a wear resistance test, a roughness test, and a contact angle observation. Figure 3 Schematic diagram of the contact angle of the super-hydrophobic coating. It can be seen that the contact angle of the droplet on the coating is 154.2°, which meets the contact angle requirements of the super-hydrophobic coating. Figure 4 This is a friction test diagram of the super hydrophobic coating. During the test, the coating was rubbed back and forth on a friction tester with a load of 150g. Figure 4 It can be seen that as the number of frictions increases, the contact angle decreases, but during the entire 160 frictions and after 160 frictions, the contact angle remains above 150°, indicating that even after multiple frictions, the coating prepared in this embodiment still maintains a superhydrophobic state and has good wear resistance. Figure 5 This is a test chart of the drag reduction rate of the super-hydrophobic coating. The acrylic plate sprayed with the super-hydrophobic coating was placed in a water tank and tested at a flow rate of 0 to 10 m / s. Figure 5 It can be seen that under different flow rates, the drag reduction rate of the super-hydrophobic coating is always maintained above 15%, indicating that the super-hydrophobic coating prepared in this embodiment has excellent drag reduction performance.
[0048] The super-hydrophobic coating obtained in this embodiment was randomly measured at 50 areas using a roughness measuring instrument, and the average roughness was measured to be 4.08 μm, indicating that the super-hydrophobic coating has a low roughness.
[0049] Example 2
[0050] The difference between this embodiment and embodiment 1 is that the silane is perfluorodecyltriethoxysilane, the resin is FEVE fluorocarbon resin, and the remaining process steps and parameter settings are the same as those in embodiment 1.
[0051] The super-hydrophobic coating obtained in this example was tested for wear resistance, drag reduction rate and roughness. Figure 6 This is a friction test diagram of the super hydrophobic coating. The super hydrophobic coating was tested by reciprocating friction on a friction tester with a load of 150g. Figure 6 It can be seen that the contact angle of the super-hydrophobic coating changes with the increase in the number of frictions, but even after 160 frictions, the contact angle of the coating is still above 150°, indicating that the coating prepared in this embodiment can still maintain a super-hydrophobic state and has good wear resistance. Figure 7This is a test chart of the drag reduction rate of the super-hydrophobic coating. During the test, the acrylic plate sprayed with the super-hydrophobic coating was placed in a water tank with a flow rate of 0 to 10 m / s. Figure 7 It can be seen that during the entire test process, the drag reduction rate of the super-hydrophobic coating is always maintained above 15%, indicating that the super-hydrophobic coating prepared in this embodiment has good drag reduction performance. The super-hydrophobic coating obtained in this embodiment is randomly measured in 50 areas by a roughness measuring instrument, and the average roughness is measured to be 4.79 μm. Although the roughness of the super-hydrophobic coating obtained in this embodiment is not as low as that in Example 1, the difference between the two is not large, indicating that the roughness of the super-hydrophobic coating prepared in this embodiment is also low.
[0052] Comparative Example 1
[0053] The difference between this comparative example and Example 2 is that the micron particles are changed into micron silica with non-mesoporous structure, and the particle size thereof is consistent with that of mesoporous silica. The other process steps and parameter settings are the same as those of Example 2.
[0054] The super-hydrophobic coating obtained in this comparative example was subjected to a roughness test. 50 areas were randomly measured using a roughness measuring instrument. The roughness measurement values are shown in Table 1, and the average roughness was 8.58 μm.
[0055] Table 1 Roughness measurement values of super hydrophobic coating
[0056]
[0057]
[0058] The drag reduction rate of the super hydrophobic coating obtained in this comparative example was tested in a water tank at a flow rate of 0 to 10 m / s. The results are as follows: Figure 8 As shown, the test found that the pressure difference of the super-hydrophobic coating is basically consistent with the pressure difference of the smooth flat plate, and there is basically no drag reduction rate. The super-hydrophobic coating obtained in this comparative example was subjected to a wear resistance test. During the test, the coating was reciprocated on a friction tester with a load of 150g. After 160 frictions, the coating remained in a super-hydrophobic state.
[0059] This comparative example shows that mixing hydrophobically modified non-mesoporous micron-silica with nano-silica can make the super-hydrophobic coating have good wear resistance, but no drag reduction performance. This is because the two particles cannot form an "embedded" structure, and their roughness is greater than that of the "embedded" micro-nano particle structure.
[0060] Comparative Example 2
[0061] The difference between this comparative example and Example 2 is that no micron silicon dioxide is added, and the remaining process steps and parameter settings are the same as those of Example 2.
[0062] The super hydrophobic coating obtained in this comparative example was subjected to a roughness test, and 50 areas were randomly measured by a roughness measuring instrument, and the average roughness was measured to be 1.25 μm. The super hydrophobic coating obtained in this comparative example was subjected to a wear resistance test, and the coating was reciprocated on a friction tester with a load of 150 g during the test. After 20 frictions, the coating could not maintain a super hydrophobic state.
[0063] This comparative example shows that the roughness of the super hydrophobic coating prepared without adding micron silicon dioxide is very low. According to the drag reduction rate formula: The results show that the super-hydrophobic coating also has a large drag reduction rate, but the coating is not wear-resistant. This is because the nano-silica will be lost after being worn, and there are no other rigid particles in the coating to withstand friction.
Claims
1. A wear-resistant super-hydrophobic coating with drag reduction performance, characterized in that: The coating is made of hydrophobic nano-silicon dioxide, hydrophobic micron-mesoporous silica and epoxy resin; The mass ratio of the hydrophobic micron mesoporous silica, the hydrophobic nano silica and the epoxy resin is 10:3:17; The hydrophobic nano-silica is obtained by modifying nano-silica, and the hydrophobic micron-mesoporous silica is obtained by modifying micron-mesoporous silica.
2. A wear-resistant super-hydrophobic coating with drag reduction performance according to claim 1, characterized in that: The particle size of the nano silicon dioxide is 5 to 15 nm.
3. A wear-resistant super-hydrophobic coating with drag reduction performance according to claim 1, characterized in that: The micron mesoporous silica particle size is 1 to 10 μm.
4. A wear-resistant super-hydrophobic coating with drag reduction performance according to claim 1, characterized in that: The epoxy resin is bisphenol A epoxy resin, polyacrylate epoxy resin, FEVE fluorocarbon resin or waterborne polyurethane.
5. A method for preparing a wear-resistant super-hydrophobic coating with drag reduction performance according to any one of claims 1 to 4, characterized in that: The steps include: Step 1: respectively adding nano-silica and micro-mesoporous silica to a solution consisting of anhydrous ethanol, deionized water and ammonium hydroxide and heating the solution, then respectively adding silane to obtain two sets of mixed solutions, centrifuging and drying the mixed solutions to obtain hydrophobic nano-silica and hydrophobic micro-mesoporous silica; Step 2: Dispersing hydrophobic nano-silica and hydrophobic micron mesoporous silica in a polar solvent and stirring to obtain a mixed solution, and adding epoxy resin to the mixed solution to obtain a coating solution; Step 3: Spray the coating liquid onto the treated substrate, and dry the substrate after the polar solvent in the coating liquid is completely evaporated to obtain a super hydrophobic coating.
6. The method for preparing a wear-resistant super-hydrophobic coating with drag reduction performance according to claim 5, characterized in that: The silane in step 1 is octyltriethoxysilane, γ-aminopropyltriethoxysilane, γ-methacryloxypropyltrimethoxysilane or perfluorodecyltriethoxysilane.
7. The method for preparing a wear-resistant super-hydrophobic coating with drag reduction performance according to claim 5, characterized in that: In the step 1, the mass ratio of nano-silica to silane is 7:1, and the mass ratio of micron-mesoporous silica to silane is 7:
1.
8. The method for preparing a wear-resistant super-hydrophobic coating with drag reduction performance according to claim 5, characterized in that: In the step 1, the mass ratio of anhydrous ethanol, deionized water and ammonium hydroxide is 10:2:
1.
9. The method for preparing a wear-resistant super-hydrophobic coating with drag reduction performance according to claim 5, characterized in that: In the step 1, the proportion of nano-silicon dioxide in the mixed solution is 5wt%, and the proportion of micron mesoporous silicon dioxide in the mixed solution is 5wt%.
10. The method for preparing a wear-resistant super-hydrophobic coating with drag reduction performance according to claim 5, characterized in that: In the step 2, the sum of the mass of the hydrophobic nano-silica and the hydrophobic micron-mesoporous silica in the coating liquid accounts for 10 wt % to 15 wt %.
Citation Information
Patent Citations
High wearing resistance normal-temperature cured bottom surface syncretic super-hydrophobic coating and preparation method thereof
CN110003735A
Porous powder loaded with super-hydrophobic particles as well as preparation method and application of porous powder
CN113604095A
Preparation method of superamphiphobic porous powder and superamphiphobic coating containing superamphiphobic porous powder
CN116814110A
Cited By
Marine cable with built-in control cable in cable core
CN121355017A
Marine cable with cable core built-in control cable
CN121355017B