Carbon-controlled smelting method for titanium-containing ultra-low carbon steel
Through the combined process of the converter, LF refining furnace and RH refining furnace, the argon and oxygen contents are controlled, solving the problem of carbon and oxygen imbalance in the smelting of ultra-low carbon steel, achieving stable control of carbon content and improving the yield rate.
Patent Information
- Application Number
- CN202410988049.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-10-01
AI Technical Summary
In the process of smelting ultra-low carbon steel, the imbalance of carbon and oxygen leads to poor decarburization effect, causing the finished product to become scrap or degraded, and it is difficult to stably control the carbon content within the range of 30×10-6 with existing technology.
The combined process of converter, LF refining furnace and RH refining furnace is used to ensure that the molten steel reaches the target carbon content in the RH vacuum furnace by controlling the argon gas flow, vacuum degree and oxygen content. Combined with the adjustment of alloying and slag materials, the carbon content is achieved. and oxygen balance.
The carbon content of ultra-low carbon steel is effectively controlled to ensure its stability within the range of 30×10-6, which avoids the degradation of finished products and improves the yield rate.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metallurgy, and in particular to a carbon-controlled smelting method for titanium-containing ultra-low carbon steel. Background Art
[0002] At present, ultra-low carbon steel has become the symbol of automobile steel plates, and the market is broad. In particular, vanadium-titanium automobile steel is popular in the market for its inherent high strength characteristics of titanium. However, it has strict requirements on steel quality and also puts forward higher requirements on the carbon content of steel, especially ultra-deep drawing steel, which requires the carbon content of steel to be controlled within 30×10 -6 Even lower, so it is critical to control carbon content during the process of smelting ultra-low carbon steel. Advanced steel mills at home and abroad have been able to stably control the carbon content at 30×10 -6 The carbon content of ultra-low carbon steel is within the range of 1% or even lower, while in the production of ultra-low carbon steel, about 1% cannot reach the target carbon content. There are many factors that affect the carbon effect in the actual operation process, mainly steel [C], [O] content, RH vacuum, circulation flow, decarburization time, etc. Summary of the invention
[0003] The purpose of the present invention is to provide a method for carbon controlled smelting of titanium-containing ultra-low carbon steel, so that the target carbon content is stably controlled at 30×10 -6 Within range.
[0004] The technical solution of the present invention: A method for carbon-controlled smelting of titanium-containing ultra-low carbon steel comprises the following steps: converter steelmaking - LF refining furnace - RH refining furnace and continuous casting; the smelting mass percentage range of the titanium-containing ultra-low carbon steel is: C: 0.03-0.04%, Si: ≤0.01%, 0.10%≤Mn≤0.20%, P: ≤0.010%, S: ≤0.006%, and the remainder is Fe and unavoidable impurities.
[0005] Preferably, the converter steelmaking process is specifically as follows: scrap steel is added to the furnace, the final temperature of the first converter furnace is 1660-1680°C, the continuous pulling temperature is 1650-1670°C, 1 / 3 of the steel is alloyed, low carbon ferromanganese 2.0-2.5Kg / t, small ash 1.76-2.94Kg / Kg / t, refined slag 1.17-1.76 Kg / t, the steel tapping process is to add alloy first, and finally add 200-300kg / furnace, the steel tapping takes 5-8 minutes, and the bottom blowing argon flow rate is 150-550Nm 3 / h, the diameter of the molten steel blown open is ≥200mm; the slag is blocked by a slide plate + a slag blocking plug, and the molten steel enters the argon blowing station to blow argon for 2-4 minutes, with an oxygen content of 600-800PPm.
[0006] Preferably, the chemical composition of the refined slag is in percentage by weight: Al: 50%, Al2O3: 33.1%, TiO2: 1.4%, MgO: 7.5%, SiO2: 2.0%, MnO: 0.049%, Fe2O3: 0.4%, and V2O5: 0.029%.
[0007] Preferably, the LF refining furnace process specifically includes: hoisting the ladle to the LF refining furnace for smelting treatment, connecting the ladle with argon after the ladle is seated, adjusting the argon to 500-1200NL / min for pre-purging argon, adopting a slightly positive pressure operation, opening the ladle to the heating position, adding low-carbon ferromanganese to slightly adjust the manganese content according to the manganese content of the chemical sample of the molten steel in the previous process, adding 500-700 kg / furnace of slag lime, and 100-200 kg / furnace of refined slag. After the addition is completed, adjust the argon to increase the stirring power; after the slag is completely melted, adjust the argon to 150-300NL / min. min, and start heating. After heating for 5-8 minutes, stop heating. After the argon strong stirring process is completed, the temperature of the molten steel is measured and sampled. After the LF furnace treatment is completed, 150-200kg / furnace of aluminum ladle slag modification agent is added. The furnace outlet temperature is 1650-1660℃ for the first furnace, and the temperature for the second and subsequent furnaces is 1610-1620℃. The manganese content in the molten steel is controlled according to the upper limit of the composition and the ladle is opened and hoisted to the RH treatment.
[0008] Preferably, the pressure of the micro-positive pressure operation is 10-12Mpa; After the argon strong stirring process, the chemical composition of the sample meets the mass percentage requirements, C: 0.03%, Si: ≤0.01%, 0.10%≤Mn≤0.20%, P: ≤0.010%, S:≤0.006%.
[0009] Preferably, the RH refining furnace process: RH furnace steam pressure ≧1.30Mpa, steam temperature ≧195℃, immersion tube aperture ≧450mm, RH vacuum degree reaches <67Pa, top gun flow rate 450-600Nm in the early 1-1.5 hours of RH smelting 3 / h baking tank operation; 2-4 furnaces of tank washing are carried out, the temperature of the washed tank steel after argon station is ≥1630℃, and the vacuum tank is clean without cold steel.
[0010] Preferably, the continuous casting process: RH titanium-containing ultra-low carbon steel RH smelting carbon controlled smelting, the vacuum pump operates in the pre-vacuum mode to evacuate, the cleanliness of the vacuum tank is observed by the camera in the vacuum tank before the molten steel is treated, and the RH is determined according to the LF chemical sample carbon and RH station oxygen content to determine whether the RH is subjected to top gun oxygen decarburization, the oxygen decarburization vacuum is blown in at 1.5-4.67KPa, the gun position is 4.5m, and the carbon and oxygen content of the molten steel are controlled to meet the process requirements; the RH circulating argon flow rate is adjusted to 120Nm 3 / h, full pump operation time ≤3min, vacuum degree in vacuum tank <67pa, vacuum pure decarburization time 6-12min; adjust circulating gas 90-100Nm 3 / h for RH oxygen determination and alloying, and the molten steel circulates for 3-6min. Temperature measurement and sampling are carried out. The tapping temperature of the first RH furnace is 1590-1600℃, and the continuous pulling temperature is 1615-1625℃. Aluminum determination and sampling are carried out. According to the alloy content of the RH chemical sample, the RH molten steel composition target alloying is adjusted, and the vacuum degree is maintained at ≤100Pa, the vacuum cycle is 35-39min, the pure degassing time is ≥8min, the standing time is 15-40min, and the carbon-free covering agent is 150-200Kg / furnace.
[0011] Preferably, the alloy composition RH molten steel composition mass percentage target is adjusted at one time, C: 0.0020%, Si: 0.02% 0.10%≤Mn≤0.20%, P: ≤0.010%, S: ≤0.006%, Ti: 0.060-0.070%, ALs: 0.030-0.045%, Cu: ≤0.05%, Ni: ≤0.05%, Cr: ≤0.05%, Nb: ≤0.005%, V: ≤0.003%, Cu+Gr+Ni: ≤0.07%, As: ≤0.010%, B: ≤0.0005%, N: ≤0.0030%.
[0012] The beneficial effects of the present invention are: The present invention controls the carbon content of ultra-low carbon steel in the RH vacuum furnace to meet the process requirements, and stably controls the carbon content of ultra-low carbon steel containing titanium to 30×10 -6 Even lower, it solves the problem that the decarburization degree cannot reach the process range due to the imbalance of carbon and oxygen in the converter, resulting in the carbon edge making the finished product become waste or downgraded, thus ensuring the yield rate. DETAILED DESCRIPTION Example 1
[0013] A carbon-controlled smelting method for titanium-containing ultra-low carbon steel, wherein the melting range of the titanium-containing ultra-low carbon steel into the furnace is: C: 0.03%, Si: 0.01%, Mn: 0.10%, P: 0.010%, S: 0.006%, and the remainder is Fe and unavoidable impurities.
[0014] Converter steelmaking: 18 tons of ordinary scrap steel, the first converter furnace end temperature is 1680℃, the continuous pulling temperature is 1670℃, 1 / 3 of the steel is alloyed, low carbon ferromanganese 2.5Kg / t, small ash 2.94Kg / Kg / t, refined slag 1.76 Kg / t, the steel tapping process is to add alloy first and then add 300kg / furnace, the steel tapping takes 8 minutes, and argon is blown from the bottom throughout the process to ensure that the molten steel is blown open with a diameter of 210mm. The slag is blocked by a slide plate + a slag plug, and the argon is blown in the argon blowing station for 4 minutes, with an oxygen content of 800PPm. The chemical composition of the refined slag is Al: 50%, Al2O3: 33.1%, TiO2: 1.4%, MgO: 7.5%, SiO2: 2.0%, MnO: 0.049%, Fe2O3: 0.4%, V2O5: 0.029%.
[0015] LF refining furnace: The ladle is hoisted to the LF refining furnace for smelting treatment. After the ladle is seated, the argon gas is connected and adjusted to 1200NL / min for pre-purging argon. The ladle is operated with a slight positive pressure. The ladle is opened to the heating position. According to the manganese content of the chemical sample of the molten steel in the previous process, low-carbon ferromanganese is added to slightly adjust the manganese. 700 kg / furnace of slag lime and 100-200kg / furnace of refined slag are added. After the addition, the argon gas is adjusted to increase the stirring power and improve the dynamic conditions. Observe that the slag is completely melted, adjust the argon gas to 300NL / min, select the appropriate voltage power and gear 4 (short arc or long arc + foam slag) for heating operation. The appropriate slag thickness is conducive to arc burial, improve thermal efficiency, and reduce nitrogen absorption by molten steel. Stop heating after heating for 8 minutes. Adjust the argon gas flow to improve the slag reaction ability and molten steel fluidity. Good fluidity is conducive to sulfur control reaction. After the argon strong stirring process is completed, the temperature of the molten steel is measured and sampled. The chemical composition of the samples meets the quality requirements, C: 0.03%, Si: 0.01%, %Mn: 0.20%, P: 0.010%, S0.006%. After the LF furnace treatment, 200kg / furnace of aluminum ladle slag modification agent is added. The furnace outlet temperature is 1660℃ for the first furnace and 1620℃ for the second and subsequent furnaces. The manganese in the molten steel is controlled according to the upper limit of the composition and the ladle is opened and hoisted to the RH treatment.
[0016] RH refining furnace: RH furnace steam pressure 1.50Mpa, steam temperature 200℃, immersion tube aperture 500mm, good circulation gas condition, RH vacuum degree below 67pa, RH smelting early 1.5 hours to carry out top gun flow 600Nm 3 / h baking tank operation. Carry out 4 furnace tank washing, the tank washing steel argon station requires the temperature after argon to be 1630℃. Ensure that the vacuum tank is clean and free of cold steel, Continuous casting: RH titanium-containing ultra-low carbon steel RH smelting and carbon controlled smelting. The vacuum pump for this process can be operated in the pre-vacuum (4a) mode to evacuate. Before the molten steel is treated, the cleanliness of the vacuum tank is observed through the camera in the vacuum tank. According to the carbon content of the LF chemical sample and the oxygen content of the RH station, it is determined whether the RH is subjected to top gun oxygen decarburization. The vacuum degree of oxygen decarburization is blown in at 4.67KPa, and the gun position is 4.5m. The carbon and oxygen content of the molten steel is controlled to meet the process requirements to avoid the imbalance of carbon and oxygen in the circulation of the RH station molten steel, which cannot remove the carbon within the process range within the effective time. Adjust the RH circulating argon flow rate to 120Nm 3 / h, full pump operation time 3min, vacuum degree in vacuum tank 67pa, vacuum pure decarburization time 12min. Adjust the circulating gas 100 Nm 3 / h for RH oxygen determination and alloying, the molten steel circulates for 6min for temperature measurement and sampling. The RH first furnace tapping temperature is 1600℃, the continuous pulling temperature is 1625℃, aluminum determination and sampling are carried out, and the RH molten steel composition target alloying is adjusted according to the alloy content of the RH chemical sample. The alloy composition compensation is adjusted once to achieve the process target, C: 0.0020%, Si: 0.02% Mn: 0.20%, P: 0.010%, S: 0.006%, Ti: 0.070%, ALs: 0.045%, Cu: 0.05%, Ni: 0.05%, Cr: 0.05%, Nb: 0.005%, V: 0.003%, Cu+Gr+Ni: 0.07%, As: 0.010%, B: 0.0005%, N: 0.0030%. Maintain vacuum degree of 100Pa, vacuum cycle of 39min, pure degassing time of 8min, standing time of 40min, carbon-free covering agent of 200Kg / furnace. Example 2
[0017] A carbon-controlled smelting method for titanium-containing ultra-low carbon steel, wherein the melting range of the titanium-containing ultra-low carbon steel into the furnace is: C: 0.04%, Si: 0.008%, Mn: 0.20%, P: 0.007%, S: 0.005%, and the remainder is Fe and unavoidable impurities.
[0018] Converter steelmaking: 3 tons of ordinary scrap steel, the first converter furnace end temperature is 1660℃, the continuous pulling temperature is 1650℃, 1 / 3 of the steel is alloyed, low carbon ferromanganese 2.0Kg / t, small ash 1.76Kg / Kg / t, refined slag 1.17 Kg / t, the steel tapping process is to add alloy first and then add 200kg / furnace, the steel tapping takes 5 minutes, and argon is blown from the bottom throughout the process to ensure that the molten steel is blown open with a diameter of 200mm. The slag is blocked by a slide plate + slag plug, and the argon is blown into the argon blowing station for 2 minutes, with an oxygen content of 600PPm. The chemical composition of the refined slag is Al: 50%, Al2O3: 33.1%, TiO2: 1.4%, MgO: 7.5%, SiO2: 2.0%, MnO: 0.049%, Fe2O3: 0.4%, V2O5: 0.029%.
[0019] LF refining furnace: The ladle is hoisted to the LF refining furnace for smelting treatment. After the ladle is seated, the argon is connected and adjusted to 500NL / min for pre-purging. The ladle is operated with a slight positive pressure. The ladle is opened to the heating position. According to the manganese content of the chemical sample of the molten steel in the previous process, low-carbon ferromanganese is added to slightly adjust the manganese. 500 kg / furnace of slag lime and 100 kg / furnace of refined slag are added. After the addition is completed, the argon is adjusted to increase the stirring power and improve the dynamic conditions. Observe that the slag is completely melted, adjust the argon to 150NL / min, select the appropriate voltage power and 4 gears (short arc or long arc + foam slag) for heating. The appropriate slag thickness is conducive to arc burial, improve thermal efficiency, and reduce nitrogen absorption by molten steel. Stop heating after heating for 5 minutes. Adjust the argon flow rate to improve the slag reaction ability and molten steel fluidity. Good fluidity is conducive to sulfur control reaction. After the argon strong stirring process is completed, the temperature of the molten steel is measured and sampled. The chemical composition of the samples meets the quality requirements, C: 0.03%, Si: 0.006%, Mn: 0.10%, P: 0.009%, S: 0.006%. After the LF furnace treatment, 150kg / furnace of aluminum ladle slag modification agent is added. The furnace outlet temperature is 1650℃ for the first furnace and 1610℃ for the second and subsequent furnaces. The manganese in the molten steel is controlled according to the upper limit of the composition and the ladle is opened and hoisted to the RH treatment.
[0020] RH refining furnace: RH furnace steam pressure 1.30Mpa, steam temperature 195℃, immersion tube aperture 450mm, circulating gas condition is good, RH vacuum degree reaches below 67pa, RH smelting in the early stage of 1 hour, top gun flow rate 450 Nm 3 / h baking tank operation. Carry out 2 furnace tank washing, the tank washing steel argon station requires the temperature after argon to be 1630℃. Ensure that the vacuum tank is clean and free of cold steel. Continuous casting: RH titanium-containing ultra-low carbon steel RH smelting and carbon controlled smelting. The vacuum pump for this process can be operated in the pre-vacuum (4a) mode to evacuate. Before the molten steel is treated, the cleanliness of the vacuum tank is observed through the camera in the vacuum tank. According to the carbon content of the LF chemical sample and the oxygen content of the RH station, it is determined whether the RH is subjected to top gun oxygen decarburization. The vacuum degree of oxygen decarburization is blown in at 2.67KPa, and the gun position is 4.5m. The carbon and oxygen content of the molten steel is controlled to meet the process requirements to avoid the imbalance of carbon and oxygen in the RH station molten steel circulation, which cannot remove the carbon within the process range within the effective time. Adjust the RH circulating argon flow rate to 120Nm 3 / h, full pump operation time 2.5min, vacuum degree in vacuum tank 65pa, vacuum pure decarburization time 8min. Adjust circulating gas 95 Nm 3 / h for RH oxygen determination and alloying, and the molten steel circulates for 5min. Temperature measurement and sampling are carried out. The tapping temperature of the first RH furnace is 1595℃, and the continuous pulling temperature is 1620℃. Aluminum determination and sampling are carried out. The target alloying of RH molten steel composition is adjusted according to the alloy content of the RH chemical sample. The alloy composition compensation is adjusted at one time to achieve the process target, C: 0.0020%, Si: 0.02%, Mn: 0.10%, P: 0.008%, S: 0.005%, Ti: 0.060%, ALs: 0.030%, Cu: 0.04%, Ni: 0.04%, Cr: 0.04%, Nb: 0.004%, V: 0.002%, Cu+Gr+Ni: 0.05%, As: 0.008%, B: 0.0003%, N: 0.0020%. Maintain vacuum degree at 90Pa, vacuum cycle at 35min, pure degassing time at 9min, standing time at 15min, carbon-free covering agent at 150Kg / furnace. Example 3
[0021] A carbon-controlled smelting method for titanium-containing ultra-low carbon steel, wherein the melting range of the titanium-containing ultra-low carbon steel into the furnace is: C: 0.05%, Si: 0.05%, Mn: 0.17%, P: 0.010%, S: 0.006%, and the remainder is Fe and unavoidable impurities.
[0022] Converter steelmaking: 10 tons of ordinary scrap steel, the first converter furnace end temperature is 1670℃, the continuous pulling temperature is 1660℃, 1 / 3 of the steel is alloyed, low carbon ferromanganese 2.3Kg / t, small ash 2.24Kg / Kg / t, refined slag 1.52 Kg / t, the steel tapping process is to add alloy first and then add 250kg / furnace, the steel tapping takes 6 minutes, and argon is blown from the bottom throughout the process to ensure that the molten steel is blown open with a diameter of 220mm. The slag is blocked by a slide plate + a slag plug, and the argon is blown into the argon blowing station for 3 minutes, with an oxygen content of 700PPm. The chemical composition of the refined slag is Al: 50%, Al2O3: 33.1%, TiO2: 1.4%, MgO: 7.5%, SiO2: 2.0%, MnO: 0.049%, Fe2O3: 0.4%, V2O5: 0.029%.
[0023] LF refining furnace: The ladle is hoisted to the LF refining furnace for smelting treatment. After the ladle is seated, the argon gas is connected and adjusted to 500-1200NL / min for pre-purging argon. The ladle is operated with a slight positive pressure. The ladle is opened to the heating position. According to the manganese content of the chemical sample of the molten steel in the previous process, low-carbon ferromanganese is added to slightly adjust the manganese. 500-700 kg / furnace of slag lime and 100-200 kg / furnace of refined slag are added. After the addition is completed, the argon gas is adjusted to increase the stirring power and improve the dynamic conditions. Observe that the slag is completely melted, adjust the argon gas to 150-300NL / min, select the appropriate voltage power and 4 gears (short arc or long arc + foam slag) for heating. The appropriate slag thickness is conducive to arc burial, improve thermal efficiency, and reduce nitrogen absorption by molten steel. Stop heating after heating for 5-8 minutes. Adjust the argon flow rate to improve the reaction ability of slag and the fluidity of molten steel. Good fluidity is conducive to sulfur control reaction. After the argon strong stirring process is completed, the temperature of the molten steel is measured and sampled. The chemical composition of the samples meets the quality requirements, C: 0.03%, Si: 0.007%, Mn: 0.13%, P: 0.008%, S: 0.005%. After the LF furnace treatment, 170kg / furnace of aluminum ladle slag modification agent is added. The furnace outlet temperature is 1655℃ for the first furnace, and 1615℃ for the second and subsequent furnaces. The manganese in the molten steel is controlled according to the upper limit of the composition and the ladle is opened and hoisted to the RH treatment.
[0024] RH refining furnace: RH furnace steam pressure 1.40Mpa, steam temperature 195℃, immersion tube hole 550mm, good circulation gas condition, RH vacuum degree below 67pa, RH smelting in the early 1.2 hours for top gun flow 550 Nm 3 / h baking tank operation. Carry out 3 furnace tank washing, the tank washing steel argon station requires the temperature after argon to be 1650℃. Ensure that the vacuum tank is clean and free of cold steel. Continuous casting: RH titanium-containing ultra-low carbon steel RH smelting and carbon controlled smelting. The vacuum pump for this process can be operated in the pre-vacuum (4a) mode to evacuate. Before the molten steel is treated, the cleanliness of the vacuum tank is observed through the camera in the vacuum tank. According to the carbon content of the LF chemical sample and the oxygen content of the RH station, it is determined whether the RH is subjected to top gun oxygen decarburization. The vacuum degree of oxygen decarburization is blown in at 1.5KPa, and the gun position is 4.5m. The carbon and oxygen content of the molten steel is controlled to meet the process requirements to avoid the imbalance of carbon and oxygen in the RH station molten steel circulation, which cannot remove the carbon within the process range within the effective time. Adjust the RH circulating argon flow rate to 120Nm 3 / h, full pump operation time 3min, vacuum degree in vacuum tank 67pa, vacuum pure decarburization time 6min. Adjust circulating gas 90 Nm 3 / h for RH oxygen determination and alloying, and the molten steel circulates for 3min. Temperature measurement and sampling are carried out. The tapping temperature of the first RH furnace is 1590℃, and the continuous pulling temperature is 1615℃. Aluminum determination and sampling are carried out. The target alloying of RH molten steel composition is adjusted according to the alloy content of the RH chemical sample. The alloy composition compensation is adjusted once to achieve the process target, C: 0.0020%, Si: 0.02%, Mn: 0.17%, P: 0.010%, S: 0.006%, Ti: 0.065%, ALs: 0.035%, Cu: 0.05%, Ni: 0.05%, Cr: 0.05%, Nb: 0.005%, V: 0.003%, Cu+Gr+Ni: 0.07%, As: 0.010%, B: 0.0005%, N: 0.0030%. Maintain vacuum degree of 100Pa, vacuum cycle of 37min, pure degassing time of 10min, standing time of 30min, carbon-free covering agent of 180Kg / furnace.
[0025] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.
Claims
1. A method for controlling carbon in titanium-containing ultra-low carbon steel, characterized in that: The process includes converter steelmaking - LF refining furnace - RH refining furnace and continuous casting; the melting mass percentage range of titanium-containing ultra-low carbon steel is: C: 0.03-0.04%, Si: ≤0.01%, 0.10%≤Mn≤0.20%, P: ≤0.010%, S:≤0.006%, and the rest is Fe and unavoidable impurities.
2. The method for carbon-controlled smelting of titanium-containing ultra-low carbon steel according to claim 1, characterized in that: The specific process of converter steelmaking is as follows: scrap steel is put into the furnace, the final temperature of the first converter furnace is 1660-1680℃, the continuous pulling temperature is 1650-1670℃, 1 / 3 of the steel is alloyed, low carbon ferromanganese 2.0-2.5Kg / t, small ash 1.76-2.94Kg / Kg / t, refined slag 1.17-1.76 Kg / t, the steel tapping process is to add alloy first, and finally add 200-300kg / furnace, steel tapping takes 5-8 minutes, and the bottom blowing argon flow rate is 150-550Nm 3 / h, the diameter of the molten steel blown open is ≥200mm; the slag is blocked by a slide plate + a slag blocking plug, and the molten steel enters the argon blowing station to blow argon for 2-4 minutes, with an oxygen content of 600-800PPm.
3. The carbon-controlled smelting method of titanium-containing ultra-low carbon steel according to claim 2, characterized in that: The chemical composition of the refined slag is in percentage by weight: Al: 50%, Al2O3: 33.1%, TiO2: 1.4%, MgO: 7.5%, SiO2: 2.0%, MnO: 0.049%, Fe2O3: 0.4%, V2O5: 0.029%.
4. The method for carbon controlled smelting of titanium-containing ultra-low carbon steel according to claim 1, characterized in that: The LF refining furnace process specifically includes: the ladle is hoisted to the LF refining furnace for smelting treatment, and after the ladle is seated, the argon is connected and adjusted to 500-1200NL / min for pre-purging of argon, and a slightly positive pressure operation is adopted. The ladle is opened to the heating position, and low-carbon ferromanganese is added to slightly adjust the manganese according to the manganese content of the chemical sample of the molten steel in the previous process, and 500-700 kg / furnace of slag lime and 100-200 kg / furnace of refined slag are added. After the addition is completed, the argon is adjusted to increase the stirring power; the slag is completely melted, and the argon is adjusted to 150-300NL / min for heating operation, and the heating is stopped after heating for 5-8 minutes; after the argon strong stirring process is completed, the temperature of the molten steel is measured and sampled; after the LF furnace treatment is completed, 150-200kg / furnace of aluminum ladle slag modification agent is added, and the outlet temperature is 1650-1660℃ for the first furnace, and the temperature after the second furnace is 1610-1620℃. The manganese in the molten steel is controlled according to the upper limit of the composition, and the ladle is opened and hoisted to the RH treatment.
5. A method for carbon-controlled smelting of titanium-containing ultra-low carbon steel according to claim 4, characterized in that: The pressure of the micro-positive pressure operation is 10-12Mpa; After the argon strong stirring process, the chemical composition of the sample meets the mass percentage requirements, C: 0.03%, Si: ≤0.01%, 0.10%≤Mn≤0.20%, P: ≤0.010%, S:≤0.006%.
6. The method for carbon-controlled smelting of titanium-containing ultra-low carbon steel according to claim 1, characterized in that: RH refining furnace process: RH furnace steam pressure ≧1.30Mpa, steam temperature ≧195℃, immersion tube aperture ≧450mm, RH vacuum degree reaches <67pa, top gun flow rate 450-600 Nm in the early 1-1.5 hours of RH smelting 3 / h baking tank operation; 2-4 furnaces of tank washing are carried out, the temperature of the washed tank steel after argon station is ≥1630℃, and the vacuum tank is clean without cold steel.
7. The method for carbon controlled smelting of titanium-containing ultra-low carbon steel according to claim 1, characterized in that: Continuous casting process: RH titanium-containing ultra-low carbon steel RH smelting and carbon controlled smelting are carried out. The vacuum pump operates in the pre-vacuum mode to evacuate the vacuum tank. The cleanliness of the vacuum tank is observed through the camera in the vacuum tank before the molten steel is processed. According to the carbon content of the LF chemical sample and the oxygen content of the RH station, it is determined whether the RH is subjected to top gun oxygen decarburization. The vacuum degree of oxygen decarburization is 1.5-4.67KPa, and the gun position is 4.5m. The carbon and oxygen content of the molten steel are controlled to meet the process requirements; the RH circulating argon flow rate is adjusted to 120Nm 3 / h, full pump operation time ≤3min, vacuum degree in vacuum tank <67pa, vacuum pure decarburization time 6-12min; adjust circulating gas 90-100Nm 3 / h for RH oxygen determination and alloying, and the molten steel circulates for 3-6min. Temperature measurement and sampling are carried out. The tapping temperature of the first RH furnace is 1590-1600℃, and the continuous pulling temperature is 1615-1625℃. Aluminum determination and sampling are carried out. According to the alloy content of the RH chemical sample, the RH molten steel composition target alloying is adjusted, and the vacuum degree is maintained at ≤100Pa, the vacuum cycle is 35-39min, the pure degassing time is ≥8min, the standing time is 15-40min, and the carbon-free covering agent is 150-200Kg / furnace.
8. The method for carbon-controlled smelting of titanium-containing ultra-low carbon steel according to claim 7, characterized in that: The target mass percentage of alloy composition RH molten steel is adjusted at one time: C: 0.0020%, Si: 0.02% 0.10%≤Mn≤0.20%, P: ≤0.010%, S: ≤0.006%, Ti: 0.060-0.070%, ALs: 0.030-0.045%, Cu: ≤0.05%, Ni: ≤0.05%, Cr: ≤0.05%, Nb: ≤0.005%, V: ≤0.003%, Cu+Gr+Ni: ≤0.07%, As: ≤0.010%, B: ≤0.0005%, N: ≤0.0030%.