Liquid crystal paste, ion transport composite film and solid-state battery
By optimizing the ratio of alkyl vinyl imidazole salts, solvents and additives, a high-purity liquid crystal slurry is formed and loaded on a porous support film, the problems of low purity and uneven structure of traditional liquid crystal monomers are solved, and high ionization is achieved Conductivity ion transport composite membrane suitable for solid-state batteries and other electronic products.
Patent Information
- Application Number
- CN202411231004.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-09-04
AI Technical Summary
The purity of the traditional alkyl vinyl imidazole salt liquid crystal monomer is not high, resulting in poor controllability and reduced conductivity in solid-state batteries and other applications. The layered compatibility causes the stability and structure of the liquid crystal to be uneven, which cannot meet high ions. The requirement of selectivity and high ion conductivity.
通过优化烷基乙烯基咪唑盐、溶剂和添加剂的配比,形成层状相溶致液晶结构,利用极性溶剂和添加剂诱导形成双分子层结构,调整烷基乙烯基咪唑盐的水合度以控制液晶层状相溶致液晶的结构参数,制备高纯度的液晶浆料,并将其负载在多孔支撑膜上制备离子传输复合膜。
The two-dimensional solvation channel of liquid crystal slurry is realized accurately control at the sub-nanometer scale, and the ion conductivity is improved to reach 36~150 mS·cm-1, which is suitable for solid-state batteries and other electronic products.
Smart Images

Figure CN118725875B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of batteries, and in particular relates to a liquid crystal paste, an ion transport composite membrane and a solid-state battery. Background Art
[0002] Liquid crystals have both the orderliness of solids (the molecules of a substance are arranged in a regular manner) and the fluidity of liquids. Under certain temperature and pressure, the molecules of liquid crystals will form a regular arrangement, and this orderly arrangement will change under the action of external forces such as electric fields, laying the foundation for the application of liquid crystals in many fields. In modern high-tech applications, especially in the fields of optoelectronic transmission equipment and chemical analysis, liquid crystal materials have received widespread attention for their unique optical properties and easily controllable configurations.
[0003] Liquid crystal monomers of alkyl vinyl imidazolium salts are considered to be ideal liquid crystal materials due to their strong chemical stability and excellent optical properties. However, the traditional synthesis method has low purity, which is mainly reflected in the high residual Br ion content, which leads to poor controllability of the liquid crystal phase and even induces the generation of harmful byproducts, resulting in a decrease in the conductivity of the liquid crystal monomer. In addition, the layered lyotropic liquid crystals prepared from liquid crystal monomers with low purity often have problems such as poor stability and uneven hierarchical structure, and cannot meet the high ion selectivity and high ion conductivity performance required by products in practical applications (such as solid-state batteries, sensors, supercapacitors, etc.). Summary of the invention
[0004] In order to overcome at least one technical problem existing in the above-mentioned prior art, one of the objectives of the present invention is to provide a liquid crystal paste.
[0005] A second object of the present invention is to provide a method for preparing a liquid crystal paste.
[0006] A third object of the present invention is to provide an ion transport composite membrane.
[0007] A fourth object of the present invention is to provide a solid-state battery.
[0008] A fifth object of the present invention is to provide application of the above-mentioned liquid crystal paste and / or the above-mentioned ion transport composite membrane in electronic products.
[0009] In order to achieve the above object, the technical solution adopted by the present invention is:
[0010] The first aspect of the present invention provides a liquid crystal paste, comprising an alkyl vinyl imidazole salt, a solvent and an additive; the mass ratio of the alkyl vinyl imidazole salt, the solvent and the additive is 1: (0.01-0.7): (0.001-1).
[0011] In the present invention, alkyl vinyl imidazolium salt forms lamellar solutropic liquid crystal under the induction of solvent (and additive), and is prepared into liquid crystal paste by optimizing the type of solvent (and additive). By adjusting the dosage ratio of alkyl vinyl imidazolium salt, solvent and additive, the lamellar solutropic liquid crystal structural parameters (for example, the single-period interlayer spacing of the lamellar solutropic liquid crystal, the thickness of the alkyl vinyl imidazolium salt liquid crystal layer, and the thickness of the solvation layer) are precisely controlled, so that the liquid crystal paste has a two-dimensional solvation channel and the size is precisely adjustable at the sub-nanometer scale.
[0012] Preferably, the mass ratio of the alkyl vinyl imidazole salt, the solvent and the additive is 1: (0.01-0.7): (0.01-1); further preferably, the mass ratio of the alkyl vinyl imidazole salt, the solvent and the additive is 1: (0.04-0.7): (0.01-1); more preferably, the mass ratio of the alkyl vinyl imidazole salt, the solvent and the additive is 1: (0.1-0.7): (0.01-0.3).
[0013] Preferably, the solvent is a polar solvent. The principle of polar solvent-induced lamellar solubility liquid crystal self-assembly of alkyl vinyl imidazole salts is that polar solvents tend to gather around the imidazole rings, which are also polar, and are easily repelled by non-polar alkyl chains. Non-polar alkyl chains tend to aggregate with adjacent alkyl chains and are arranged in order and gathered in the middle, forming a bilayer structure (similar to a phospholipid bilayer) with the imidazole rings facing outward and the alkyl chains gathered inside. At this time, the polar solvents gather around the imidazole rings and are distributed between the bilayers, thereby forming a lamellar solubility liquid crystal.
[0014] Preferably, the solvent is selected from at least one of water, methanol, ethanol, butanol, propanol, ethylene glycol, acetic acid, dichloromethane, chloroform, acetonitrile, tetrahydrofuran, dimethyl sulfoxide, dimethylformamide and dimethylacetamide.
[0015] Preferably, the additive is a polar additive. The additive used in the present invention has a certain polarity, for example, most acids are polar molecules; most two-dimensional materials are asymmetric polar structures, and most bases are polar molecules. The mechanism by which polar additives can assist the formation of lamellar solutropic liquid crystals is that polar additives tend to aggregate with polar imidazole rings (solvent-free state) and polar solvents (solvent state), and induce alkyl vinyl imidazole salts to assemble a lamellar solutropic liquid crystal structure with bilayer characteristics by the same mechanism.
[0016] Preferably, the additive is selected from at least one of sulfuric acid, hydrochloric acid, nitric acid, phosphoric acid, tetrafluoroboric acid, hexafluorophosphoric acid, a photoinitiator, a crosslinker, titanium oxide, graphene, graphene oxide, boron nitride, molybdenum disulfide, MXene, sodium hydroxide, potassium hydroxide, an organic amine, a sulfonic acid, and a sulfonate.
[0017] Preferably, the alkyl vinyl imidazole salt is selected from at least one of alkyl vinyl imidazole hydrogen sulfate, alkyl vinyl imidazole bromide, alkyl vinyl imidazole chloride, alkyl vinyl imidazole nitrate, alkyl vinyl imidazole tetrafluoroborate, and alkyl vinyl imidazole hexafluorophosphate. Further preferably, the alkyl vinyl imidazole salt is selected from at least one of tetradecyl vinyl imidazole bromide, tetradecyl vinyl imidazole chloride, tetradecyl vinyl imidazole nitrate, dodecyl vinyl imidazole bromide, tetradecyl vinyl imidazole tetrafluoroborate, tetradecyl vinyl imidazole hexafluorophosphate, dodecyl vinyl imidazole chloride, dodecyl vinyl imidazole nitrate, dodecyl vinyl imidazole hydrogen sulfate, dodecyl vinyl imidazole tetrafluoroborate, and dodecyl vinyl imidazole hexafluorophosphate.
[0018] Wherein, the structural formula of the alkyl vinyl imidazole hydrogen sulfate in the present invention is as follows:
[0019]
[0020] Preferably, the alkyl group in the alkyl vinyl imidazole salt is selected from C1 to C 30 Preferably, the alkyl group in the alkyl vinyl imidazole salt is selected from C1 to C 20 Preferably, the alkyl group in the alkyl vinyl imidazole salt is selected from C 10 ~C 20 More preferably, the alkyl group in the alkyl vinyl imidazole salt is selected from C 10 ~C 15 A straight chain or branched chain alkyl group.
[0021] Preferably, when the solvent in the liquid crystal slurry is water, the hydration degree of the alkyl vinyl imidazolate salt is 1 to 13, for example, the hydration degree of the alkyl vinyl imidazolate salt may be 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13. In the present invention, the hydration degree of the alkyl vinyl imidazolate salt can be adjusted to be in the range of 1 to 13 by adjusting the usage amount of the alkyl vinyl imidazolate salt and the solvent water. By adjusting the hydration degree, the water content between two adjacent molecular layers of the alkyl vinyl imidazolate salt can be regulated, and the increase in water content leads to the thickening of the water layer, thereby controlling the structural parameters of the lamellar lyotropic liquid crystal.
[0022] Preferably, the liquid crystal paste is a lamellar lyotropic liquid crystal.
[0023] Preferably, the liquid crystal slurry contains an alkyl vinyl imidazole salt molecular layer and a solvent layer; the alkyl vinyl imidazole salt molecular layer and the solvent layer are alternately stacked. The alkyl vinyl imidazole salt in the present invention can form a liquid crystal with a layered monolayer structure or a layered bilayer structure under the induction of a solvent. When the alkyl vinyl imidazole salt forms a layered monolayer structure under the induction of a solvent, a solvent layer exists between two adjacent layers of the layered monolayer structure, and the solvent layer serves as an ion transmission channel. When the alkyl vinyl imidazole salt forms a layered bilayer structure under the induction of a solvent, a solvent layer exists between two adjacent layers of the layered bilayer structure.
[0024] Preferably, the distance between two adjacent alkyl vinyl imidazolium salt molecular layers is 0.2-0.98 nm.
[0025] Preferably, the alkyl vinyl imidazole salt is prepared by a preparation method comprising the following steps:
[0026] S1: mixing alkyl halide and vinyl imidazole to react to obtain a crude product;
[0027] S2: recrystallizing the crude product at least twice to obtain a first product;
[0028] S3: Under inert gas purging, the first product and the acid solution are mixed and reacted at a temperature below 10° C., and then refluxed to react. After the reaction is completed, the product is crystallized at least twice to obtain.
[0029] Step S3 of the present invention is to react the first product with concentrated sulfuric acid at low temperature first, and then heat it to react at a higher temperature, which is to ensure that the halide in the reaction container fully participates in the reaction and reduce the content of halogen elements in the obtained alkyl vinyl imidazole salt.
[0030] Preferably, the acid solution is selected from at least one of sulfuric acid, hydrobromic acid, hydrochloric acid, nitric acid, tetrafluoroboric acid, and hexafluorophosphoric acid.
[0031] Preferably, in the step S1, the mixing reaction temperature is 20-100°C; further preferably, in the step S1, the mixing reaction temperature is 20-80°C; more preferably, in the step S1, the mixing reaction temperature is 20-50°C.
[0032] Preferably, in step S1, the mass ratio of vinyl imidazole to alkyl halide is 1:(0.1-10).
[0033] Preferably, the solvent used in step S1 is at least one selected from alcohols, esters, chloroalkanes and acetonitrile.
[0034] Preferably, in step S1, the mass ratio of the total mass of the alkyl halide and vinyl imidazole to the solvent is 1:(80-120); further preferably, in step S1, the mass ratio of the total mass of the alkyl halide and vinyl imidazole to the solvent is 1:(90-110).
[0035] Preferably, in step S1, the reaction atmosphere of the mixed reaction is selected from air, nitrogen and argon.
[0036] Preferably, in step S1, the mixing reaction time is 24 to 72 hours; further preferably, in step S1, the mixing reaction time is 30 to 40 hours.
[0037] Preferably, in step S2, the solvent used for recrystallization is selected from n-hexane or ethyl acetate.
[0038] Preferably, the step S2 further comprises the step of vacuum drying the first product obtained by recrystallization.
[0039] Preferably, the vacuum drying temperature is 20-80°C.
[0040] Preferably, in step S3, the molar ratio of the first product to concentrated sulfuric acid is 1:(1-1.5).
[0041] Preferably, the reaction solvent in step S3 is selected from anhydrous ethanol and anhydrous ethyl acetate.
[0042] Preferably, the reaction environment humidity in step S3 is less than 60RH%.
[0043] Preferably, in step S3, the inert gas purge rate is: the gas purge rate per gram of reactant is greater than 0.1 L / min.
[0044] Preferably, in step S3, the reaction time is ≥ 2 h / g of reactant at a temperature below 10°C.
[0045] Preferably, in step S3, the recrystallization solvent is anhydrous ether, and the recrystallization temperature is less than 0°C.
[0046] Preferably, the content of halogen element in the alkyl vinyl imidazolium salt is less than 0.01%.
[0047] Preferably, the stirring rate in the mixing reaction step in step S3 is 10-1000 rpm; further preferably, the stirring rate in the mixing reaction step in step S3 is 200-800 rpm; more preferably, the stirring rate in the mixing reaction step in step S3 is 400-800 rpm.
[0048] Preferably, the stirring rate in the reflux reaction step in step S3 is 10-1000 rpm; further preferably, the stirring rate in the reflux reaction step in step S3 is 100-500 rpm; more preferably, the stirring rate in the reflux reaction step in step S3 is 200-500 rpm.
[0049] Preferably, the white smoke generated in the mixing reaction step in step S3 is absorbed by alkaline solution.
[0050] The second aspect of the present invention provides a method for preparing the liquid crystal paste according to the first aspect of the present invention, comprising the following steps:
[0051] The alkyl vinyl imidazole salt, solvent and additive are mixed, and the mixture is allowed to stand after degassing to obtain the liquid crystal paste.
[0052] Preferably, the mixing method includes at least one of stirring, shaking, oscillating, ultrasonic, centrifugal and ball milling.
[0053] Preferably, the standing time is ≥ 1 day.
[0054] Preferably, the solvent is added in a manner selected from the group consisting of a dropwise addition method, a pouring method, a drainage method, and an injection method.
[0055] Preferably, the degassing step is to degas by centrifugation.
[0056] The third aspect of the present invention provides an ion transport composite membrane, comprising a porous support membrane and the liquid crystal paste described in the first aspect of the present invention; the liquid crystal paste is loaded on the porous support membrane.
[0057] Preferably, the porous support membrane is selected from a polymer porous support membrane, an inorganic material porous support membrane or a combination thereof.
[0058] Preferably, the polymer porous support membrane is selected from at least one of polyvinylidene fluoride membrane, polypropylene membrane, polysulfone membrane, polyethersulfone membrane, polyimide membrane, polytetrafluoroethylene membrane, polyurethane membrane and polyvinyl cyanate membrane.
[0059] Preferably, the inorganic material porous support membrane is selected from at least one of an aluminum oxide membrane, a silicon dioxide membrane, a titanate membrane, a zirconium oxide membrane, a carbon material membrane, a molecular sieve membrane, a metal oxide membrane, a magnesium aluminum spinel membrane, and a barium sulfate membrane.
[0060] Preferably, the ion conductivity of the ion transport composite membrane is 36-150 mS·cm -1 .
[0061] Preferably, the ion transport composite membrane is used to transport an ion selected from H + 、Na+ , Li + , Cl - CF3SO3 - 、SO4 2- OH - At least one ion.
[0062] Preferably, the ion transport composite membrane is prepared by a preparation method comprising the following steps:
[0063] The liquid crystal paste is loaded on the porous supporting film, which is then sealed and left to stand under the protection of an inert gas to obtain the product.
[0064] Preferably, the loading method is selected from at least one of a coating method, a spraying method, a template transfer method, a pre-rolling method, and a slit coating method.
[0065] The fourth aspect of the present invention provides a solid-state battery, comprising the ion transport composite membrane described in the first aspect of the present invention.
[0066] The fifth aspect of the present invention provides the use of the liquid crystal paste described in the first aspect of the present invention and / or the ion transport composite membrane described in the third aspect of the present invention in electronic products.
[0067] Preferably, the electronic product includes a battery, a sensor, and a supercapacitor.
[0068] The beneficial effects of the present invention are as follows: the liquid crystal paste in the present invention can make the alkyl vinyl imidazolium salt self-assemble under the induction of solvents and additives to form lamellar solubility liquid crystals, and by adjusting the dosage ratio of the alkyl vinyl imidazolium salt, the solvent and the additive, the lamellar solubility liquid crystal structural parameters (for example, the single-period interlayer spacing of the lamellar solubility liquid crystal, the thickness of the alkyl vinyl imidazolium salt liquid crystal layer, and the thickness of the solvation layer) can be precisely controlled, so that the liquid crystal paste has a two-dimensional solvation channel and the size is precisely adjustable at the sub-nanometer scale.
[0069] The ion transport composite membrane of the present invention can achieve adjustable ion conductivity of the composite membrane by loading liquid crystal slurry on the porous support membrane, and achieve a higher ion conductivity, specifically 36~150 mS·cm -1 , can be used to transmit H + 、Na + , Li + , Cl - CF3SO3 - 、SO4 2- OH - Plasma can be used in electronic products such as batteries, sensors, and supercapacitors. BRIEF DESCRIPTION OF THE DRAWINGS
[0070] Figure 1 1 is a flow chart of the preparation process of the lamellar lyotropic liquid crystal composite film based on the lamellar lyotropic liquid crystal in Examples 1 to 3.
[0071] Figure 2 This is a physical picture of the lamellar lyotropic liquid crystal prepared in Examples 1 to 3.
[0072] Figure 3 This is a physical picture of the layered lyotropic liquid crystal composite film prepared in Examples 1 to 3.
[0073] Figure 4 This is the energy spectrum of the tetradecylvinyl imidazole hydrogen sulfate liquid crystal monomer in Example 1.
[0074] Figure 5 This is the FTIR spectrum of the tetradecylvinyl imidazole hydrogen sulfate liquid crystal monomer in Example 1.
[0075] Figure 6 This is the POM image of the lamellar lyotropic liquid crystal paste prepared in Example 1.
[0076] Figure 7 This is the POM image of the lamellar lyotropic liquid crystal paste prepared in Example 2.
[0077] Figure 8 This is the POM image of the lamellar lyotropic liquid crystal paste prepared in Example 3.
[0078] Fig. 9 1 is the SAXS graph of the lamellar lyotropic liquid crystal paste prepared in Examples 1 to 3.
[0079] Fig.10 This is a test graph of the ionic conductivity of the lamellar solutropic liquid crystal paste prepared in Examples 1 to 3. DETAILED DESCRIPTION
[0080] The specific implementation of the present invention is further described in detail below in conjunction with the accompanying drawings and examples, but the implementation and protection of the present invention are not limited thereto. It should be noted that if there are processes that are not particularly described in detail below, they can be implemented or understood by those skilled in the art with reference to the prior art. The reagents or instruments used that do not indicate the manufacturer are all conventional products that can be purchased commercially.
[0081] Example 1
[0082] Reference Figure 1 The preparation process flow chart in this example provides a preparation method of a composite film based on lamellar lyotropic liquid crystal, and the preparation method comprises the following steps:
[0083] 1. Preparation of high purity tetradecyl vinyl imidazole hydrogen sulfate liquid crystal monomer
[0084] (1) At room temperature, tetradecane bromide (100 g) and vinyl imidazole (30 g) were added to the reactor in sequence, and the reaction was carried out under the protection of nitrogen atmosphere with isopropanol as solvent (volume ratio of isopropanol to reactants = 100:1). After 5 hours, the reaction was completed and the residual solvent was removed by vacuum rotary evaporation. The crude product was gradually dripped into n-hexane for recrystallization. During the process, the crude product was ensured to be in full contact with n-hexane, and then recrystallized at 0 ° C. This was repeated three times, and filtered to obtain a white powder. The obtained white powder was added to n-hexane, recrystallized at 0 ° C. This was repeated three times, and filtered to obtain a white powder, which was the first step monomer.
[0085] (2) At a temperature higher than 25°C, for example, 30°C, the first step monomer is dissolved in anhydrous ethanol and stabilized under gas purge to ensure that the environmental humidity of the reaction system is less than 60% RH. After the reaction temperature is lower than 10°C, concentrated sulfuric acid is slowly dripped in under vigorous stirring (stirrer speed 100 rpm) and gas purge (gas sweep rate 0.5 L / min), and the reaction is continued at 2°C. The white smoke produced by the reaction is absorbed by an aqueous solution containing sodium hydroxide until the pH of the tail gas is monitored to be neutral. Then, the reaction is switched from medium-low temperature to medium-high temperature to ensure that there is no bromide residue in the reactor. Specifically, the reaction is heated under reflux for 10 hours under nitrogen purge, and the pH of the tail gas is monitored to be neutral to mark the end of the reaction. After the reaction is completed, the residual solvent in the reaction system is removed by vacuum rotary evaporation to obtain a crude product. The crude product was added into 50 mL of anhydrous ether. During the process, the crude product was ensured to be in full contact with the anhydrous ether. The product was recrystallized at 0°C and repeated three times. After filtration and vacuum drying, a white powdery solid was obtained, which was the high-purity tetradecylvinyl imidazole hydrogen sulfate liquid crystal monomer in this example.
[0086] 2. Preparation of lamellar lyotropic liquid crystal slurry
[0087] The solvent in this example is water, and the additive is an aqueous sulfuric acid solution.
[0088] 52g of tetradecyl vinyl imidazole hydrogen sulfate powder was placed in a container, and 15.65g of 3 mol / L sulfuric acid aqueous solution was added dropwise into the container, and a mixed system was prepared with a monomer hydration degree of 5 as the target; the following steps were adopted to obtain a uniformly dispersed lamellar phase-solubilizing liquid crystal slurry: ① Use a glass rod to stir fully to make the solid and liquid phases preliminarily mixed and uniform; ② Use ultrasonic vibration to shake at room temperature to fully dissolve the undissolved solid in the system; ③ Repeat the above two steps in sequence for no less than 3 times; ④ Use a centrifuge to centrifuge at 10000 rpm at room temperature for 10 min to remove bubbles in the system; ⑤ Use a sealing film to seal the centrifuge tube mouth to prevent solvent volatilization and impurities from mixing, and let it stand for 1 day to achieve full and uniform self-assembly of tetradecyl vinyl imidazole hydrogen sulfate, and at the same time eliminate the residual stress generated between the two-dimensional liquid crystal domains during the stirring and mixing process of the sample, so as to obtain a lamellar phase-solubilizing liquid crystal slurry, the actual picture of which is shown in the figure below. Figure 2 As shown in (A), the hydration degree of tetradecylvinyl imidazole hydrogen sulfate in the lamellar soluble liquid crystal paste is 5.
[0089] 3. Preparation of composite films based on lamellar lyotropic liquid crystals
[0090] The porous support membrane in this example takes a PTFE hydrophilic membrane as an example.
[0091] The PTFE porous support membrane was cut into a circle with a diameter of 1 cm, and 1 mL of the prepared lamellar solutropic liquid crystal slurry was applied to the surface of the PTFE porous support membrane. The PTFE porous support membrane loaded with the lamellar solutropic liquid crystal slurry was sealed with nitrogen gas protection and left to stand for 1 day to obtain a composite membrane, and then the obtained composite membrane was vacuum dried at 40°C for 24 h to obtain the composite membrane based on lamellar solutropic liquid crystal in this example, as shown in the physical picture Figure 3 As shown in (a) in .
[0092] The energy spectrum of the tetradecyl vinyl imidazole hydrogen sulfate liquid crystal monomer prepared in this example is tested. Figure 4 As shown by Figure 4 It can be seen that the Br content is not measured in the tetradecyl vinyl imidazole hydrogen sulfate liquid crystal monomer, indicating that the Br content is less than 0.01%. The tetradecyl vinyl imidazole hydrogen sulfate liquid crystal monomer prepared in this example has a high purity.
[0093] The FTIR spectrum of the tetradecyl vinyl imidazole hydrogen sulfate liquid crystal monomer prepared in this example is as follows: Figure 5 As shown by Figure 5 It can be seen that the tetradecylvinylimidazole hydrogen sulfate liquid crystal monomer contains carbon-carbon double bonds, -SO2, oxygen-sulfur single bonds, and absorption waves of imidazole rings, which further proves that the tetradecylvinylimidazole hydrogen sulfate liquid crystal monomer was successfully synthesized in this example.
[0094] Example 2
[0095] Reference Figure 1 The preparation process flow chart in this example provides a preparation method of a composite film based on lamellar lyotropic liquid crystal, and the preparation method comprises the following steps:
[0096] 1. Synthesis of Tetradecylvinylimidazole Hydrogen Sulfate Liquid Crystalline Monomer:
[0097] (1) At room temperature, tetradecane bromide (100 g) and vinyl imidazole (30 g) were added to the reactor in sequence, and the reaction was carried out under the protection of nitrogen atmosphere with isopropanol as solvent (volume ratio of isopropanol to reactants = 100:1). After 5 hours, the reaction was completed and the residual solvent was removed by vacuum rotary evaporation. The crude product was gradually dropped into n-hexane for recrystallization. During the process, the crude product was ensured to be in full contact with n-hexane, and then recrystallized at 0 ° C. This was repeated four times, and filtered to obtain a white powder. The obtained white powder was added to n-hexane, recrystallized at 0 ° C. This was repeated four times, and filtered to obtain a white powder, which was the first step monomer.
[0098] (2) At a temperature not lower than 25°C, for example, 30°C, the first step monomer is dissolved in anhydrous ethanol and stabilized under gas purge to ensure that the environmental humidity of the reaction system is lower than 50% RH. After the reaction temperature is lower than 20°C, concentrated sulfuric acid is slowly dripped under vigorous stirring (stirrer speed is 300 rpm) and gas purge (gas sweep rate is 0.6 L / min), and the reaction is continued at 2°C. The white smoke produced by the reaction is absorbed by an aqueous solution containing sodium hydroxide until the pH of the tail gas is monitored to be neutral. Then, the reaction is switched from medium-low temperature to medium-high temperature to ensure that there is no bromide residue in the reactor. Specifically, the reaction is heated under reflux for 10 hours under nitrogen purge, and the pH of the tail gas is monitored to be neutral to mark the end of the reaction. After the reaction is completed, the residual solvent in the reaction system is removed by vacuum rotary evaporation to obtain a crude product. The crude product was added into 150 mL of anhydrous ether. During the process, the crude product was ensured to be in full contact with the anhydrous ether. The product was recrystallized at 0°C and the process was repeated three times. After filtration and vacuum drying, a white powdery solid was obtained, which was the high-purity tetradecylvinylimidazole hydrogen sulfate liquid crystal monomer in this example.
[0099] 2. Preparation of two-dimensional lamellar liquid crystal slurry:
[0100] In this example, the solvent is water, and the additive is aqueous sulfuric acid solution.
[0101] 33g of tetradecyl vinyl imidazole hydrogen sulfate powder was placed in a container, and 16.40g of 2mol / L sulfuric acid aqueous solution was added dropwise to the container, and a mixed system was prepared with a monomer hydration degree of 9 as the target; the following steps were adopted to obtain a uniformly dispersed lamellar solubility liquid crystal system: ① Use a glass rod to stir fully to make the solid and liquid phases preliminarily mixed and uniform; ② Use ultrasonic vibration to vibrate at room temperature to fully dissolve the undissolved solid in the system; ③ Repeat the above two steps in sequence for no less than 2 times; ④ Use a centrifuge to centrifuge at 10000 rpm at room temperature for 10 min to remove bubbles in the system; ⑤ Use a sealing film to seal the centrifuge tube mouth to prevent solvent volatilization and impurities from mixing, and let it stand for 1 day to achieve full and uniform self-assembly of tetradecyl vinyl imidazole hydrogen sulfate, and at the same time eliminate the residual stress generated between the two-dimensional liquid crystal domains during the stirring and mixing process of the sample, and prepare a lamellar solubility liquid crystal slurry, the actual picture of which is as shown in the figure Figure 2 As shown in (B), the hydration degree of tetradecylvinyl imidazole hydrogen sulfate in the lamellar soluble liquid crystal paste is 9.
[0102] 3. Preparation of composite films based on lamellar lyotropic liquid crystals:
[0103] In this example, the porous support membrane takes a PTFE hydrophilic membrane as an example.
[0104] The PTFE porous support membrane was cut into a circle with a diameter of 1 cm, and 1 mL of the prepared lamellar solutropic liquid crystal slurry was applied to the surface of the PTFE porous support membrane. The PTFE porous support membrane loaded with the lamellar solutropic liquid crystal slurry was sealed, protected with nitrogen gas and left to stand for 1 day, and then the obtained composite membrane was vacuum dried at 40 °C for 24 h to obtain the composite membrane based on lamellar solutropic liquid crystal in this example, as shown in the physical picture Figure 3 As shown in (b) in .
[0105] After testing, the Br content was not detected in the energy spectrum of the tetradecyl vinyl imidazole hydrogen sulfate liquid crystal monomer prepared in this example, indicating that the Br content was less than 0.01%. The tetradecyl vinyl imidazole hydrogen sulfate liquid crystal monomer prepared in this example has a high purity.
[0106] Example 3
[0107] Reference Figure 1 The preparation process flow chart in this example provides a preparation method of a composite film based on lamellar lyotropic liquid crystal, and the preparation method comprises the following steps:
[0108] 1. Synthesis of Tetradecylvinylimidazole Hydrogen Sulfate Liquid Crystalline Monomer:
[0109] (1) At room temperature, tetradecane bromide (100 g) and vinyl imidazole (30 g) were added to the reactor in sequence, and the reaction was carried out under the protection of nitrogen atmosphere with isopropanol as solvent (volume ratio of isopropanol to reactants = 100:1). After 5 hours, the reaction was completed and the residual solvent was removed by vacuum rotary evaporation. The crude product was gradually dripped into n-hexane for recrystallization. During the process, the crude product was ensured to be in full contact with n-hexane, and then recrystallized at 0 ° C. This was repeated three times, and filtered to obtain a white powder. The obtained white powder was added to n-hexane, recrystallized at 0 ° C. This was repeated three times, and filtered to obtain a white powder, which was the first step monomer.
[0110] (2) At a temperature not lower than 25°C, for example, 30°C, the first step monomer is dissolved in anhydrous ethanol and stabilized under gas purge to ensure that the environmental humidity of the reaction system is lower than 70% RH. After the reaction temperature is lower than 20°C, concentrated sulfuric acid is slowly dripped under vigorous stirring (stirrer speed is 80 rpm) and gas purge (gas sweep rate is 0.1L / min), and the reaction is continued at 2°C. The white smoke produced by the reaction is absorbed by an aqueous solution containing sodium hydroxide until the pH of the tail gas is monitored to be neutral. Then, the reaction is switched from medium-low temperature to medium-high temperature to ensure that there is no bromide residue in the reactor. Specifically, the reaction is heated under reflux for 10 hours under nitrogen purge, and the pH of the tail gas is monitored to be neutral to mark the end of the reaction. After the reaction is completed, the residual solvent in the reaction system is removed by vacuum rotary evaporation to obtain a crude product. The crude product was added into 100 mL of anhydrous ether. During the process, the crude product was ensured to be in full contact with the anhydrous ether. The product was recrystallized at 0° C. and the process was repeated three times. After filtration and vacuum drying, a white powdery solid was obtained, which was a high-purity tetradecylvinylimidazole hydrogen sulfate liquid crystal monomer.
[0111] 2. Preparation of two-dimensional lamellar liquid crystal slurry:
[0112] In this example, the solvent is water, and the additive is aqueous sulfuric acid solution.
[0113] 25.7g of tetradecyl vinyl imidazole hydrogen sulfate powder was placed in a container, and 17g of 1mol / L sulfuric acid aqueous solution was added dropwise to the container, and a mixed system was prepared with a monomer hydration degree of 13 as the target; the following steps were adopted to obtain a uniformly dispersed lamellar solubility liquid crystal system: ① Use a glass rod to stir fully to make the solid and liquid phases preliminarily mixed and uniform; ② Use ultrasonic vibration to vibrate at room temperature to fully dissolve the undissolved solid in the system; ③ Repeat the above two steps in sequence for no less than 2 times; ④ Use a centrifuge to centrifuge at 10000 rpm at room temperature for 10 min to remove bubbles in the system; ⑤ Use a sealing film to seal the centrifuge tube mouth to prevent solvent volatilization and impurities from mixing, and let it stand for 1 day to achieve full and uniform self-assembly of tetradecyl vinyl imidazole hydrogen sulfate, and at the same time eliminate the residual stress generated between the two-dimensional liquid crystal domains during the stirring and mixing process of the sample, and obtain a lamellar solubility liquid crystal slurry, the actual picture of which is as shown in the figure Figure 2 As shown in (C), the hydration degree of tetradecylvinyl imidazole hydrogen sulfate in the lamellar soluble liquid crystal paste is 13.
[0114] 3. Preparation of composite films based on lamellar lyotropic liquid crystals:
[0115] In this example, the porous support membrane takes a PTFE hydrophilic membrane as an example.
[0116] The PTFE porous support membrane was cut into a circle with a diameter of 1 cm, and 1 mL of the prepared lamellar solutropic liquid crystal slurry was applied to the surface of the PTFE porous support membrane. The porous support membrane loaded with the lamellar solutropic liquid crystal slurry was sealed and protected with nitrogen gas and left to stand for 1 day, and then the obtained composite membrane was vacuum dried at 40°C for 24 h to obtain the composite membrane based on lamellar solutropic liquid crystal in this example, as shown in the physical picture. Figure 3 As shown in (c) in .
[0117] After testing, the Br content was not detected in the energy spectrum of the tetradecyl vinyl imidazole hydrogen sulfate liquid crystal monomer prepared in this example, indicating that the Br content was less than 0.01%. The tetradecyl vinyl imidazole hydrogen sulfate liquid crystal monomer prepared in this example has a high purity.
[0118] Example 4
[0119] The method for preparing the composite film based on lamellar lyotropic liquid crystal in this example is different from that in Example 3 only in that the preparation steps of the two-dimensional lamellar liquid crystal slurry in step 2 are different, specifically:
[0120] 30 g of tetradecyl vinyl imidazole hydrogen sulfate powder was placed in a container, 1.5 g of 1 mol / L sulfuric acid aqueous solution was added dropwise into the container, and a mixed system was prepared with a monomer hydration degree of 1 as the target; the following steps were adopted to obtain a uniformly dispersed lamellar solubility liquid crystal system: ① Use a glass rod to stir fully to make the solid and liquid phases preliminarily mixed and uniform; ② Use ultrasonic vibration to vibrate at room temperature to fully dissolve the undissolved solid in the system; ③ Repeat the above two steps in sequence for no less than 2 times; ④ Use a centrifuge to centrifuge at 10000 rpm at room temperature for 10 min to remove bubbles in the system; ⑤ Use a sealing film to seal the centrifuge tube mouth to prevent solvent volatilization and impurities from mixing, and let it stand for 1 day to achieve full and uniform self-assembly of tetradecyl vinyl imidazole hydrogen sulfate, and at the same time eliminate the residual stress generated between the two-dimensional liquid crystal domains during the stirring and mixing process of the sample to obtain a lamellar solubility liquid crystal slurry.
[0121] Example 5
[0122] This example provides a solid-state battery, including a solid-state electrolyte, wherein the solid-state electrolyte includes the composite film based on lamellar lyotropic liquid crystal in Example 1.
[0123] Example 6
[0124] This example provides a solid-state battery, including a solid-state electrolyte, wherein the solid-state electrolyte includes the composite film based on lamellar lyotropic liquid crystal in Example 1.
[0125] Example 7
[0126] This example provides a solid-state battery, including a solid-state electrolyte, wherein the solid-state electrolyte includes the composite film based on lamellar lyotropic liquid crystal in Example 1.
[0127] The composite film based on lamellar phase-solid liquid crystal in the embodiment of the present invention can be used as a quasi-solid electrolyte in a solid-state battery. Depending on the application scenario, different ions can be selected to assemble the liquid crystal slurry and fill it to form a quasi-solid electrolyte membrane for different scenarios, such as: hydroxide (for anion exchange membrane fuel cells / electrolysis of water to produce hydrogen), hydrogen sulfate (for proton exchange membrane fuel cells / electrolysis of water to produce hydrogen), anhydrous + sodium ions (for sodium ion batteries), anhydrous + lithium ions (for lithium ion batteries), water + zinc ions (for zinc ion batteries), water + any ions (for supercapacitors).
[0128] Performance Testing:
[0129] The layered lyotropic liquid crystal pastes prepared in Examples 1 to 3 were observed under a polarizing microscope, and the polarizing microtexture characteristics were monitored and recorded at different temperatures. The POM image of Example 1 (hydration degree of 5) measured at 35° C. is shown in FIG. Figure 6 As shown, the POM diagram of Example 2 (hydration degree 9) measured at 30°C is as follows Figure 7 As shown, the POM diagram of Example 3 (hydration degree is 13) measured at 25°C is as follows Figure 8 As shown. Figure 6~Figure 8 It can be seen that the tetradecylvinyl imidazole hydrogen sulfate in the lamellar lyotropic liquid crystal pastes prepared in Examples 1 to 3 is not oriented.
[0130] The SAXS spectra of the layered lyotropic liquid crystal pastes prepared in Examples 1 to 3 were tested using a small-angle X-ray scattering instrument. The specific test results are as follows: Fig. 9 As shown. Fig. 9It can be seen that in the lamellar interphase lyotropic liquid crystal slurry of Example 1, the hydration degree of tetradecyl vinyl imidazole hydrogen sulfate is 5, and its two-dimensional lamellar liquid crystal single period interlayer spacing is 0.46nm. In the lamellar interphase lyotropic liquid crystal slurry of Example 2, the hydration degree of tetradecyl vinyl imidazole hydrogen sulfate is 9, and its two-dimensional lamellar liquid crystal single period interlayer spacing is 0.72nm. In the lamellar interphase lyotropic liquid crystal slurry of Example 3, the hydration degree of tetradecyl vinyl imidazole hydrogen sulfate is 13, and its two-dimensional lamellar liquid crystal single period interlayer spacing is 0.98nm. By comparing Examples 1 to 3, it can be seen that the present invention can adjust the dosage ratio of the solvent and the alkyl vinyl imidazole hydrogen sulfate in the lamellar interphase lyotropic liquid crystal slurry to adjust the hydration degree of the alkyl vinyl imidazole hydrogen sulfate so that the hydration degree of the alkyl vinyl imidazole hydrogen sulfate is between 1 and 13. In addition, the present invention can also adjust the hydration parameters of alkyl vinyl imidazole hydrogen sulfate to adjust the water content between the lamellar solutropic liquid crystal layers, thereby adjusting the thickness of the water layer, and then adjusting the structural parameters of the lamellar solutropic liquid crystal, thereby achieving control of the structural parameters of the lamellar solutropic liquid crystal composite film.
[0131] The ionic conductivity of the layered lyotropic liquid crystal composite films prepared in Examples 1 to 3 was tested respectively. The testing method is as follows: the ionic conductivity of the composite films in Examples 1 to 3 was tested by two-electrode electrochemical impedance spectroscopy at room temperature and indoor humidity using a "sandwich" method: the composite film was sandwiched between two stainless steel plates to ensure that the composite film was in full contact with the plates, and the ionic conductivity of the composite film was measured. The specific test results are shown in FIG. Fig.10 As shown. Fig.10 It can be seen that the ionic conductivity of the layered lyotropic liquid crystal composite films in Examples 1 to 3 is 36.1 mS·cm -1 、93.03 mS·cm -1 、148.1 mS·cm -1 It can be seen that with the increase of the hydration degree of alkyl vinyl imidazolium hydrogen sulfate, the thickness of the ion transport solvent layer increases, and the ionic conductivity of the lamellar solubility liquid crystal composite film based on alkyl vinyl imidazolium hydrogen sulfate also gradually increases.
[0132] In summary, the two-dimensional liquid crystal lamellar channels formed by solvation in the lamellar solutropic liquid crystal composite film of the present invention are conducive to the rapid conduction of ions, and can achieve precise control of the channel size at the subnanometer level by regulating the hydration parameters of alkyl vinyl imidazolium hydrogen sulfate, and precisely regulate the ion conduction performance of the composite film, thereby obtaining a lamellar solutropic liquid crystal composite film with higher ion conductivity.
[0133] The above is a detailed description of the embodiments of the present invention, but the present invention is not limited to the above embodiments. Various changes can be made within the knowledge of ordinary technicians in the relevant technical field without departing from the purpose of the present invention. In addition, the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.
Claims
1. An ion transport composite membrane, characterized in that: It comprises a porous support film and a liquid crystal paste; the liquid crystal paste is loaded on the porous support film; the liquid crystal paste comprises an alkyl vinyl imidazole salt, a solvent and an additive; the mass ratio of the alkyl vinyl imidazole salt, the solvent and the additive is 1: (0.01-0.7): (0.001-1); The additive is selected from sulfuric acid; The liquid crystal paste is a lamellar lyotropic liquid crystal; The liquid crystal paste contains alkyl vinyl imidazole salt molecular layers and solvent layers; the alkyl vinyl imidazole salt molecular layers and solvent layers are alternately stacked; The solvent in the liquid crystal slurry is water, and the hydration degree of the alkyl vinyl imidazole salt is 1 to 13; The alkyl vinyl imidazole salt is alkyl vinyl imidazole hydrogen sulfate; The alkyl group in the alkyl vinyl imidazole salt is selected from C 10 ~C 20 A straight chain or branched chain alkyl group.
2. The ion transport composite membrane according to claim 1, characterized in that: The distance between two adjacent alkyl vinyl imidazolium salt molecular layers is 0.2-0.98 nm.
3. The ion transport composite membrane according to claim 1, characterized in that: The alkyl vinyl imidazole salt is prepared by a preparation method comprising the following steps: S1: mixing alkyl halide and vinyl imidazole to react to obtain a crude product; S2: recrystallizing the crude product at least twice to obtain a first product; S3: Under inert gas purging, the first product and the acid solution are mixed and reacted at a temperature below 10° C., and then refluxed to react. After the reaction is completed, the product is crystallized at least twice to obtain.
4. The ion transport composite membrane according to claim 3, characterized in that: The content of halogen in the alkyl vinyl imidazole salt is less than 0.01%; And / or, the acid solution is selected from sulfuric acid.
5. The ion transport composite membrane according to claim 1, characterized in that: The liquid crystal paste is prepared by a preparation method comprising the following steps: The alkyl vinyl imidazole salt, solvent and additive are mixed, and the mixture is allowed to stand after degassing to obtain the liquid crystal paste.
6. The ion transport composite membrane according to claim 1, characterized in that: The porous support membrane is selected from a polymer porous support membrane, an inorganic material porous support membrane or a combination thereof.
7. The ion transport composite membrane according to claim 6, characterized in that: The polymer porous support membrane is selected from at least one of polyvinylidene fluoride membrane, polypropylene membrane, polysulfone membrane, polyethersulfone membrane, polyimide membrane, polytetrafluoroethylene membrane, polyurethane membrane and polyvinyl cyanate membrane; And / or, the inorganic material porous support membrane is selected from at least one of aluminum oxide membrane, silicon dioxide membrane, titanate membrane, zirconium oxide membrane, carbon material membrane, molecular sieve membrane, metal oxide membrane, magnesium aluminum spinel membrane and barium sulfate membrane.
8. The ion transport composite membrane according to claim 1, characterized in that: The ion conductivity of the ion transport composite membrane is 36-150 mS·cm -1 .
9. The ion transport composite membrane according to claim 1, characterized in that: The ion transport composite membrane is used to transport H + 、Na + , Li + , Cl - CF3SO3 - 、SO4 2- OH - At least one ion.
10. A solid-state battery, characterized in that: It comprises the ion transport composite membrane according to any one of claims 1 to 9.
11. Use of the ion transport composite membrane according to any one of claims 1 to 9 in electronic products.
12. The use according to claim 11, characterized in that: The electronic product is selected from a battery, a sensor or a supercapacitor.