Vanadium titano-magnetite smelting process capable of improving titanium recovery rate

The vanadium-titanium magnetite is smelted through pre-oxidation treatment and direct reduction process, and clean energy is used for element separation and enrichment, which solves the problems of low titanium resource utilization and environmental pollution, and achieves efficient titanium recovery and element recovery.

CN118726767APending Publication Date: 2024-10-01SICHUAN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410584462.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-11
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The utilization rate of titanium resources in the existing vanadium-titanium magnetite smelting process is low. The titanium recovery rate under traditional processes is only 10% to 15%. The symbiosis of iron and titanium results in poor beneficiation and separation effects, resulting in a large loss of titanium resources and environmental pollution.

Method used

After pre-oxidation treatment, the vanadium-titanium magnetite raw material is smelted through a direct reduction process (such as direct reduction-electric furnace method or direct reduction-grinding method), using clean energy such as H2, CO or natural gas as the reducing agent to achieve elemental reduction. separation and enrichment.

Benefits of technology

It improves the titanium recovery rate, reduces environmental pollution, reduces titanium loss, simplifies the process flow, and increases the element recovery rate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention discloses a vanadium titano-magnetite smelting process capable of improving titanium recovery rate, which belongs to the technical field of metallurgy, and comprises the following steps of: firstly carrying out pre-oxidation treatment on a vanadium titano-magnetite raw material to obtain a pre-oxidized material, and then smelting the pre-oxidized material by adopting a direct reduction process to realize separation and enrichment of elements. The process is simple, clean energy is adopted as a reducing agent, environmental pollution is greatly reduced, titanium loss is reduced, and the recovery rate of titanium resources is greatly increased.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metallurgy, and in particular relates to a vanadium-titanium magnetite smelting process for improving titanium recovery rate. Background Art

[0002] Vanadium-titanium magnetite is a low-grade polymetallic mineral mainly containing iron, titanium and vanadium, accompanied by other metal elements such as chromium, cobalt, nickel, copper and gallium, and has high utilization value. China has abundant vanadium-titanium magnetite resources, but the comprehensive utilization rate is low, especially for titanium, whose recovery rate is only 10% to 15% under traditional processes.

[0003] The traditional "ore dressing-smelting" process of vanadium-titanium magnetite is to first enrich the raw ore through ore dressing to obtain iron concentrate and titanium concentrate, and then use the iron concentrate and titanium concentrate as raw materials for smelting. In the ore dressing process, there are a large number of valuable metal elements such as titanium, vanadium, chromium, cobalt, nickel, scandium, etc. in the waste generated, among which about 33% of the titanium in the raw ore enters the titanium ore and tailings without being effectively utilized. In addition, due to the close symbiosis of titanium and iron, the physical ore dressing method can only achieve the separation and enrichment of iron concentrate (titanium magnetite) and titanium concentrate (ilmenite), so that the iron in the titanium concentrate and the titanium in the iron concentrate are not efficiently utilized. About 25% of the iron in the raw ore enters the titanium dioxide production process with the titanium concentrate, and is finally produced in the form of by-products such as ferrous sulfate heptahydrate or ferrous chloride; about 54% of the titanium follows the iron concentrate into the blast furnace process to form titanium-containing blast furnace slag and is discarded.

[0004] At present, the smelting methods of iron ore concentrate mainly include blast furnace method, direct reduction method and smelting reduction method. The blast furnace process for treating vanadium-titanium magnetite iron ore concentrate is mature and is the current mainstream technical method, but it faces the dual pressures of coke resource shortage and carbon emission reduction. In order to reduce carbon emissions, researchers have proposed and studied non-blast furnace smelting technology that uses other reducing agents to replace coke. In the non-blast furnace method, it is divided into direct reduction and smelting reduction technology according to whether the reduction is molten. The smelting process is reduced in a molten state, and the iron slag is completely separated to obtain molten iron to enter the converter for steelmaking. This process not only saves the use of coke, but also eliminates the sintering section to reduce pollution. It has the characteristics of short process flow, simple operation, stable production, and low raw material requirements. However, several mature smelting processes currently still have problems such as incomplete coke removal and high production energy consumption.

[0005] In summary, the existing smelting of vanadium-titanium magnetite has the following problems: (1) The "selection-smelting" process of first selecting the ore and then smelting them separately causes a 30% loss of titanium resources during the selection process; (2) Due to the close coexistence of iron and titanium, the selection and separation effect is poor, and about 50% of the titanium follows the iron concentrate through the blast furnace to form blast furnace slag and is abandoned. Summary of the invention

[0006] The purpose of the embodiment of the present invention is to provide a vanadium-titanium magnetite smelting process for improving the titanium recovery rate, which has a simple process, convenient operation and high recovery rate of each element.

[0007] The embodiment of the present invention is achieved as follows:

[0008] The embodiment of the present invention provides a vanadium-titanium magnetite smelting process for improving titanium recovery, comprising the following steps:

[0009] S1: pre-oxidizing the vanadium-titanium magnetite raw material to obtain a pre-oxidized material;

[0010] S2: The pre-oxidized materials are smelted by direct reduction process to achieve element separation and enrichment.

[0011] Optionally, the vanadium-titanium magnetite raw material is vanadium-titanium magnetite ore or coarse ore obtained by pre-selection and discarding tailings of low-grade vanadium-titanium magnetite.

[0012] Optionally, in step S1, the pre-oxidation temperature is 700-1000°C.

[0013] Optionally, the pre-oxidation temperature is 800°C or 900°C.

[0014] Optionally, in step S2, the direct reduction process is a direct reduction-electric furnace method and / or a direct reduction-grinding method.

[0015] Optionally, in step S2, the temperature of the direct reduction process is 1000-1300°C, and the reducing agent includes at least one of H2, CO, natural gas, hydrogen-rich coal gas and coal.

[0016] The beneficial effects of the present invention are:

[0017] The vanadium-titanium magnetite smelting process for improving titanium recovery rate provided in the embodiment of the present invention is simple in process, uses clean energy as a reducing agent, greatly reduces environmental pollution, reduces titanium loss, and greatly improves the recovery rate of titanium resources. DETAILED DESCRIPTION

[0018] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments.

[0019] Therefore, the following detailed description of the embodiments of the present invention is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0020] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features of the embodiments may be combined with each other.

[0021] Example 1

[0022] Embodiment 1 of the present invention provides a vanadium-titanium magnetite smelting process for improving titanium recovery rate, comprising the following steps:

[0023] S1: pre-oxidizing the vanadium-titanium magnetite raw material to obtain a pre-oxidized material.

[0024] The vanadium-titanium magnetite raw material can be the original vanadium-titanium magnetite ore, or the coarse ore obtained by pre-selection and discarding of low-grade vanadium-titanium magnetite.

[0025] In this embodiment, the contents of various elements in the selected vanadium-titanium magnetite raw material are shown in Table 1.

[0026] Table 1

[0027]

[0028] In this embodiment, the pre-oxidation process is to put the vanadium-titanium magnetite into a crucible, place it in a muffle furnace, heat it to 900°C at a rate of 10°C / min in an air atmosphere and keep it warm for 1 hour, then cool the material to room temperature with the furnace, and take out the pre-oxidized material for standby use. Of course, the pre-oxidation temperature can also be set to 700°C, 750°C, 800°C, 950°C or 1000°C, etc.

[0029] S2: The pre-oxidized materials are smelted by direct reduction process to achieve element separation and enrichment.

[0030] The direct reduction process can adopt the direct reduction-electric furnace method, the direct reduction-grinding method, or a combination of the direct reduction-electric furnace method and the direct reduction-grinding method for smelting.

[0031] In this embodiment, carbon is used as a reducing agent, and then the reaction is carried out at 1140° C. for 3 hours. When C / Fe=1.2, the metallization rate of iron is 97.8%.

[0032] In this step, during ball milling, the ball-to-material ratio is 12:1, the slurry ratio is 4:1, and the ball milling is required to be performed until D50 is 4.33 μm, and then magnetic separation is performed at 250 mT to obtain non-magnetic phase elements Ti and V, and magnetic phase element Fe, wherein the recovery rate of Ti is 87.07%, the recovery rate of V is 85.53%, and the recovery rate of Fe is 93.41%.

[0033] Example 2

[0034] Embodiment 2 of the present invention provides a vanadium-titanium magnetite smelting process for improving titanium recovery rate, comprising the following steps:

[0035] S1: pre-oxidizing the vanadium-titanium magnetite raw material to obtain a pre-oxidized material.

[0036] The vanadium-titanium magnetite raw material can be the original vanadium-titanium magnetite ore, or the coarse ore obtained by pre-selection and discarding of low-grade vanadium-titanium magnetite.

[0037] In this embodiment, the contents of various elements in the selected vanadium-titanium magnetite raw material are shown in Table 2.

[0038] Table 2

[0039]

[0040] In this embodiment, the pre-oxidation process is to put the vanadium-titanium magnetite into a crucible, place it in a muffle furnace, heat it to 800°C at a rate of 10°C / min in an air atmosphere and keep it warm for 2 hours, then cool the material to room temperature with the furnace, and take out the pre-oxidized material for standby use. Of course, the pre-oxidation temperature can also be set to 700°C, 750°C, 900°C, 950°C or 1000°C, etc.

[0041] S2: The pre-oxidized materials are smelted by direct reduction process to achieve element separation and enrichment.

[0042] The direct reduction process can adopt the direct reduction-electric furnace method, the direct reduction-grinding method, or a combination of the direct reduction-electric furnace method and the direct reduction-grinding method for smelting.

[0043] In this embodiment, H2 is used as a reducing agent, and then the reaction is carried out at 1120°C for 35 minutes. When the H2 concentration is 100% and the flow rate is 500 ml / min, the metallization rate of iron is 97.8%.

[0044] In this step, during ball milling, the ball-to-material ratio is 10:1, the slurry ratio is 4:1, and the ball milling is required to be performed until D50 is 5.28 μm, and then magnetic separation is performed at 250 mT to obtain non-magnetic phase elements Ti and V, and magnetic phase element Fe, wherein the recovery rate of Ti is 58.44%, the recovery rate of V is 59.30%, and the recovery rate of Fe is 91.00%.

[0045] Example 3

[0046] Embodiment 3 of the present invention provides a vanadium-titanium magnetite smelting process for improving titanium recovery rate, comprising the following steps:

[0047] S1: pre-oxidizing the vanadium-titanium magnetite raw material to obtain a pre-oxidized material.

[0048] The vanadium-titanium magnetite raw material can be the original vanadium-titanium magnetite ore, or the coarse ore obtained by pre-selection and discarding of low-grade vanadium-titanium magnetite.

[0049] In this embodiment, the contents of various elements in the selected vanadium-titanium magnetite raw material are shown in Table 3.

[0050] Table 3

[0051]

[0052] In this embodiment, the pre-oxidation process is to put the vanadium-titanium magnetite into a crucible, place it in a muffle furnace, heat it to 800°C at a rate of 10°C / min in an air atmosphere and keep it warm for 2 hours, then cool the material to room temperature with the furnace, and take out the pre-oxidized material for standby use. Of course, the pre-oxidation temperature can also be set to 700°C, 750°C, 900°C, 950°C or 1000°C, etc.

[0053] S2: The pre-oxidized materials are smelted by direct reduction process to achieve element separation and enrichment.

[0054] The direct reduction process can adopt the direct reduction-electric furnace method, the direct reduction-grinding method, or a combination of the direct reduction-electric furnace method and the direct reduction-grinding method for smelting.

[0055] In this embodiment, CO is used as a reducing agent, and then the reaction is carried out at 1110° C. for 2 hours. When the CO concentration is 100% and the flow rate is 500 ml / min, the metallization rate of iron is 85.5%.

[0056] In this step, during ball milling, the ball-to-material ratio is 10:1, the slurry ratio is 4:1, and the ball milling is required to be performed until D50 is 4.97 μm, and then magnetic separation is performed at 250 mT to obtain non-magnetic phase elements Ti and V, and magnetic phase element Fe, wherein the recovery rate of Ti is 64.6%, the recovery rate of V is 15.59%, and the recovery rate of Fe is 93.2%.

[0057] It should be noted that the calculation formula of the metallization rate in this application is as follows:

[0058]

[0059] Wherein: η-iron metallization rate, %; MFe-metallic iron content in the reduced material, %; TFe-total iron content in the reduced material, %.

[0060] In the magnetic separation step, the recovery rate of each element is calculated as follows:

[0061]

[0062] In the formula: R1-recovery rate of corresponding elements, %; w1-content of corresponding elements in magnetic phase iron or non-magnetic phase titanium, %; m1-mass of magnetic phase (iron) or non-magnetic phase (titanium), g; w-content of corresponding elements in reduced sample, %; m-mass of reduced sample used for magnetic separation, g.

[0063] The metallic iron content in the above formula is determined by potassium dichromate titration (national standard GB / T 38812.2-2020). The total iron and titanium contents are determined by X-ray fluorescence spectrometer (XRF, XRF-180, Shimadzu, Japan) and alkali fusion-inductively coupled plasma atomic emission spectrometry (ICP-AES, spectro ARCOS ICP, Germany).

[0064] The present invention is not limited to the above-mentioned optional implementation modes. Anyone can derive other various forms of products under the inspiration of the present invention. However, no matter what changes are made in the shape or structure, all technical solutions that fall within the scope defined by the claims of the present invention fall within the protection scope of the present invention.

Claims

1. A vanadium-titanium magnetite smelting process for improving titanium recovery, characterized in that: The following steps are involved: S1: pre-oxidizing the vanadium-titanium magnetite raw material to obtain a pre-oxidized material; S2: The pre-oxidized materials are smelted by direct reduction process to achieve element separation and enrichment.

2. The vanadium-titanium magnetite smelting process for improving titanium recovery according to claim 1, characterized in that: The raw material of vanadium-titanium magnetite is the original vanadium-titanium magnetite ore or the coarse ore obtained by pre-selection and discarding the tailings of low-grade vanadium-titanium magnetite.

3. The vanadium-titanium magnetite smelting process for improving titanium recovery rate according to claim 1, characterized in that: In step S1, the pre-oxidation temperature is 700-1000°C.

4. The vanadium-titanium magnetite smelting process for improving titanium recovery rate according to claim 3, characterized in that: The pre-oxidation temperature is 800°C or 900°C.

5. The vanadium-titanium magnetite smelting process for improving titanium recovery rate according to claim 1, characterized in that: In step S2, the direct reduction process is a direct reduction-electric furnace method and / or a direct reduction-grinding method.

6. The vanadium-titanium magnetite smelting process for improving titanium recovery rate according to claim 1, characterized in that: In step S2, the temperature of the direct reduction process is 1000-1300°C, and the reducing agent includes at least one of H2, CO, natural gas, hydrogen-rich coal gas and coal.