Anti-scale and anti-wear polyurea coating as well as preparation method and use method thereof

Through the combination of functionalized graphene-modified polyurea coating and nanopowder, the problem of insufficient anti-scaling and wear resistance of oil pipe coatings is solved, and good anti-scaling and wear resistance in high salinity and microbial medium environments are achieved. The wear-resistant effect extends the service life of oil pipes.

CN118725705AActive Publication Date: 2024-10-01CHINA NAT PETROLEUM CORP +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202310338542.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-01
Estimated Expiration
2043-03-31

AI Technical Summary

Technical Problem

Existing oil pipe coatings have insufficient anti-scaling and wear resistance in environments with high salinity and microbial media, leading to increased pipe damage, and the dispersion problem of graphene in anti-corrosion coatings has not been effectively solved.

Method used

Functionalized graphene modified polyurea coating is used, and components such as partially reduced graphene oxide dispersion are modified by isophorone diisocyanate, polyethylene glycol and nanopowder, combined with α~Al2O3 and YSZ micro-nano powder, to form a The anti-fouling and wear-resistant coating uses modified nano-molybdenum disulfide and modified nano-cerium dioxide to improve the impermeability and hardness of the coating.

Benefits of technology

Significantly improves the anti-scaling and anti-wear properties of the coating, extending the service life of oil pipes. The coating shows excellent anti-corrosion and anti-fouling effects, wear resistance and anti-fouling in high temperature, high pressure and high bacterial content environments. Performance is much higher than traditional coatings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004157331330000201
    Figure BDA0004157331330000201
Patent Text Reader

Abstract

The invention provides an anti-scale and anti-wear polyurea coating as well as a preparation method and a use method thereof, and belongs to the technical field of petroleum drilling and production. The coating comprises a primer and a finish; the finish paint comprises a component A and a component B, wherein the component A comprises isophorone diisocyanate, polyethylene glycol, an alpha-Al2O3 and YSZ nano powder modified partially reduced graphene oxide dispersion liquid, and a mixture of alpha-Al2O3 micro-nano powder and YSZ micro-nano powder; the component B comprises a chain extender, amine-terminated polyether, a diluent, a foaming agent, modified nano molybdenum disulfide and an auxiliary agent; the primer comprises a component C and a component D, and the component C comprises isophorone diisocyanate, polyethylene glycol, cerium dioxide nano powder modified partially reduced graphene oxide dispersion liquid, and a mixture of cerium dioxide micro-nano powder and yttrium oxide stabilized zirconium oxide micro-nano powder; the component D comprises a chain extender, amine-terminated polyether, a diluent, a foaming agent, modified nano cerium dioxide and an auxiliary agent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of petroleum drilling and production, and specifically relates to an anti-scaling and anti-wear polyurea coating and a preparation method and a use method thereof. Background Art

[0002] At present, with the deepening of oil and gas exploration and development, the damage and failure of oil pipes have intensified due to factors such as oil product degradation, which has put forward higher requirements for the corrosion resistance and high temperature resistance of oil pipe anti-corrosion coatings. In addition to the insufficient high temperature resistance and anti-corrosion performance, the poor anti-scaling and wear resistance of the anti-corrosion coating technology used in oil fields has become one of the main factors affecting its long-term service in harsh working conditions. In terms of anti-scaling performance requirements, in addition to corrosive media such as chloride ions and carbon dioxide, high-mineralized formation water also contains microorganisms such as sulfate-reducing bacteria, planktonic bacteria, iron bacteria, and easy-to-scale ions such as calcium ions and magnesium ions. Microorganisms and local scaling and corrosion products deposit and interact on the surface of oil pipe coatings, causing scaling on the surface of oil pipes and causing under-scale corrosion; in addition, the use of chemical flooding, ternary composite flooding and other operating processes in oil fields further aggravates the scaling phenomenon on the surface of oil pipes, increasing the difficulty of subsequent production operations. In terms of wear resistance, the coating faces a multiphase medium environment such as oil, water, gas, and solids. High-speed complex fluids will cause erosion and wear to the coating. In addition, the use of mechanical extraction methods such as sucker rods and submersible pumps, as well as operations such as pipe clearance and periodic pipe inspections, will inevitably cause wear and damage to the coating. Therefore, it is urgent to obtain anti-scaling and wear-resistant coating protection technology that can increase the service life of oil pipes and have stable performance.

[0003] In recent years, polyurea coatings have been widely used in the anti-corrosion field due to their good impact strength, flexibility, waterproofness, corrosion resistance and construction performance. However, the surface of the polyurea coating has a large friction coefficient and does not have anti-fouling functionality. In addition, the coating formed by graphene-modified coatings has attracted widespread attention because of its better anti-corrosion performance. However, the current application of graphene in anti-corrosion coatings requires solving technical problems such as graphene dispersion. Graphene is easy to agglomerate due to its large specific surface area, and it is often necessary to improve its dispersibility in organic solvents through functional modification. Therefore, it is necessary to provide a polyurea coating modified with functionalized graphene, which can greatly improve the anti-fouling and wear resistance of the coating while improving the corrosion resistance and high temperature resistance of the coating. Summary of the invention

[0004] In order to overcome the shortcomings of the above-mentioned prior art, the purpose of the present invention is to provide an anti-fouling and anti-wear polyurea coating and a preparation method and a use method, so as to solve the problem that the existing polyurea coating has a large friction coefficient on its surface and does not have the anti-fouling functionality; the technical difficulties of graphene dispersion in the current application of graphene in anti-corrosion coatings solve the problem that graphene is easy to agglomerate due to its large specific surface area, and obtain a coating with anti-fouling and wear-resistant properties.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions:

[0006] The invention provides an anti-fouling and anti-wear polyurea coating, comprising a primer and a topcoat; the topcoat comprises an A component and a B component, wherein the weight ratio of the A component to the B component is 1:(1.9-2.1); in terms of parts, the raw materials for preparing the A component of the topcoat comprise: 46-61 parts of isophorone diisocyanate, 15-30 parts of polyethylene glycol, 5-15 parts of a dispersion of partially reduced graphene oxide modified by α-Al2O3 nanopowder and yttria-stabilized zirconium oxide nanopowder, and 5-9 parts of a mixture of α-Al2O3 micro-nano powder and yttria-stabilized zirconium oxide micro-nano powder, with a total of 100 parts;

[0007] In terms of parts, the raw materials for preparing component B of the topcoat include: 29 to 32 parts of chain extender, 30 to 39 parts of amino-terminated polyether, 11 to 15 parts of diluent, 6 to 8 parts of foaming agent, 11 to 15 parts of modified nano molybdenum disulfide and 1 to 3 parts of auxiliary agent, with a total of 100 parts;

[0008] The primer comprises a C component and a D component, wherein the weight ratio of the C component to the D component is 1:(1.9-2.1); in terms of parts, the raw materials for preparing the C component of the primer comprise: 46-61 parts of isophorone diisocyanate, 15-30 parts of polyethylene glycol, 5-15 parts of a dispersion of partially reduced graphene oxide modified by cerium dioxide nanopowder, and 5-9 parts of a mixture of cerium dioxide micro-nano powder and yttria-stabilized zirconium oxide micro-nano powder, with a total of 100 parts;

[0009] In terms of parts, the raw materials for preparing component D of the primer include: 29-32 parts of chain extender, 30-39 parts of terminal amino polyether, 11-15 parts of diluent, 6-8 parts of foaming agent, 11-15 parts of modified nano cerium dioxide and 1-3 parts of auxiliary agent, with a total of 100 parts.

[0010] The present invention further comprises that the mass ratio of α-Al2O3 micro-nano powder and yttria-stabilized zirconia micro-nano powder in the mixture of α-Al2O3 micro-nano powder and yttria-stabilized zirconia micro-nano powder is 1:3; the mass ratio of nano powder to micron powder in the α-Al2O3 micro-nano powder is 1:1; and the mass ratio of nano powder to micron powder in the yttria-stabilized zirconia micro-nano powder is 2:1.

[0011] The present invention further comprises that the mass ratio of cerium dioxide micro-nano powder to yttria-stabilized zirconia micro-nano powder in the mixture of cerium dioxide micro-nano powder and yttria-stabilized zirconia micro-nano powder is 2:1; the mass ratio of nano powder to micron powder in the cerium dioxide micro-nano powder is 2:1; and the mass ratio of nano powder to micron powder in the yttria-stabilized zirconia micro-nano powder is 2:1.

[0012] The present invention further comprises: the chain extender is diethyltoluenediamine; the diluent is a mixture of propylene carbonate, n-butyl acetate and n-butanol, and the mass ratio of the propylene carbonate, n-butyl acetate and n-butanol is 3:3:1; the foaming agent is azobisisobutyronitrile; and the auxiliary agents include a leveling agent, a defoaming agent and a dispersant.

[0013] The present invention also provides a method for preparing the anti-fouling and anti-wear polyurea coating according to any one of the above, comprising the following steps:

[0014] S1: mixing isophorone diisocyanate and polyethylene glycol, heating them and reacting them to obtain polymer A, preparing α-Al2O3 nanopowder and yttria-stabilized zirconia nanopowder-modified partially reduced graphene oxide dispersion; adding α-Al2O3 nanopowder and yttria-stabilized zirconia nanopowder-modified partially reduced graphene oxide dispersion, α-Al2O3 micro-nano powder and yttria-stabilized zirconia micro-nano powder to polymer A in sequence, stirring to obtain component A of topcoat;

[0015] S2: preparing modified nano molybdenum disulfide, mixing a chain extender, an amino-terminated polyether, a diluent, a foaming agent, and the modified nano molybdenum disulfide, stirring and heating, and then adding an auxiliary agent and mixing evenly to obtain component B of the topcoat;

[0016] S3: preparing a dispersion of partially reduced graphene oxide modified by cerium dioxide nanopowder; sequentially adding a mixture of the dispersion of partially reduced graphene oxide modified by cerium dioxide nanopowder, cerium dioxide micro-nano powder and yttria-stabilized zirconium oxide micro-nano powder to polymer A, and stirring to obtain component C of the primer;

[0017] S4: preparing modified nano-cerium dioxide, mixing a chain extender, an amino-terminated polyether, a diluent, a foaming agent, and the modified nano-cerium dioxide, stirring and heating the mixture, and then adding an auxiliary agent and mixing the mixture evenly to obtain a D component of the primer;

[0018] S5: evenly mix the prepared component A of the topcoat and the component B of the topcoat to prepare a topcoat; evenly mix the prepared component C of the primer and the component D of the primer to prepare a primer, wherein the topcoat and the primer are anti-fouling and anti-wear polyurea coatings for oil and gas well pipes.

[0019] The present invention further comprises that in S1, the process of preparing the dispersion of α-Al2O3 nanopowder and yttria-stabilized zirconium oxide nanopowder modified partially reduced graphene oxide is as follows:

[0020] The method comprises the following steps: mixing trimethylsiloxane with partially reduced graphene oxide X, and performing a first modification reaction to obtain a mixed solution a; adding α-Al2O3 nanopowder and yttria-stabilized zirconia nanopowder to the mixed solution a, and reacting to obtain a mixed solution b; drying the mixed solution b to obtain partially reduced graphene oxide modified with α-Al2O3 nanopowder and yttria-stabilized zirconia nanopowder, and then sequentially adding n-butanol, polydimethylsiloxane and a silane coupling agent to the partially reduced graphene oxide modified with α-Al2O3 nanopowder and yttria-stabilized zirconia nanopowder, performing a second modification reaction and performing ultrasonic treatment, and finally obtaining a dispersion of partially reduced graphene oxide modified with α-Al2O3 nanopowder and yttria-stabilized zirconia nanopowder;

[0021] The mass ratio of the α-Al2O3 nanopowder to the yttria-stabilized zirconia nanopowder is 1:2;

[0022] The oxygen content of the partially reduced graphene oxide X is 10%.

[0023] The present invention further, in said S2, the process of preparing modified nano molybdenum disulfide is as follows:

[0024] Mixing nano-molybdenum disulfide, n-butanol and anhydrous ethanol, adjusting the pH value to neutral to obtain a nano-molybdenum disulfide suspension; mixing vinyl triethoxysilane and the nano-molybdenum disulfide suspension, and then adding partially reduced graphene oxide Y to react to obtain a modified nano-molybdenum disulfide dispersion, filtering, and vacuum drying to obtain the modified nano-molybdenum disulfide;

[0025] The volume ratio of the vinyl triethoxysilane to the nano-molybdenum disulfide suspension is 1:10;

[0026] The oxygen content of the partially reduced graphene oxide Y is 15%.

[0027] The present invention further, in said S3, the process of preparing the cerium dioxide nanopowder modified partially reduced graphene oxide dispersion is as follows:

[0028] The trimethylsiloxane and the partially reduced graphene oxide X are mixed to carry out a first modification reaction to obtain a mixed solution a; the cerium dioxide nanopowder is added to the mixed solution a to react to obtain a mixed solution c; the mixed solution b is dried to obtain the cerium dioxide nanopowder modified partially reduced graphene oxide, and then n-butanol, polydimethylsiloxane and a silane coupling agent are sequentially added to the cerium dioxide nanopowder modified partially reduced graphene oxide, a second modification reaction is carried out and ultrasonic treatment is performed to obtain a cerium dioxide nanopowder modified partially reduced graphene oxide dispersion;

[0029] The oxygen content of the partially reduced graphene oxide X is 10%.

[0030] The present invention further states that in S4, the process of preparing the modified nano-cerium dioxide is as follows:

[0031] Mixing nano-cerium disulfide, n-butanol and anhydrous ethanol, adjusting the pH value to neutral to obtain a nano-cerium disulfide suspension, mixing vinyl triethoxysilane and the nano-cerium disulfide suspension, adding partially reduced graphene oxide Y, reacting to obtain a modified nano-cerium disulfide dispersion, and then filtering and vacuum drying to obtain modified nano-cerium dioxide;

[0032] The volume ratio of the vinyl triethoxysilane to the nano-cerium disulfide suspension is 1:10;

[0033] The oxygen content of the partially reduced graphene oxide Y is 15%.

[0034] The present invention provides a method for using the anti-scaling and anti-wear polyurea coating, wherein the polyurea coating is used for anti-scaling and anti-wear of oil and gas well pipes, and the method for using is as follows:

[0035] The primer in the polyurea coating is coated on the pretreated substrate and then cured to obtain a substrate coated with the primer; the topcoat is coated on the substrate coated with the primer and then cured to form an anti-fouling and anti-wear polyurea coating.

[0036] Compared with the prior art, the present invention has the following beneficial effects:

[0037] The invention provides a method for preparing an anti-fouling and anti-wear polyurea coating. In the topcoat, trimethylsiloxane is firstly used to graft and modify partially reduced graphene oxide X, and then nanoparticles α-Al2O3 and YSZ (yttria-stabilized zirconia) are used to graft and react with trimethylsiloxane, polydimethylsiloxane, silane coupling agent and the like in a highly surface active state due to their unique surface effect and small size effect. The modified partially reduced graphene oxide is coated on the α-Al2O3 and YSZ nanoparticles in a manner of sharing "O" atoms, thereby achieving the beneficial effects of efficient dispersion and organic fusion of organic materials and inorganic materials (partially reduced graphene oxide, α-Al2O3 and YSZ).

[0038] Furthermore, through the requirements of the coating nanofiller's impermeability, wear resistance, corrosion resistance, pore filling, density mismatch design (anti-settling), and organic combination with the organic coating, after material structure design and experimental verification, a partially reduced graphene oxide X with an oxygen content of 10% is used as a raw material, and the hydroxyl and carboxyl groups retained in the partially reduced graphene oxide are used to undergo a coupling reaction with trimethylsiloxane, polydimethylsiloxane, and a silane coupling agent, and a modified partially reduced graphene oxide is prepared. While achieving efficient dispersion and fusion of organic and inorganic materials, the beneficial effects of high impermeability, corrosion resistance, high toughness, super hydrophobicity, self-lubrication, and sterilization and anti-scaling of the partially reduced graphene oxide are retained.

[0039] The invention provides an anti-scaling and anti-wear polyurea coating for oil and gas well pipes. The topcoat contains α-Al2O3 and YSZ micro-nano powders, modified nano molybdenum disulfide, and reduced graphene oxide. These micro-nano particles / nano sheets with different particle sizes effectively block gaps of different sizes in the coating through size mismatch, thereby improving the impermeability and corrosion resistance of the coating; in addition, the α-Al2O3 and YSZ micro-nano powders effectively improve the hardness and strength of the coating, thereby improving the wear resistance and impact resistance of the coating; in addition, the topcoat also takes into account the self-lubricating performance of the modified nano molybdenum disulfide, thereby further improving the wear resistance of the coating. The primer contains modified partially reduced graphene oxide, cerium dioxide (CeO2) and YSZ micro-nano powder, and modified nano cerium dioxide. In addition to the corrosion resistance, hydrophobicity, wear resistance and performance advantages of the topcoat, cerium dioxide has a unique oxygen storage capacity and can absorb free oxygen that diffuses into the coating through the topcoat, preventing the free oxygen from further entering the interface between the oil pipe and the coating, greatly improving the corrosion resistance of the coating.

[0040] Furthermore, after the CeO2, α~Al2O3 and YSZ ceramics or rare earth oxide micro-nanoparticles are organically composited with partially reduced graphene oxide, the average density is close to that of the resin matrix, which effectively solves the problem of single b-RGO floating in the coating and single CeO2, α~Al2O3 and YSZ ceramics or rare earth oxide micro-nanoparticles sinking in the coating.

[0041] Furthermore, according to the characteristics of different nanopowders, two types of partially reduced graphene oxide, X and Y, with different oxygen contents were used, so that the graphene surface had sufficient and appropriate functional groups to participate in the grafting reaction.

[0042] The present invention provides a method for using an anti-scaling and anti-wear polyurea coating for oil and gas well pipes. The present invention accurately designs the precise control of each coating component and the coating preparation process according to the service condition requirements of the oil and gas well pipes and in combination with the functional differences of each component. Under high pressure (up to 100Mpa), high mineralization (no more than 200,000 ppm), and high bacterial content (no more than 50,000 / ml), the unexpected long-term service (more than 6 years) effect is achieved on the surface of the oil and gas well pipe at a temperature of 160°C. The wear resistance index is in accordance with the SY / T 6717-2016 (Technical Conditions for Inner Coatings of Oil Pipes and Casings) standard. The wear resistance index of the coating measured by the falling sand method is higher than 3.5L / μm, which is much higher than the wear resistance index requirement of 2L / μm in the standard. The anti-scaling performance index is in accordance with the T / CSTM 00242-2021 (Quality Requirements and Inspection of Graphene Modified Coatings for Oil Pipes) standard. The anti-scaling grade of the coating measured by the weight gain method is 1 (<0.5mg / cm 2 ), which is much higher than the conventional oil pipe anti-corrosion coating level 2 (0.5mg / cm 2 ~ 1.0mg / cm 2 ) or level 3 (1.0 mg / cm 2 ~ 1.5mg / cm 2 ) performance.

[0043] The coating of the present invention has a temperature resistance of up to 180°C and has excellent anti-scaling and wear-resistant properties in drilling and mining conditions at or below 160°C. DETAILED DESCRIPTION

[0044] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used in the text are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definition in this specification shall prevail.

[0045] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.

[0046] Herein, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are for simplicity and convenience only. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible secondary ranges and individual values ​​within the range (including integers and fractions).

[0047] In this document, unless otherwise specified, “includes,” “including,” “contains,” “has,” or similar terms cover the meanings of “consisting of” and “mainly consisting of,” for example, “A includes a” covers the meanings of “A includes a and other” and “A only includes a.”

[0048] In this document, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.

[0049] The invention provides an anti-scaling and anti-wear polyurea coating and a preparation method and a use method thereof.

[0050] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.

[0051] The following examples use conventional instruments and equipment in the art. The experimental methods in the following examples where specific conditions are not specified are usually carried out under conventional conditions or under conditions recommended by the manufacturer. The various raw materials used in the following examples are conventional commercial products unless otherwise specified, and their specifications are conventional specifications in the art. In the specification of the present invention and the following examples, unless otherwise specified, "%" means weight percentage, "part" means weight part, and ratio means weight ratio.

[0052] The invention provides an anti-fouling and anti-wear polyurea coating, which comprises a primer and a topcoat, wherein the topcoat is arranged above the primer, the topcoat consists of an A component and a B component, and the primer consists of a C component and a D component; the weight ratio of the A component to the B component of the topcoat and the C component to the D component of the primer are both 1:(1.9-2.1), that is, the weight ratio of the A component to the B component of the topcoat is 1:(1.9-2.1), and the weight ratio of the C component to the D component of the primer is 1:(1.9-2.1).

[0053] In terms of parts, the raw materials for preparing component A of the topcoat include: 46-61 parts of isophorone diisocyanate, 15-30 parts of polyethylene glycol, 5-15 parts of α-Al2O3 nanopowder and yttria-stabilized zirconium oxide nanopowder modified partially reduced graphene oxide dispersion, 5-9 parts of a mixture of α-Al2O3 micro-nano powder and yttria-stabilized zirconium oxide (YSZ) micro-nano powder, with a total of 100 parts; the raw materials for preparing component B include: 29-32 parts of chain extender, 30-39 parts of terminal amino polyether, 11-15 parts of diluent, 6-8 parts of foaming agent, 11-15 parts of modified nano molybdenum disulfide and 1-3 parts of auxiliary agent, with a total of 100 parts;

[0054] The mass ratio of α-Al2O3 micro-nano powder and yttria-stabilized zirconia micro-nano powder in the mixture of α-Al2O3 micro-nano powder and yttria-stabilized zirconia micro-nano powder is 1:3; the mass ratio of nano powder to micron powder in the α-Al2O3 micro-nano powder is 1:1; the mass ratio of nano powder to micron powder in the yttria-stabilized zirconia micro-nano powder is 2:1; the particle size of the nano powder in the α-Al2O3 micro-nano powder is 10-80nm, and the particle size of the micron powder in the α-Al2O3 micro-nano powder is 0.5-3μm; the particle size of the nano powder in the yttria-stabilized zirconia micro-nano powder is 20-50nm, and the particle size of the micron powder in the yttria-stabilized zirconia micro-nano powder is 0.5-2μm; the particle size of the nano molybdenum disulfide is 30-60nm.

[0055] Calculated by parts, the raw materials for preparing component C of the primer include: 46 to 61 parts of isophorone diisocyanate, 15 to 30 parts of polyethylene glycol, 5 to 15 parts of cerium dioxide nanopowder modified partially reduced graphene oxide dispersion, 5 to 9 parts of a mixture of cerium dioxide micro (CeO2) nanopowder and yttria-stabilized zirconium oxide micro-nano powder, totaling 100 parts; the raw materials for preparing component D of the primer include: 29 to 32 parts of chain extender, 30 to 39 parts of terminal amino polyether, 11 to 15 parts of diluent, 6 to 8 parts of foaming agent, 11 to 15 parts of modified nano cerium dioxide and 1 to 3 parts of auxiliary agent, totaling 100 parts.

[0056] The mass ratio of cerium dioxide micro-nano powder and yttria-stabilized zirconia micro-nano powder in the mixture of cerium dioxide micro-nano powder and yttria-stabilized zirconia micro-nano powder is 2:1; the mass ratio of nano powder to micron powder in the cerium dioxide micro-nano powder is 2:1; the mass ratio of nano powder to micron powder in the yttria-stabilized zirconia micro-nano powder is 2:1; the particle size of the nano powder in the cerium dioxide micro-nano powder is 10-50nm, and the particle size of the micron powder in the cerium dioxide micro-nano powder is 0.5-2μm; the particle size of the nano powder in the yttria-stabilized zirconia micro-nano powder is 30-80nm, and the particle size of the micron powder in the yttria-stabilized zirconia micro-nano powder is 0.5-3μm; the particle size of the modified nano cerium dioxide is 30-80nm.

[0057] The chain extender is preferably diethyltoluenediamine; the diluent is preferably a mixture of propylene carbonate, n-butyl acetate and n-butanol in a mass ratio of 3:3:1; the foaming agent is preferably azobisisobutyronitrile; and the auxiliary agents include a leveling agent, a defoaming agent and a dispersant.

[0058] The present invention also provides a method for preparing an anti-fouling and anti-wear polyurea coating, comprising the following steps:

[0059] Raw material preparation: preparing isophorone diisocyanate, modified partially reduced graphene oxide slurry, i.e., α-Al2O3 nanopowder and yttria-stabilized zirconia nanopowder modified partially reduced graphene oxide dispersion, cerium dioxide nanopowder modified partially reduced graphene oxide dispersion, amino-terminated polyether, modified nano-molybdenum disulfide, and modified nano-cerium dioxide.

[0060] S1: 46-61 parts of isophorone diisocyanate and 15-30 parts of polyethylene glycol are mixed, heated to 50-70°C, and reacted for 4-6 hours to obtain polymer A, and α-Al2O3 nanopowder and yttria-stabilized zirconia nanopowder-modified partially reduced graphene oxide dispersion are prepared; 5-15 parts of α-Al2O3 nanopowder and yttria-stabilized zirconia nanopowder-modified partially reduced graphene oxide dispersion, and 5-9 parts of a mixture of α-Al2O3 micro-nano powder and yttria-stabilized zirconia micro-nano powder are added to polymer A in sequence, and stirred at 2100-2500 r / min for 2-3 hours to obtain topcoat component A, wherein the viscosity of topcoat component A is 900-1000 mPa·s;

[0061] S2: 29-32 parts of chain extender, 30-39 parts of amino-terminated polyether, 11-15 parts of diluent, 6-8 parts of foaming agent and 11-15 parts of modified nano molybdenum disulfide are mixed and stirred at 2100-2500 r / min for 20-30 min, then heated at 90-102° C. for 3-4 h, and then the auxiliary agent is added, and stirred at 2100-2500 r / min for 20-30 min to obtain topcoat component B;

[0062] Mixing of components A and B: Mix components A and B evenly at 50-70°C.

[0063] S3: adding 5 to 15 parts of a dispersion of partially reduced graphene oxide modified with cerium dioxide nanopowder and 5 to 9 parts of a mixture of cerium dioxide micro-nano powder and yttria-stabilized zirconium oxide micro-nano powder to polymer A in sequence, stirring at 2100 to 2500 r / min for 2 to 3 hours to obtain a primer C component, wherein the viscosity of the primer C component is 900 to 1000 mPa·s;

[0064] S4: Mix 29-32 parts of chain extender, 30-39 parts of terminal amino polyether, 11-15 parts of diluent, 6-8 parts of foaming agent and 11-15 parts of modified nano cerium dioxide, stir at 2100-2500r / min for 20-30min, then heat at 90-102°C for 3-4h, add auxiliary agent, stir at 2100-2500r / min for 20-30min to obtain primer D component; CD component mixing: at 50-70°C, mix component C and component D evenly, the topcoat and primer are anti-fouling and anti-wear polyurea coatings for oil and gas well pipes.

[0065] The process of preparing α-Al2O3 nanopowder and yttria-stabilized zirconia nanopowder modified partially reduced graphene oxide dispersion is as follows:

[0066] At 25-30° C., trimethylsiloxane and partially reduced graphene oxide X are mixed in a volume weight ratio of 100 mL: 1 g, and a first modification reaction is performed for 25-30 min to obtain a mixed solution a; 3 g of α-Al2O3 nanopowder and yttria-stabilized zirconia nanopowder are added to the mixed solution a, and the mixture is reacted at 80-100° C. for 5-8 h to obtain a mixed solution b; wherein the α-Al2O3 and YSZ nanopowders are mixed in a mass ratio of 1:2, wherein the particle size of the α-Al2O3 nanopowder is 10-80 nm, and the particle size of the YSZ nanopowder is 20-50 nm; the mixed solution b is heated at 90-100° C. The reaction mixture was dried for 9 to 12 h at 40 ° C. to obtain α-Al2O3 nanopowder and yttria-stabilized zirconia nanopowder-modified partially reduced graphene oxide, and then 50 mL of n-butanol, 100 mL of polydimethylsiloxane and 50 mL of silane coupling agent were added to the α-Al2O3 nanopowder and yttria-stabilized zirconia nanopowder-modified partially reduced graphene oxide at 50 to 80 ° C. to carry out a second modification reaction for 60 to 80 min, and then ultrasonically treated at 55 to 60 kHz for 60 to 80 min to obtain an α-Al2O3 nanopowder and yttria-stabilized zirconia nanopowder-modified partially reduced graphene oxide dispersion.

[0067] The mass ratio of the α-Al2O3 nanopowder to the yttria-stabilized zirconium oxide nanopowder is 1:2; the oxygen content of the partially reduced graphene oxide X is 10%, and the specific surface area is 150-250 g / m 2 , particle size is 3 to 5 μm.

[0068] The process of preparing modified nano-molybdenum disulfide is as follows:

[0069] Nano molybdenum disulfide, n-butanol and anhydrous ethanol are mixed in a mass volume ratio of 30g:50mL and 100mL, and then stirred at a speed of 1600-1800r / min for 30min, and then ammonia water is used to adjust the pH value to neutral to obtain a nano molybdenum disulfide suspension, and then vinyl triethoxysilane and the nano molybdenum disulfide suspension are mixed in a volume ratio of 10:100, 2g of partially reduced graphene oxide Y is added, and then the reaction is carried out at a temperature of 50-60°C and a speed of 1000-1500r / min for 18-22h to obtain a modified nano molybdenum disulfide dispersion, the dispersion is filtered, and then dried at 80-100°C for 3h in a vacuum environment to obtain modified nano molybdenum disulfide.

[0070] The volume ratio of the vinyl triethoxysilane and the nano molybdenum disulfide suspension is 1:10; the oxygen content of the partially reduced graphene oxide Y is 15%, and the specific surface area is 100-200 g / m 2 , particle size is 0.5~3μm.

[0071] The process of preparing the cerium dioxide nanopowder modified partially reduced graphene oxide dispersion is as follows:

[0072] At 25-30° C., trimethylsiloxane and partially reduced graphene oxide X are mixed in a volume weight ratio of 100 mL:1 g, and a first modification reaction is carried out for 25-30 min to obtain a mixed solution a; 3 g of cerium dioxide nanopowder is added to the mixed solution a, and the mixture is reacted at 80-100° C. for 5-8 h to obtain a mixed solution c; the mixed solution c is dried at 90-100° C. for 9-12 h to obtain cerium dioxide nanopowder modified partially reduced graphene oxide, and then 50 mL of n-butanol, 100 mL of polydimethylsiloxane and 50 mL of silane coupling agent are sequentially added to the cerium dioxide nanopowder modified partially reduced graphene oxide at 50-80° C., a second modification reaction is carried out for 60-80 min, and then an ultrasonic treatment is carried out at 55-60 kHz for 60-80 min to obtain a cerium dioxide nanopowder modified partially reduced graphene oxide dispersion.

[0073] The oxygen content of the partially reduced graphene oxide X is 10%.

[0074] The process of preparing modified nano-cerium dioxide is as follows:

[0075] Nano-cerium disulfide, n-butanol and anhydrous ethanol are mixed in a mass volume ratio of 30g:50mL and 100mL, and then stirred at a speed of 1600-1800r / min for 30min, and then ammonia water is used to adjust the pH value to neutral to obtain a nano-cerium disulfide suspension, and then vinyl triethoxysilane and the nano-cerium disulfide suspension are mixed in a volume ratio of 10:100, 2g of partially reduced graphene oxide Y is added, and then the reaction is carried out at a temperature of 50-60°C and a speed of 1000-1500r / min for 18-22h to obtain a modified nano-cerium disulfide dispersion, the dispersion is filtered, and then dried at 80-100°C for 3h in a vacuum environment to obtain the modified nano-cerium disulfide.

[0076] The volume ratio of the vinyl triethoxysilane to the nano-cerium disulfide suspension is 1:10; the oxygen content of the partially reduced graphene oxide Y is 15%, and the specific surface area is 100-200 g / m 2 , particle size is 0.5~3μm.

[0077] The present invention also provides a method for using the anti-scaling and anti-wear polyurea coating for oil and gas well pipes in the anti-corrosion and anti-scaling of oil and gas well pipes. The method for using the anti-scaling and anti-wear polyurea coating for oil and gas well pipes is as follows: spray the primer for the anti-scaling and anti-wear polyurea coating for oil and gas well pipes onto the pretreated substrate, and cure it at 100-140°C for 40-60min; then spray the topcoat onto the substrate coated with the primer, and cure it at 100-140°C for 1.5-2h to form a coating. The coating is used in the surface coating of oil and gas well pipes.

[0078] The purpose of the present invention is to provide an anti-fouling and anti-wear polyurea coating and a preparation method and a use method thereof, so as to solve the problem that the existing polyurea coating is far from reaching a super-hydrophobic surface, and its surface has a large friction coefficient, cannot promote the rolling of droplets, delay the crystallization process, and reduce the adhesion of scale to the substrate after crystallization, so it does not have the anti-fouling functionality.

[0079] Example 1

[0080] The weight ratio of component A to component B of the topcoat is 1:1.9; the weight ratio of component C to component D of the primer is 1:2.1;

[0081] The raw materials for preparing component A of the topcoat include: 60 parts of isophorone diisocyanate, 20 parts of polyethylene glycol, 15 parts of α-Al2O3 nano powder and yttria-stabilized zirconium oxide nano powder modified partially reduced graphene oxide dispersion, 5 parts of a mixture of α-Al2O3 micro-nano powder and yttria-stabilized zirconium oxide (YSZ) micro-nano powder; the raw materials for preparing component B include: 29 parts of chain extender, 39 parts of terminal amino polyether, 11 parts of diluent, 6 parts of foaming agent, 14 parts of modified nano molybdenum disulfide and 1 part of auxiliary agent;

[0082] The raw materials for preparing component C of the primer include: 60 parts of isophorone diisocyanate, 20 parts of polyethylene glycol, 15 parts of cerium dioxide nanopowder modified partially reduced graphene oxide dispersion, and 5 parts of a mixture of cerium dioxide micro (CeO2) nanopowder and yttria-stabilized zirconium oxide micro-nano powder; the raw materials for preparing component D of the primer include: 29 parts of a chain extender, 39 parts of terminal amino polyether, 11 parts of a diluent, 6 parts of a foaming agent, 14 parts of modified nano cerium dioxide and 1 part of an auxiliary agent.

[0083] The preparation process is as follows:

[0084] S1: 60 parts of isophorone diisocyanate and 20 parts of polyethylene glycol were mixed, heated to 50°C, and reacted for 4 hours to obtain polymer A, and α-Al2O3 nanopowder and yttria-stabilized zirconia nanopowder-modified partially reduced graphene oxide dispersion were prepared; 15 parts of α-Al2O3 nanopowder and yttria-stabilized zirconia nanopowder-modified partially reduced graphene oxide dispersion and 5 parts of a mixture of α-Al2O3 micro-nano powder and yttria-stabilized zirconia micro-nano powder were added to polymer A in sequence, and stirred at 2100 r / min for 2 hours to obtain topcoat component A, wherein the viscosity of topcoat component A is 900 mPa·s;

[0085] S2: 29 parts of chain extender, 39 parts of amino-terminated polyether, 11 parts of diluent, 6 parts of foaming agent and 14 parts of modified nano molybdenum disulfide were mixed and stirred at 2100 r / min for 20 min, then heated at 90°C for 3 h, 1 part of auxiliary agent was added, and stirred at 2100 r / min for 20 min to obtain topcoat component B;

[0086] Mixing of components A and B: At 50°C, mix component A and component B evenly.

[0087] S3: 15 parts of a dispersion of partially reduced graphene oxide modified with cerium dioxide nanopowder and 5 parts of a mixture of cerium dioxide micro-nano powder and yttria-stabilized zirconium oxide micro-nano powder were added to polymer A in sequence, and the mixture was stirred at 2100 r / min for 2 h to obtain a primer C component, wherein the viscosity of the primer C component was 900 mPa·s;

[0088] S4: 29 parts of chain extender, 39 parts of amino-terminated polyether, 11 parts of diluent, 6 parts of foaming agent and 14 parts of modified nano-cerium dioxide are mixed, and the mixture is stirred at 2100 r / min for 20 min. After that, 1 part of auxiliary agent is added after heating at 90°C for 3 h, and the mixture is stirred at 2100 r / min for 20 min to obtain primer D component; CD component mixing: at 50°C, component C and component D are mixed evenly. The topcoat and primer are anti-fouling and anti-wear polyurea coatings for oil and gas well pipes.

[0089] Example 2

[0090] The weight ratio of component A to component B of the topcoat is 1:2.0; the weight ratio of component C to component D of the primer is 1:2.0;

[0091] The raw materials for preparing component A of the topcoat include: 46 parts of isophorone diisocyanate, 30 parts of polyethylene glycol, 15 parts of α-Al2O3 nano powder and yttria-stabilized zirconium oxide nano powder modified partially reduced graphene oxide dispersion, 9 parts of a mixture of α-Al2O3 micro-nano powder and yttria-stabilized zirconium oxide (YSZ) micro-nano powder; the raw materials for preparing component B include: 32 parts of chain extender, 30 parts of amino-terminated polyether, 15 parts of diluent, 8 parts of foaming agent, 14 parts of modified nano molybdenum disulfide and 1 part of auxiliary agent;

[0092] The raw materials for preparing component C of the primer include: 46 parts of isophorone diisocyanate, 30 parts of polyethylene glycol, 15 parts of cerium dioxide nanopowder modified partially reduced graphene oxide dispersion, and 9 parts of a mixture of cerium dioxide micro (CeO2) nanopowder and yttria-stabilized zirconium oxide micro-nano powder; the raw materials for preparing component D of the primer include: 32 parts of a chain extender, 30 parts of terminal amino polyether, 15 parts of a diluent, 8 parts of a foaming agent, 14 parts of modified nano cerium dioxide and 1 part of an auxiliary agent.

[0093] The preparation process is as follows:

[0094] S1: 46 parts of isophorone diisocyanate and 30 parts of polyethylene glycol are mixed, heated to 70°C, and reacted for 6 hours to obtain polymer A, and α-Al2O3 nanopowder and yttria-stabilized zirconia nanopowder-modified partially reduced graphene oxide dispersion are prepared; 15 parts of α-Al2O3 nanopowder and yttria-stabilized zirconia nanopowder-modified partially reduced graphene oxide dispersion, and 9 parts of a mixture of α-Al2O3 micro-nano powder and yttria-stabilized zirconia micro-nano powder are added to polymer A in sequence, and stirred at 2500 r / min for 3 hours to obtain topcoat component A, wherein the viscosity of topcoat component A is 1000 mPa·s;

[0095] S2: 32 parts of chain extender, 30 parts of amino-terminated polyether, 15 parts of diluent, 8 parts of foaming agent and 14 parts of modified nano molybdenum disulfide were mixed and stirred at 2500 r / min for 30 min, then heated at 102° C. for 4 h, 1 part of auxiliary agent was added, and stirred at 2500 r / min for 30 min to obtain topcoat component B;

[0096] Mixing of components A and B: At 70°C, mix component A and component B evenly.

[0097] S3: 15 parts of a dispersion of partially reduced graphene oxide modified with cerium dioxide nanopowder and 9 parts of a mixture of cerium dioxide micro-nano powder and yttria-stabilized zirconium oxide micro-nano powder were added to polymer A in sequence, and stirred at 2500 r / min for 3 hours to obtain a primer C component, wherein the viscosity of the primer C component was 1000 mPa·s;

[0098] S4: Mix 32 parts of chain extender, 30 parts of terminal amino polyether, 15 parts of diluent, 8 parts of foaming agent and 14 parts of modified nano cerium dioxide, stir at 2500r / min for 30min, then heat at 102°C for 4h, add auxiliary agent, and stir at 2500r / min for 30min to obtain primer D component; CD component mixing: at 70°C, mix component C and component D evenly. The topcoat and primer are anti-fouling and anti-wear polyurea coatings for oil and gas well pipes.

[0099] Example 3

[0100] The weight ratio of component A to component B of the topcoat is 1:2.1; the weight ratio of component C to component D of the primer is 1:1.9;

[0101] The raw materials for preparing component A of the topcoat include: 55 parts of isophorone diisocyanate, 30 parts of polyethylene glycol, 10 parts of α-Al2O3 nano powder and yttria-stabilized zirconium oxide nano powder modified partially reduced graphene oxide dispersion, 5 parts of a mixture of α-Al2O3 micro-nano powder and yttria-stabilized zirconium oxide (YSZ) micro-nano powder; the raw materials for preparing component B include: 29 parts of chain extender, 37 parts of amino-terminated polyether, 14 parts of diluent, 6 parts of foaming agent, 11 parts of modified nano molybdenum disulfide and 3 parts of auxiliary agent;

[0102] The raw materials for preparing component C of the primer include: 55 parts of isophorone diisocyanate, 30 parts of polyethylene glycol, 10 parts of cerium dioxide nanopowder modified partially reduced graphene oxide dispersion, and 5 parts of a mixture of cerium dioxide micro (CeO2) nanopowder and yttria-stabilized zirconium oxide micro-nano powder; the raw materials for preparing component D of the primer include: 29 parts of a chain extender, 37 parts of terminal amino polyether, 14 parts of a diluent, 6 parts of a foaming agent, 11 parts of modified nano cerium dioxide and 3 parts of an auxiliary agent.

[0103] The preparation process is as follows:

[0104] S1: 55 parts of isophorone diisocyanate and 30 parts of polyethylene glycol were mixed, heated to 70°C, and reacted for 6 hours to obtain polymer A, and α-Al2O3 nanopowder and yttria-stabilized zirconia nanopowder-modified partially reduced graphene oxide dispersion were prepared; 10 parts of α-Al2O3 nanopowder and yttria-stabilized zirconia nanopowder-modified partially reduced graphene oxide dispersion and 5 parts of a mixture of α-Al2O3 micro-nano powder and yttria-stabilized zirconia micro-nano powder were added to polymer A in sequence, and stirred at 2100 r / min for 2.5 hours to obtain topcoat component A, wherein the viscosity of topcoat component A is 1000 mPa·s;

[0105] S2: 29 parts of chain extender, 37 parts of amino-terminated polyether, 14 parts of diluent, 6 parts of foaming agent and 11 parts of modified nano molybdenum disulfide were mixed and stirred at 2100 r / min for 30 min, then heated at 90-102° C. for 3-4 h, 3 parts of auxiliary agent were added, and stirred at 2500 r / min for 30 min to obtain topcoat component B;

[0106] Mixing of components A and B: At 70°C, mix component A and component B evenly.

[0107] S3: 10 parts of a dispersion of partially reduced graphene oxide modified with cerium dioxide nanopowder and 5 parts of a mixture of cerium dioxide micro-nano powder and yttria-stabilized zirconium oxide micro-nano powder were added to polymer A in sequence, and stirred at 2500 r / min for 3 hours to obtain a primer C component, wherein the viscosity of the primer C component was 1000 mPa·s;

[0108] S4: 29 parts of chain extender, 37 parts of amino-terminated polyether, 14 parts of diluent, 6 parts of foaming agent and 11 parts of modified nano-cerium dioxide are mixed and stirred at 2100r / min for 30min, then heated at 102°C for 3-4h, and then the auxiliary agent is added and stirred at 2500r / min for 30min to obtain primer D component; CD component mixing: at 70°C, component C and component D are mixed evenly. The topcoat and primer are anti-fouling and anti-wear polyurea coatings for oil and gas well pipes.

[0109] Example 4

[0110] The weight ratio of component A to component B of the topcoat is 1:2.1; the weight ratio of component C to component D of the primer is 1:1.9;

[0111] The raw materials for preparing component A of the topcoat include: 60 parts of isophorone diisocyanate, 16 parts of polyethylene glycol, 15 parts of α-Al2O3 nano powder and yttria-stabilized zirconium oxide nano powder modified partially reduced graphene oxide dispersion, 9 parts of a mixture of α-Al2O3 micro-nano powder and yttria-stabilized zirconium oxide (YSZ) micro-nano powder; the raw materials for preparing component B include: 32 parts of chain extender, 30 parts of amino-terminated polyether, 15 parts of diluent, 7 parts of foaming agent, 15 parts of modified nano molybdenum disulfide and 1 part of auxiliary agent;

[0112] The raw materials for preparing component C of the primer include: 60 parts of isophorone diisocyanate, 16 parts of polyethylene glycol, 15 parts of cerium dioxide nanopowder modified partially reduced graphene oxide dispersion, and 9 parts of a mixture of cerium dioxide micro (CeO2) nanopowder and yttria-stabilized zirconium oxide micro-nano powder; the raw materials for preparing component D of the primer include: 32 parts of a chain extender, 30 parts of terminal amino polyether, 15 parts of a diluent, 7 parts of a foaming agent, 15 parts of modified nano cerium dioxide and 1 part of an auxiliary agent.

[0113] The preparation process is as follows:

[0114] S1: 60 parts of isophorone diisocyanate and 16 parts of polyethylene glycol were mixed, the temperature was raised to 60°C, and the mixture was reacted for 5 hours to obtain polymer A, and a dispersion of partially reduced graphene oxide modified by α-Al2O3 nanopowder and yttria-stabilized zirconia nanopowder was prepared; 15 parts of a dispersion of partially reduced graphene oxide modified by α-Al2O3 nanopowder and yttria-stabilized zirconia nanopowder, and 9 parts of a mixture of α-Al2O3 micro-nano powder and yttria-stabilized zirconia micro-nano powder were added to polymer A in sequence, and the mixture was stirred at 2500 r / min for 3 hours to obtain a topcoat component A, wherein the viscosity of the topcoat component A was 950 mPa·s;

[0115] S2: 32 parts of chain extender, 30 parts of amino-terminated polyether, 15 parts of diluent, 7 parts of foaming agent and 15 parts of modified nano molybdenum disulfide were mixed and stirred at 2500 r / min for 25 min, then heated at 100° C. for 3.5 h, and then the additive was added and stirred at 2500 r / min for 25 min to obtain topcoat component B;

[0116] Mixing of components A and B: At 60°C, mix component A and component B evenly.

[0117] S3: 15 parts of a dispersion of partially reduced graphene oxide modified with cerium dioxide nanopowder and 9 parts of a mixture of cerium dioxide micro-nano powder and yttria-stabilized zirconium oxide micro-nano powder were added to polymer A in sequence, and stirred at 2500 r / min for 3 hours to obtain a primer C component, wherein the viscosity of the primer C component was 1000 mPa·s;

[0118] S4: Mix 32 parts of chain extender, 30 parts of terminal amino polyether, 15 parts of diluent, 7 parts of foaming agent and 15 parts of modified nano cerium dioxide, stir at 2500r / min for 30min, then heat at 100°C for 4h, add auxiliary agent, and stir at 2500r / min for 30min to obtain primer D component; CD component mixing: at 70°C, mix component C and component D evenly. The topcoat and primer are anti-fouling and anti-wear polyurea coatings for oil and gas well pipes.

[0119] Example 5

[0120] The weight ratio of component A to component B of the topcoat is 1:1.9; the weight ratio of component C to component D of the primer is 1:2.1;

[0121] The raw materials for preparing component A of the topcoat include: 46 parts of isophorone diisocyanate, 30 parts of polyethylene glycol, 15 parts of α-Al2O3 nano powder and yttria-stabilized zirconium oxide nano powder modified partially reduced graphene oxide dispersion, 9 parts of a mixture of α-Al2O3 micro-nano powder and yttria-stabilized zirconium oxide (YSZ) micro-nano powder; the raw materials for preparing component B include: 32 parts of chain extender, 30 parts of amino-terminated polyether, 15 parts of diluent, 7 parts of foaming agent, 15 parts of modified nano molybdenum disulfide and 1 part of auxiliary agent;

[0122] The raw materials for preparing component C of the primer include: 46 parts of isophorone diisocyanate, 30 parts of polyethylene glycol, 15 parts of cerium dioxide nanopowder modified partially reduced graphene oxide dispersion, and 9 parts of a mixture of cerium dioxide micro (CeO2) nanopowder and yttria-stabilized zirconium oxide micro-nano powder; the raw materials for preparing component D of the primer include: 32 parts of a chain extender, 30 parts of terminal amino polyether, 15 parts of a diluent, 7 parts of a foaming agent, 15 parts of modified nano cerium dioxide and 1 part of an auxiliary agent.

[0123] Example 6

[0124] The weight ratio of component A to component B of the topcoat is 1:1.9; the weight ratio of component C to component D of the primer is 1:2.1;

[0125] The raw materials for preparing component A of the topcoat include: 60 parts of isophorone diisocyanate, 26 parts of polyethylene glycol, 5 parts of α-Al2O3 nano powder and yttria-stabilized zirconium oxide nano powder modified partially reduced graphene oxide dispersion, 9 parts of a mixture of α-Al2O3 micro-nano powder and yttria-stabilized zirconium oxide (YSZ) micro-nano powder; the raw materials for preparing component B include: 29 parts of chain extender, 37 parts of amino-terminated polyether, 14 parts of diluent, 6 parts of foaming agent, 11 parts of modified nano molybdenum disulfide and 3 parts of auxiliary agent;

[0126] The raw materials for preparing component C of the primer include: 60 parts of isophorone diisocyanate, 26 parts of polyethylene glycol, 5 parts of cerium dioxide nano powder modified partially reduced graphene oxide dispersion, and 9 parts of a mixture of cerium dioxide micro (CeO2) nano powder and yttria stabilized zirconium oxide micro-nano powder; the raw materials for preparing component D of the primer include: 29 parts of a chain extender, 37 parts of terminal amino polyether, 14 parts of a diluent, 6 parts of a foaming agent, 11 parts of modified nano cerium dioxide and 3 parts of an auxiliary agent.

[0127] Example 7

[0128] The weight ratio of component A to component B of the topcoat is 1:2.0; the weight ratio of component C to component D of the primer is 1:2.1;

[0129] The raw materials for preparing component A of the topcoat include: 61 parts of isophorone diisocyanate, 15 parts of polyethylene glycol, 15 parts of α-Al2O3 nano powder and yttria-stabilized zirconium oxide nano powder modified partially reduced graphene oxide dispersion, 9 parts of a mixture of α-Al2O3 micro-nano powder and yttria-stabilized zirconium oxide (YSZ) micro-nano powder; the raw materials for preparing component B include: 29 parts of chain extender, 39 parts of terminal amino polyether, 11 parts of diluent, 6 parts of foaming agent, 14 parts of modified nano molybdenum disulfide and 1 part of auxiliary agent;

[0130] The raw materials for preparing component C of the primer include: 61 parts of isophorone diisocyanate, 15 parts of polyethylene glycol, 15 parts of cerium dioxide nanopowder modified partially reduced graphene oxide dispersion, and 9 parts of a mixture of cerium dioxide micro (CeO2) nanopowder and yttria-stabilized zirconium oxide micro-nano powder; the raw materials for preparing component D of the primer include: 29 parts of a chain extender, 39 parts of terminal amino polyether, 11 parts of a diluent, 6 parts of a foaming agent, 14 parts of modified nano cerium dioxide and 1 part of an auxiliary agent.

[0131] Example 8

[0132] The weight ratio of component A to component B of the topcoat is 1:2.0; the weight ratio of component C to component D of the primer is 1:2.0;

[0133] The raw materials for preparing component A of the topcoat include: 61 parts of isophorone diisocyanate, 29 parts of polyethylene glycol, 5 parts of α-Al2O3 nano powder and yttria stabilized zirconium oxide nano powder modified partially reduced graphene oxide dispersion, 5 parts of a mixture of α-Al2O3 micro-nano powder and yttria stabilized zirconium oxide (YSZ) micro-nano powder; the raw materials for preparing component B include: 29 parts of chain extender, 39 parts of amino-terminated polyether, 11 parts of diluent, 6 parts of foaming agent, 14 parts of modified nano molybdenum disulfide and 1 part of auxiliary agent;

[0134] The raw materials for preparing component C of the primer include: 61 parts of isophorone diisocyanate, 29 parts of polyethylene glycol, 5 parts of cerium dioxide nanopowder modified partially reduced graphene oxide dispersion, and 5 parts of a mixture of cerium dioxide micro (CeO2) nanopowder and yttria-stabilized zirconium oxide micro-nano powder; the raw materials for preparing component D of the primer include: 29 parts of a chain extender, 39 parts of terminal amino polyether, 11 parts of a diluent, 6 parts of a foaming agent, 14 parts of modified nano cerium dioxide and 1 part of an auxiliary agent.

[0135] The preparation process and temperature, time and stirring conditions of Examples 5-8 are the same as those of Example 1.

[0136] Performance Test:

[0137] The coating samples of Example 1, Example 2 and Example 3 were placed for 7 days before performance testing. The test results are as follows:

[0138]

[0139] From the above table, it can be seen that the anti-scaling and anti-wear coating prepared by the present invention has a low surface energy, a contact angle of more than 105 degrees, and exhibits excellent hydrophobicity, and can form a super-slip polyurea coating with high adhesion and anti-scaling performance on the surface of oil pipes; the wear resistance of the coating prepared by the present invention is improved by more than 70%; the coating developed by the present invention has good corrosion resistance in harsh oil and gas drilling environments such as ultra-high temperature and high pressure acidic oil and gas media, alkaline media, and simulated formation water with high mineralization and high bacteria content. Therefore, the coating developed by the present invention has greatly improved corrosion resistance, anti-scaling and anti-wear performance, and has broad application prospects in deep and ultra-deep oil and gas drilling.

[0140] The above contents are only for explaining the technical idea of ​​the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.

Claims

1. An anti-fouling and anti-wear polyurea coating, It is characterized in that It comprises a primer and a topcoat; the topcoat comprises a component A and a component B, and the weight ratio of the component A to the component B is 1:(1.9-2.1); The raw materials for preparing component A of the topcoat include, by parts: 46-61 parts of isophorone diisocyanate, 15-30 parts of polyethylene glycol, α-Al 2 O 3 Nanopowder and yttria-stabilized zirconium oxide nanopowder modified partially reduced graphene oxide dispersion 5-15 parts, α-Al 2 O 3 5 to 9 parts of a mixture of micro-nano powder and yttria-stabilized zirconium oxide micro-nano powder, with a total of 100 parts; In terms of parts, the raw materials for preparing component B of the topcoat include: 29 to 32 parts of chain extender, 30 to 39 parts of amino-terminated polyether, 11 to 15 parts of diluent, 6 to 8 parts of foaming agent, 11 to 15 parts of modified nano molybdenum disulfide and 1 to 3 parts of auxiliary agent, with a total of 100 parts; The primer comprises a C component and a D component, wherein the weight ratio of the C component to the D component is 1:(1.9-2.1); in terms of parts, the raw materials for preparing the C component of the primer comprise: 46-61 parts of isophorone diisocyanate, 15-30 parts of polyethylene glycol, 5-15 parts of a dispersion of partially reduced graphene oxide modified by cerium dioxide nanopowder, and 5-9 parts of a mixture of cerium dioxide micro-nano powder and yttria-stabilized zirconium oxide micro-nano powder, with a total of 100 parts; In terms of parts, the raw materials for preparing component D of the primer include: 29-32 parts of chain extender, 30-39 parts of terminal amino polyether, 11-15 parts of diluent, 6-8 parts of foaming agent, 11-15 parts of modified nano cerium dioxide and 1-3 parts of auxiliary agent, with a total of 100 parts.

2. The anti-fouling and anti-wear polyurea coating according to claim 1, It is characterized in that The α~Al 2 O 3 α~Al in the mixture of micro-nano powder and yttria-stabilized zirconia micro-nano powder 2 O 3 The mass ratio of the micro-nano powder to the yttria-stabilized zirconium oxide micro-nano powder is 1:3; the α~Al 2 O 3 The mass ratio of nanometer powder to micrometer powder in the micro-nanometer powder is 1:1; the mass ratio of nanometer powder to micrometer powder in the yttria-stabilized zirconia micro-nanometer powder is 2:

1.

3. The anti-fouling and anti-wear polyurea coating according to claim 1, It is characterized in that The mass ratio of cerium dioxide micro-nano powder to yttria-stabilized zirconia micro-nano powder in the mixture of cerium dioxide micro-nano powder and yttria-stabilized zirconia micro-nano powder is 2:1; the mass ratio of nano powder to micron powder in the cerium dioxide micro-nano powder is 2:1; the mass ratio of nano powder to micron powder in the yttria-stabilized zirconia micro-nano powder is 2:

1.

4. The anti-fouling and anti-wear polyurea coating according to claim 1, It is characterized in that The chain extender is diethyltoluenediamine; the diluent is a mixture of propylene carbonate, n-butyl acetate and n-butanol, and the mass ratio of the propylene carbonate, n-butyl acetate and n-butanol is 3:3:1; the foaming agent is azobisisobutyronitrile; and the auxiliary agents include a leveling agent, a defoaming agent and a dispersant.

5. A method for preparing the anti-fouling and anti-wear polyurea coating according to any one of claims 1 to 4, It is characterized in that The following steps are involved: S1: Mix isophorone diisocyanate and polyethylene glycol and heat them to obtain polymer A to prepare α~Al 2 O 3 Nanopowder and yttria-stabilized zirconium oxide nanopowder modified partially reduced graphene oxide dispersion; α~Al 2 O 3 Nanopowder and yttria-stabilized zirconium oxide nanopowder modified partially reduced graphene oxide dispersion, α~Al 2 O 3 A mixture of micro-nano powder and yttria-stabilized zirconium oxide micro-nano powder is stirred to obtain component A of the topcoat; S2: preparing modified nano molybdenum disulfide, mixing a chain extender, an amino-terminated polyether, a diluent, a foaming agent, and the modified nano molybdenum disulfide, stirring and heating, and then adding an auxiliary agent and mixing evenly to obtain component B of the topcoat; S3: preparing a dispersion of partially reduced graphene oxide modified by cerium dioxide nanopowder; sequentially adding a mixture of the dispersion of partially reduced graphene oxide modified by cerium dioxide nanopowder, cerium dioxide micro-nano powder and yttria-stabilized zirconium oxide micro-nano powder to polymer A, and stirring to obtain component C of the primer; S4: preparing modified nano-cerium dioxide, mixing a chain extender, an amino-terminated polyether, a diluent, a foaming agent, and the modified nano-cerium dioxide, stirring and heating the mixture, and then adding an auxiliary agent and mixing the mixture evenly to obtain a D component of the primer; S5: evenly mix the prepared component A of the topcoat and the component B of the topcoat to prepare a topcoat; evenly mix the prepared component C of the primer and the component D of the primer to prepare a primer, wherein the topcoat and the primer are anti-fouling and anti-wear polyurea coatings for oil and gas well pipes.

6. The preparation method according to claim 5, It is characterized in that In S1, the preparation of α~Al 2 O 3 The process of modifying the partially reduced graphene oxide dispersion with nanopowder and yttria-stabilized zirconium oxide nanopowder is as follows: The trimethylsiloxane is mixed with the partially reduced graphene oxide X to perform a first modification reaction to obtain a mixed solution a; α-Al is added to the mixed solution a. 2 O 3 The nano powder and the yttria-stabilized zirconium oxide nano powder are reacted to obtain a mixed solution b; the mixed solution b is dried to obtain α~Al 2 O 3 Nanopowder and yttria-stabilized zirconium oxide nanopowder modified partially reduced graphene oxide, then α~Al 2 O 3 The nanopowder and yttria-stabilized zirconium oxide nanopowder modified partially reduced graphene oxide, n-butanol, polydimethylsiloxane and silane coupling agent were added in sequence, and a second modification reaction was carried out and ultrasonic treatment was performed to obtain α-Al 2 O 3 Nanopowder and yttria-stabilized zirconium oxide nanopowder modified partially reduced graphene oxide dispersion; The α~Al 2 O 3 The mass ratio of nanopowder to yttria-stabilized zirconia nanopowder is 1:2; The oxygen content of the partially reduced graphene oxide X is 10%.

7. The preparation method according to claim 5, It is characterized in that In S2, the process of preparing modified nano molybdenum disulfide is as follows: Mixing nano-molybdenum disulfide, n-butanol and anhydrous ethanol, adjusting the pH value to neutral to obtain a nano-molybdenum disulfide suspension; mixing vinyl triethoxysilane and the nano-molybdenum disulfide suspension, and then adding partially reduced graphene oxide Y to react to obtain a modified nano-molybdenum disulfide dispersion, filtering, and vacuum drying to obtain the modified nano-molybdenum disulfide; The volume ratio of the vinyl triethoxysilane to the nano-molybdenum disulfide suspension is 1:10; The oxygen content of the partially reduced graphene oxide Y is 15%.

8. The preparation method according to claim 5, It is characterized in that In S3, the process of preparing the cerium dioxide nanopowder modified partially reduced graphene oxide dispersion is as follows: The trimethylsiloxane and the partially reduced graphene oxide X are mixed to carry out a first modification reaction to obtain a mixed solution a; the cerium dioxide nanopowder is added to the mixed solution a to react to obtain a mixed solution c; the mixed solution b is dried to obtain the cerium dioxide nanopowder modified partially reduced graphene oxide, and then n-butanol, polydimethylsiloxane and a silane coupling agent are sequentially added to the cerium dioxide nanopowder modified partially reduced graphene oxide, a second modification reaction is carried out and ultrasonic treatment is performed to obtain a cerium dioxide nanopowder modified partially reduced graphene oxide dispersion; The oxygen content of the partially reduced graphene oxide X is 10%.

9. The preparation method according to claim 5, It is characterized in that In S4, the process of preparing modified nano-cerium dioxide is as follows: Mixing nano-cerium disulfide, n-butanol and anhydrous ethanol, adjusting the pH value to neutral to obtain a nano-cerium disulfide suspension, mixing vinyl triethoxysilane and the nano-cerium disulfide suspension, adding partially reduced graphene oxide Y, reacting to obtain a modified nano-cerium disulfide dispersion, and then filtering and vacuum drying to obtain modified nano-cerium dioxide; The volume ratio of the vinyl triethoxysilane to the nano-cerium disulfide suspension is 1:10; The oxygen content of the partially reduced graphene oxide Y is 15%.

10. A method for using the anti-fouling and anti-wear polyurea coating according to claim 1, It is characterized in that The polyurea coating is used for anti-scaling and anti-wear of oil and gas well pipes, and the method of use is as follows: The primer in the polyurea coating is coated on the pretreated substrate and then cured to obtain a substrate coated with the primer; the topcoat is coated on the substrate coated with the primer and then cured to form an anti-fouling and anti-wear polyurea coating.

Citation Information

Patent Citations

  • Anti-icing super-smooth polyurea coating for wind power blade as well as preparation method and application of anti-icing super-smooth polyurea coating

    CN113773732A