Water-based degradable glue and preparation method thereof

By preparing a combination of water-based degradable resin core-shell solution and water-based rosin resin emulsion, combined with specific ingredients and processing methods, the problem of low performance of existing water-based degradable glue is solved, and the improvement of high-efficiency adhesive and biodegradable performance is achieved, which is suitable for In the fields of plastic films and tapes, it meets the needs of safety, environmental protection, and sustainable development.

CN118725819APending Publication Date: 2024-10-01SHANGHAI HUZHENG IND CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202310318514.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The performance of existing water-based degradable glues is low, which limits its application scope, and the preparation methods and performance improvements have not been fully expanded to meet the needs of safer, environmentally friendly, and sustainable development.

Method used

By preparing a combination of water-based degradable resin core-shell solution and water-based rosin resin emulsion, combined with ingredients such as hydroxypropyl methylcellulose, silane coupling agent and alkyl glycoside, and using specific stirring and dialysis methods, a highly efficient adhesive is formed. Water-based degradable glue with high performance and effective degradability.

Benefits of technology

It achieves stable adhesive properties and significant biodegradability of water-based degradable glue. It is suitable for plastic films, tapes and other fields. It is safe, environmentally friendly and degradable, which significantly improves its value in practical applications.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses water-based degradable glue, which is prepared from the following components in parts by mass: 30 to 50 parts of water-based degradable resin core-shell solution, 5 to 10 parts of water-based rosin resin emulsion, 2 to 4 parts of hydroxypropyl methyl cellulose, 0.5 to 1.5 parts of silane coupling agent KH-450, 0.5 to 1 part of alkyl glycoside 1214, 3 to 5 parts of isopropanol and 90 to 120 parts of deionized water. The water-based degradable glue disclosed by the invention has excellent adhesion performance and outstanding degradability, and has a very good application prospect in the related fields of films, adhesive tapes, labels and the like. In addition, the invention also discloses a preparation method of the water-based degradable glue.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to water-based degradable glue and a preparation method thereof. Background Art

[0002] Social development requires people to pay more and more attention to the protection of environmental resources, which is not only conducive to the health and comfort of people's lives, but also conducive to the sustainable development of the economy. The widespread use of plastic products has gradually caused damage to environmental resources. Degradable materials, as an important concept of sustainable development, have received widespread attention. Degradable materials can effectively avoid the long-term damage to the marine and soil environment caused by waste materials, but can be degraded and re-enter the carbon cycle of nature.

[0003] As one of the branches, there have been many related studies on degradable glue, such as the biodegradable copolyester pressure-sensitive adhesive disclosed in Chinese patent CN111117544A, the biodegradable polyurethane adhesive disclosed in Chinese patent CN112226191A, and the degradable polyurethane pressure-sensitive adhesive disclosed in US patent US20170362478A1.

[0004] However, in terms of water-based degradable glue, the performance is still at a low level and its application is also greatly limited. Chinese patent CN1995086A discloses a water-based haze degradable polyurethane elastomer that can be used for medical tissue engineering materials. At present, the expansion of the preparation method of water-based degradable glue, the improvement of performance and the expansion of application are important directions in this field, which conforms to the concept of safer, environmentally friendly and sustainable development, can meet the increasingly urgent development needs, and ultimately achieve the coordinated and harmonious development of human society and nature. Summary of the invention

[0005] In view of the above-mentioned deficiencies of the existing methods and technologies, according to an embodiment of the present invention, it is hoped to provide a water-based degradable glue, which can achieve outstanding adhesive properties and effective degradation properties through efficient preparation and appropriate formulation, and can be widely used.

[0006] According to the embodiment, the water-based degradable glue provided by the present invention has the following composition and weight parts:

[0007] Aqueous biodegradable resin core-shell solution: 30-50 parts;

[0008] Water-based rosin resin emulsion: 5-10 parts;

[0009] Hydroxypropyl methylcellulose: 2-4 parts;

[0010] Silane coupling agent KH-450: 0.5-1.5 parts;

[0011] Alkyl glycoside 1214: 0.5-1 part;

[0012] Isopropyl alcohol: 3-5 parts;

[0013] Deionized water: 90-120 parts.

[0014] According to one embodiment, the method for preparing an aqueous degradable resin core-shell solution comprises the following steps:

[0015] (1) According to the mass ratio, 1 mass part of polylactic acid polyol is dissolved in 50 mass parts of N,N′-dimethylacetamide, and 0.05-0.1 mass parts of 1-ethyl-(3-dimethylaminopropyl)carbodiimide is added, which is recorded as solution A. 0.7-0.9 mass parts of modified cellulose is dissolved in 50 mass parts of N,N′-dimethylacetamide, and 0.01-0.05 mass parts of 4-dimethylaminopyridine is added, which is recorded as solution B.

[0016] (2) Under nitrogen atmosphere and at 55°C, solution B was gradually added to solution A at a rate of 3-5 ml / min, and the reaction was stirred for 5-7 h.

[0017] (3) After cooling to room temperature, ethanol precipitation and centrifugation were performed, and the product was repeatedly washed with ethanol and water for three times, and freeze-dried to obtain a pre-product.

[0018] (4) According to the mass ratio, 1 mass part of the pre-product is dissolved in 50 mass parts of N,N′-dimethylformamide, which is recorded as solution C. 20 mass parts of deionized water are dripped into solution C at a rate of 5-10 ml / min and stirred for 5-8 h.

[0019] (5) After continuous dialysis and concentration, an aqueous biodegradable resin core-shell solution is obtained.

[0020] According to one embodiment, in step (1), the molecular weight of polylactic acid polyol is 500-1000, and the hydroxyl value is 100-230 mg KOH / g; the modified cellulose is hydroxyethyl cellulose modified with maleic anhydride. In step (5), the resin content of the solution is 45-55 wt%.

[0021] According to an embodiment, the preparation method of the water-based degradable glue provided by the present invention comprises the following steps: weighing by mass, stirring and mixing alkyl polyglycoside 1214, hydroxypropyl methylcellulose, silane coupling agent KH450, and water-based rosin resin emulsion in a mixed solvent of isopropanol and water for 1-3 hours to obtain a dispersion. Slowly adding the water-based degradable resin core-shell solution to the dispersion, stirring for 5-8 hours, and obtaining a uniform water-based degradable glue.

[0022] Compared with the prior art, the water-based degradable glue of the present invention has reached a new level in terms of safety, environmental protection, and degradability through the synthesis of degradable resins, the compounding of degradable components, and the establishment of a water-based system, and has stable performance in terms of adhesive function. The water-based degradable glue can play an important role in the fields of plastic films, adhesive tapes, etc. The subsequent embodiments and test examples will prove that the water-based degradable glue of the present invention is safe and environmentally friendly, has outstanding degradability, and has strong adhesiveness. DETAILED DESCRIPTION

[0023] The present invention will be further described below in conjunction with specific embodiments. These embodiments should be understood to be only used to illustrate the present invention and not to limit the scope of protection of the present invention. After reading the content of the present invention, those skilled in the art may make various changes or modifications to the present invention, and these equivalent changes and modifications also fall within the scope defined by the claims of the present invention.

[0024] In the following examples of the present invention, maleic anhydride-modified hydroxyethyl cellulose is prepared by the following method:

[0025] Dissolve 0.8g of maleic anhydride in 50ml of N,N'-dimethylformamide and stir for 3h to obtain 1 solution. Dissolve 9.2g of hydroxyethyl cellulose in 450ml of N,N'-dimethylformamide and stir for 5h to obtain another solution. Mix the two solutions and add 0.6g of anhydrous sodium acetate at the same time. Stir the reaction for 3h at 85℃ under nitrogen atmosphere, cool to room temperature, wash with acetone, centrifuge, and vacuum dry to obtain maleic anhydride-modified hydroxyethyl cellulose.

[0026] The raw materials used in the following examples of the present invention are all commercially available products unless otherwise specified.

[0027] Example 1

[0028] The aqueous degradable resin core-shell solution was prepared by the following method:

[0029] (1) 10 g of polylactic acid polyol (molecular weight 500 g / mol, hydroxyl value 100 mg KOH / g) was dissolved in 500 g of N,N′-dimethylacetamide, and 0.5 g of 1-ethyl-(3-dimethylaminopropyl)carbodiimide was added, which was recorded as solution A. 8 g of maleic anhydride-modified hydroxyethyl cellulose was dissolved in 500 g of N,N′-dimethylacetamide, and 0.1 g of 4-dimethylaminopyridine was added, which was recorded as solution B.

[0030] (2) Under nitrogen atmosphere and at 55°C, solution B was gradually added to solution A at a rate of 3 ml / min and the reaction was stirred for 5 h.

[0031] (3) After cooling to room temperature, ethanol precipitation and centrifugation were performed, and the product was repeatedly washed with ethanol and water for three times, and freeze-dried to obtain a pre-product.

[0032] (4) 10 g of the pre-product was dissolved in 500 g of N,N′-dimethylformamide, which was recorded as solution C. 200 g of deionized water was dripped into solution C at a rate of 8 ml / min and stirred for 6 h.

[0033] (5) After continuous dialysis and concentration, an aqueous degradable resin core-shell solution with a resin content of 50 wt% is obtained.

[0034] The water-based degradable glue was prepared by the following method: 0.4 g of alkyl polyglycoside 1214, 2 g of hydroxypropyl methylcellulose, 0.3 g of silane coupling agent KH450, and 5 g of water-based rosin resin emulsion were stirred for 2 h in a mixed solvent of 3 g of isopropanol and 40 g of water to obtain a dispersion. 20 g of the water-based degradable resin core-shell solution was slowly added to the dispersion and stirred for 5 h to obtain a uniform water-based degradable glue.

[0035] Example 2

[0036] The aqueous degradable resin core-shell solution was prepared by the following method:

[0037] (1) 10 g of polylactic acid polyol (molecular weight: 1000 g / mol, hydroxyl value: 230 mg KOH / g) was dissolved in 500 g of N,N′-dimethylacetamide, and 0.6 g of 1-ethyl-(3-dimethylaminopropyl)carbodiimide was added, which was recorded as solution A. 9 g of maleic anhydride-modified hydroxyethyl cellulose was dissolved in 500 g of N,N′-dimethylacetamide, and 0.1 g of 4-dimethylaminopyridine was added, which was recorded as solution B.

[0038] (2) Under nitrogen atmosphere and at 55°C, solution B was gradually added to solution A at a rate of 5 ml / min and the reaction was stirred for 6 h.

[0039] (3) After cooling to room temperature, ethanol precipitation and centrifugation were performed, and the product was repeatedly washed with ethanol and water for three times, and freeze-dried to obtain a pre-product.

[0040] (4) 10 g of the pre-product was dissolved in 500 g of N,N′-dimethylformamide, which was recorded as solution C. 200 g of deionized water was dripped into solution C at a rate of 8 ml / min and stirred for 8 h.

[0041] (5) After continuous dialysis and concentration, an aqueous degradable resin core-shell solution with a resin content of 55 wt % was obtained.

[0042] The water-based degradable glue was prepared by the following method: 0.6 g of alkyl polyglycoside 1214, 2.4 g of hydroxypropyl methylcellulose, 0.4 g of silane coupling agent KH450, and 6 g of water-based rosin resin emulsion were stirred for 3 h in a mixed solvent of 3 g of isopropanol and 50 g of water to obtain a dispersion. 10 g of the water-based degradable resin core-shell solution was slowly added to the dispersion and stirred for 8 h to obtain a uniform water-based degradable glue.

[0043] Example 3

[0044] The aqueous degradable resin core-shell solution was prepared by the following method:

[0045] (1) 10 g of polylactic acid polyol (molecular weight 500 g / mol, hydroxyl value 100 mg KOH / g) was dissolved in 500 g of N,N′-dimethylacetamide, and 0.5 g of 1-ethyl-(3-dimethylaminopropyl)carbodiimide was added, which was recorded as solution A. 9 g of maleic anhydride-modified hydroxyethyl cellulose was dissolved in 500 g of N,N′-dimethylacetamide, and 0.1 g of 4-dimethylaminopyridine was added, which was recorded as solution B.

[0046] (2) Under nitrogen atmosphere and at 55°C, solution B was gradually added to solution A at a rate of 3 ml / min and the reaction was stirred for 6 h.

[0047] (3) After cooling to room temperature, ethanol precipitation and centrifugation were performed, and the product was repeatedly washed with ethanol and water for three times, and freeze-dried to obtain a pre-product.

[0048] (4) 10 g of the pre-product was dissolved in 500 g of N,N′-dimethylformamide, which was recorded as solution C. 200 g of deionized water was dripped into solution C at a rate of 8 ml / min and stirred for 8 h.

[0049] (5) After continuous dialysis and concentration, an aqueous degradable resin core-shell solution with a resin content of 55 wt % was obtained.

[0050] The water-based degradable glue was prepared by the following method: 0.5 g of alkyl polyglycoside 1214, 2.4 g of hydroxypropyl methylcellulose, 0.5 g of silane coupling agent KH450, and 5 g of water-based rosin resin emulsion were stirred for 3 h in a mixed solvent of 3 g of isopropanol and 45 g of water to obtain a dispersion. 10 g of the water-based degradable resin core-shell solution was slowly added to the dispersion and stirred for 8 h to obtain a uniform water-based degradable glue.

[0051] Test example

[0052] The degradable glue prepared in each embodiment was uniformly applied to each PET sheet and heated at 80°C for 10 min. Its degradation performance was tested according to the national standard GB / T 19277.1-2011. Its initial adhesion was tested according to the national standard GB / T4852-2002, its sustained adhesion was tested according to the national standard GB / T4851-2014, and its 180° peel strength was tested according to the national standard GB / T2792-2014. The results of the bonding performance test are shown in Table 1, and the biodegradability test is shown in Table 2.

[0053] As can be seen from Tables 1-2, the degradable glues prepared in various embodiments have outstanding adhesion and outstanding biodegradability. Among them, the degradable glue prepared in Example 2 has the most outstanding adhesive performance, with an initial adhesion of a No. 8 steel ball, a sustained adhesion of 42 hours, and a 180° peel strength of 3.6 N / cm. It also has outstanding degradable performance, with a 180-day degradation rate of 94.2%, and has good practical application value in related fields such as films, tapes, and labels.

[0054] Table 1. Adhesive properties test of various embodiments

[0055] Example 1 Example 2 Example 3 Initial adhesion (steel ball number) 8 8 8 Holding force(h) 38 42 39 180° peel strength (N / cm) 3.4 3.6 3.4

[0056] Table 2. Biodegradability test of each example

[0057] Example 1 Example 2 Example 3 30-day degradation rate (%) 24.6% 25.5% 25.1% 90-day degradation rate (%) 64.9% 65.7% 65.2% 180-day degradation rate (%) 93.1% 94.2% 93.5%

Claims

1. A water-based degradable glue, characterized in that: It consists of the following components and mass parts: Aqueous biodegradable resin core-shell solution: 30-50 parts; Water-based rosin resin emulsion: 5-10 parts; Hydroxypropyl methylcellulose: 2-4 parts; Silane coupling agent KH-450: 0.5-1.5 parts; Alkyl glycoside 1214: 0.5-1 part; Isopropyl alcohol: 3-5 parts; Deionized water: 90-120 parts.

2. The water-based degradable glue according to claim 1, characterized in that: The aqueous degradable resin core-shell solution was prepared by the following method: (1) According to the mass ratio, 1 mass part of polylactic acid polyol is dissolved in 50 mass parts of N,N′-dimethylacetamide, and 0.05-0.1 mass part of 1-ethyl-(3-dimethylaminopropyl)carbodiimide is added, which is recorded as solution A; 0.7-0.9 mass parts of modified cellulose is dissolved in 50 mass parts of N,N′-dimethylacetamide, and 0.01-0.05 mass parts of 4-dimethylaminopyridine is added, which is recorded as solution B; (2) Under nitrogen atmosphere and at 55°C, solution B was gradually added to solution A at a rate of 3-5 ml / min, and the reaction was stirred for 5-7 h; (3) After cooling to room temperature, ethanol precipitation and centrifugation were performed, and the product was repeatedly washed with ethanol and water for 3 times, and freeze-dried to obtain a pre-product; (4) According to the mass ratio, 1 mass part of the pre-product is dissolved in 50 mass parts of N,N′-dimethylformamide, which is recorded as solution C; 20 mass parts of deionized water are dripped into solution C at a rate of 5-10 ml / min and stirred for 5-8 hours; (5) After continuous dialysis and concentration, an aqueous biodegradable resin core-shell solution is obtained.

3. The water-based degradable glue according to claim 2, characterized in that: In step (1), the molecular weight of the polylactic acid polyol is 500-1000, and the hydroxyl value is 100-230 mg KOH / g.

4. The water-based degradable glue according to claim 2, characterized in that: In step (1), the modified cellulose is hydroxyethyl cellulose modified with maleic anhydride.

5. The water-based degradable glue according to claim 2, characterized in that: In step (5), the resin content of the solution is 45-55wt%.

6. The method for preparing the water-based degradable glue according to any one of claims 1 to 5, characterized in that: Weigh according to mass, stir and mix alkyl polyglycoside 1214, hydroxypropyl methylcellulose, silane coupling agent KH450, and water-based rosin resin emulsion in a mixed solvent of isopropanol and water for 1-3 hours to obtain a dispersion; slowly add the water-based degradable resin core-shell solution into the dispersion and stir for 5-8 hours to obtain a water-based degradable glue.

Citation Information

Patent Citations

  • Biodegradable pressure-sensitive adhesive and preparation method thereof

    CN111117544A

  • Biodegradable adhesive and preparation method thereof

    CN112226191A

  • Method for preparing aqueous nontoxic degradable polyurethane elastomer

    CN1995086A

  • Biodegradable pressure-sensitive adhesive

    US20170362478A1