Barite powder for oil field

Through the modification treatment of sodium stearate, silane coupling agent and hydrophobic monomer, barite powder suitable for oil-based drilling fluids is prepared, which solves the lack of applicability of barite powder in oil-based drilling fluids in the existing technology. problem, significantly improving its hydrophobicity and application effect.

CN118725833APending Publication Date: 2024-10-01ZHENGZHOU CITY XINZHENG MEIJIU IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410937451.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The existing barite powder modification method is mainly suitable for water-based drilling fluids and is difficult to adapt to the needs of oil-based drilling fluids, resulting in an increased risk of blowout accidents.

Method used

By combining sodium stearate, silane coupling agent, hydrophobic monomer and initiator with barite powder, and adjusting the pH value and stirring conditions, barite powder suitable for oil-based drilling fluids is prepared and its hydrophobicity is improved.

Benefits of technology

The prepared barite powder for oil fields has good surface hydrophobicity and is suitable for oil-based drilling fluids, which significantly improves its application effect in oil-based drilling fluids and reduces the risk of blowout accidents.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides barite powder for an oil field, which is prepared by the following steps: dissolving sodium stearate in an ethanol solution, adding a barite powder raw material, and uniformly mixing to obtain a barite powder suspension; dispersing a silane coupling agent in an ethanol solution, and adjusting the pH value to 3-4 or 9-10 to obtain a silane coupling agent solution; slowly adding the silane coupling agent solution into the barite powder suspension, and uniformly stirring; adding a hydrophobic monomer and an initiator, reacting at 30-120 DEG C for 0.5-4 hours, and sequentially filtering, washing, drying and scattering to obtain the barite powder for the oil field. The barite powder for the oil field has good surface hydrophobicity and is suitable for oil-based drilling fluid.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of oil field exploitation, in particular to barite powder for oil fields. Background Art

[0002] Barite is made of barium sulfate (BaSO 4) As a non-metallic mineral product with barite as the main component, pure barite is white and shiny. Due to the influence of impurities and mixed materials, it is often gray, light red, light yellow, etc. When drilling some oil wells and gas wells, the drilling mud and clay used generally have a specific gravity of about 2.5, and the specific gravity of water is 1. Therefore, the mud specific gravity is low. If the mud weight is not balanced with the underground oil and gas pressure, it will cause a blowout accident. In the case of high underground pressure, it is necessary to add barite powder to the mud to increase the mud specific gravity.

[0003] In order to improve the dispersibility of barite powder, it is usually necessary to modify and activate the barite powder, for example: Chinese patent CN112322259A discloses surface-modified barite powder for drilling fluid and its preparation method and water-based drilling fluid, Chinese patent CN102127318A discloses a modification method of activated barite powder, etc. However, the barite powder obtained by these methods is for water-based drilling fluid and is not suitable for oil-based drilling fluid.

[0004] In order to solve the above problems, people have been seeking an ideal technical solution. Summary of the invention

[0005] The purpose of the present invention is to provide a barite powder for oil field in view of the deficiencies of the prior art.

[0006] In order to achieve the above object, the technical solution adopted by the present invention is: A barite powder for oil field is prepared by the following steps: Dissolve sodium stearate in an ethanol solution, add barite powder raw material, mix well, and obtain a barite powder suspension; Dispersing a silane coupling agent in an ethanol solution, adjusting the pH to 3-4 or 9-10, to obtain a silane coupling agent solution; Slowly add the silane coupling agent solution into the barite powder suspension and stir evenly; A hydrophobic monomer and an initiator are added, reacted at 30-120° C. for 0.5-4 h, and filtering, washing, drying, and breaking up are performed in sequence to obtain barite powder for oil fields.

[0007] The particle size of the barite powder raw material is less than 1 micron; the dosage of sodium stearate is 0.1%-1.0% of the barite powder raw material; the dosage of silane coupling agent is 0.3%-1.0% of the barite powder raw material; the dosage of hydrophobic monomer is 1%-5% of the barite powder raw material; the dosage of initiator is 0.1%-1% of the hydrophobic monomer.

[0008] Slowly add the silane coupling agent solution into the barite powder suspension and stir at a speed of 1000-2000 r / min for 10-30 min.

[0009] The hydrophobic monomer is one or a combination of at least two of styrene, isobutylene, butadiene, butyl methacrylate, methyl methacrylate, and hexafluorobutyl acrylate.

[0010] The initiator is one of azobisisobutyronitrile, potassium persulfate, sodium persulfate, dibenzoyl peroxide, and N,N-dimethylaniline, or a combination of at least two of them.

[0011] The silane coupling agent is vinyl triethoxysilane, vinyl tri(β-methoxyethoxy)silane or γ-methacryloxypropyl trimethoxysilane.

[0012] The present invention has outstanding substantial characteristics and significant progress compared with the prior art. Specifically, the present invention provides a barite powder for oil field with good surface hydrophobicity, which is suitable for oil-based drilling fluid. Specifically, the present invention modifies the barite powder raw material by sodium stearate, silane coupling agent and hydrophobic monomer to improve the hydrophilicity of the barite powder and facilitate the application of oil-based drilling fluid. DETAILED DESCRIPTION

[0013] The technical solution of the present invention is further described in detail below through specific implementation methods. Example

[0014] This embodiment provides a barite powder for oil field, which is prepared by the following steps: Dissolve sodium stearate in an ethanol solution, add barite powder raw material, mix well, and obtain a barite powder suspension; Dispersing a silane coupling agent in an ethanol solution, adjusting the pH to 3-4 or 9-10, to obtain a silane coupling agent solution; Slowly add the silane coupling agent solution into the barite powder suspension and stir evenly; A hydrophobic monomer and an initiator are added, reacted at 30-120° C. for 0.5-4 h, and filtering, washing, drying, and breaking up are performed in sequence to obtain barite powder for oil fields.

[0015] The particle size of the barite powder raw material is less than 1 micron; the dosage of sodium stearate is 0.1%-1.0% of the barite powder raw material; the dosage of silane coupling agent is 0.3%-1.0% of the barite powder raw material; the dosage of hydrophobic monomer is 1%-5% of the barite powder raw material; the dosage of initiator is 0.1%-1% of the hydrophobic monomer.

[0016] Slowly add the silane coupling agent solution into the barite powder suspension and stir at a speed of 1000-2000 r / min for 10-30 min.

[0017] The hydrophobic monomer is one or a combination of at least two of styrene, isobutylene, butadiene, butyl methacrylate, methyl methacrylate, and hexafluorobutyl acrylate.

[0018] The initiator is one of azobisisobutyronitrile, potassium persulfate, sodium persulfate, dibenzoyl peroxide, and N,N-dimethylaniline, or a combination of at least two of them.

[0019] The silane coupling agent is vinyl triethoxysilane, vinyl tri(β-methoxyethoxy)silane or γ-methacryloxypropyl trimethoxysilane.

[0020] The hydrophobicity of barite powder for oil field is evaluated by testing the floating rate of powder in water. The floating rate H = sample floating mass H1 / sample floating mass H2.

[0021] Example 1 This embodiment provides a barite powder for oil field, which is prepared by the following steps: Dissolve sodium stearate in an ethanol solution, add barite powder raw material, mix well, and obtain a barite powder suspension; Dispersing a silane coupling agent in an ethanol solution and adjusting the pH to 3-4 to obtain a silane coupling agent solution; Slowly add the silane coupling agent solution to the barite powder suspension, and stir at a speed of 1500 r / min for 200 minutes; add a hydrophobic monomer and an initiator, react at 60-120°C for 4 hours, and perform filtering, washing, drying, and dispersing steps in sequence to obtain barite powder for oil fields; the hydrophobic monomer is styrene; the initiator is azobisisobutyronitrile; the silane coupling agent is vinyltriethoxysilane; the particle size of the barite powder raw material is less than 1 micron; the amount of sodium stearate is 0.5% of the barite powder raw material; the amount of silane coupling agent is 0.3% of the barite powder raw material; the amount of hydrophobic monomer is 1% of the barite powder raw material; and the amount of initiator is 0.5% of the hydrophobic monomer.

[0022] According to the test, the floating rate H of barite powder used in oil fields is 99.7%.

[0023] Example 2 This embodiment provides a barite powder for oil field, which is prepared by the following steps: Dissolve sodium stearate in an ethanol solution, add barite powder raw material, mix well, and obtain a barite powder suspension; Dispersing a silane coupling agent in an ethanol solution and adjusting the pH to 9-10 to obtain a silane coupling agent solution; Slowly add the silane coupling agent solution to the barite powder suspension, and stir at a speed of 2000 r / min for 10 minutes; add a hydrophobic monomer and an initiator, react at 60-120°C for 4 hours, and perform filtering, washing, drying, and dispersing steps in sequence to obtain barite powder for oil fields; the hydrophobic monomer is isobutylene; the initiator is azobisisobutyronitrile; the silane coupling agent is vinyltri(β-methoxyethoxy)silane; the particle size of the barite powder raw material is less than 1 micron; the amount of sodium stearate is 1.0% of the barite powder raw material; the amount of the silane coupling agent is 0.3% of the barite powder raw material; the amount of the hydrophobic monomer is 2% of the barite powder raw material; and the amount of the initiator is 0.3% of the hydrophobic monomer.

[0024] According to the test, the floating rate H of barite powder used in oil fields is 98.2%.

[0025] Example 3 This embodiment provides a barite powder for oil field, which is prepared by the following steps: Dissolve sodium stearate in an ethanol solution, add barite powder raw material, mix well, and obtain a barite powder suspension; Dispersing a silane coupling agent in an ethanol solution and adjusting the pH to 3-4 to obtain a silane coupling agent solution; Slowly add the silane coupling agent solution into the barite powder suspension and stir at 1000 r / min for 30 min; A hydrophobic monomer and an initiator are added, reacted at 100-120°C for 0.5 h, and filtering, washing, drying and breaking up are performed in sequence to obtain barite powder for oil fields; the hydrophobic monomer is hexafluorobutyl acrylate; the initiator is azobisisobutyronitrile; the silane coupling agent is γ-methacryloxypropyltrimethoxysilane; the particle size of the barite powder raw material is less than 1 micron; the amount of sodium stearate is 0.5% of the barite powder raw material; the amount of silane coupling agent is 0.8% of the barite powder raw material; the amount of hydrophobic monomer is 3% of the barite powder raw material; and the amount of initiator is 0.5% of the hydrophobic monomer.

[0026] After testing, the floating rate H of barite powder used in oil fields is 99.1%.

[0027] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, ordinary technicians in the field should understand that the specific implementation methods of the present invention can still be modified or some technical features can be replaced by equivalents without departing from the spirit of the technical solution of the present invention, which should be included in the scope of the technical solution for protection of the present invention.

Claims

1. A barite powder for oil field, which is prepared by the following steps: Dissolve sodium stearate in an ethanol solution, add barite powder raw material, mix well, and obtain a barite powder suspension; Dispersing a silane coupling agent in an ethanol solution, adjusting the pH to 3-4 or 9-10, to obtain a silane coupling agent solution; Slowly add the silane coupling agent solution into the barite powder suspension and stir evenly; A hydrophobic monomer and an initiator are added, reacted at 30-120° C. for 0.5-4 h, and filtering, washing, drying, and breaking up are performed in sequence to obtain barite powder for oil fields.

2. The barite powder for oil field according to claim 1, characterized in that: The particle size of the barite powder raw material is less than 1 micron; the dosage of sodium stearate is 0.1%-1.0% of the barite powder raw material; the dosage of silane coupling agent is 0.3%-1.0% of the barite powder raw material; the dosage of hydrophobic monomer is 1%-5% of the barite powder raw material; the dosage of initiator is 0.1%-1% of the hydrophobic monomer.

3. The barite powder for oil field according to claim 2, characterized in that: Slowly add the silane coupling agent solution into the barite powder suspension and stir at a speed of 1000-2000 r / min for 10-30 min.

4. The barite powder for oil field according to claim 3, characterized in that: The hydrophobic monomer is one or a combination of at least two of styrene, isobutylene, butadiene, butyl methacrylate, methyl methacrylate, and hexafluorobutyl acrylate.

5. The barite powder for oil field according to claim 4, characterized in that: The initiator is one of azobisisobutyronitrile, potassium persulfate, sodium persulfate, dibenzoyl peroxide, and N,N-dimethylaniline, or a combination of at least two of them.

6. The barite powder for oil field according to claim 5, characterized in that: The silane coupling agent is vinyl triethoxysilane, vinyl tri(β-methoxyethoxy)silane or γ-methacryloxypropyl trimethoxysilane.