Vacuum consumable melting method for improving titanium ingot yield

By accurately controlling vacuum arc melting parameters and multiple melting processes, combined with non-uniform speed welding and ultrasonic cleaning, the problems of low yield and poor composition uniformity in vacuum consumable smelting of titanium alloys are solved, and the production of high-quality titanium ingots is achieved.

CN118726778APending Publication Date: 2024-10-01ZHEJIANG SHENJI TITANIUM IND

Patent Information

Application Number
CN202411038087.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

In the existing titanium alloy vacuum consumable smelting technology, the yield of titanium ingots is low, the composition uniformity is poor, the surface quality is poor, and the production process is complex and the cost is high.

Method used

By accurately controlling the melting voltage, melting current, arc stabilizing current and cooling water parameters of vacuum arc melting, using secondary or tertiary melting processes, combined with non-uniform speed welding and ultrasonic cleaning, the uniformity and high quality of titanium alloy consumable electrodes are ensured .

Benefits of technology

It significantly improves the yield and composition uniformity of titanium ingots, reduces impurity content and preparation costs, and is suitable for the industrial production of large-diameter titanium ingots.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

The invention discloses a vacuum consumable smelting method for improving the titanium ingot yield. The vacuum consumable smelting method comprises the following steps: preparing a titanium alloy consumable electrode; the smelting current is 13-17 kA, the smelting voltage is 31-34 V, and the arc stabilizing current is 10-16 A; the smelting current ranges from 23 KA to 26 KA, the smelting voltage ranges from 31.5 V to 33.5 V, the arc stabilizing current ranges from 10 A to 16 A, and the total loss rate of secondary smelting is smaller than or equal to 4%; the smelting current ranges from 25 KA to 27 KA, the smelting voltage ranges from 32 V to 34 V, the arc stabilizing current ranges from 10 A to 16 A, and the total loss rate of three-time smelting is smaller than or equal to 5%; in the feeding and arc stopping stages, the smelting current, the arc voltage and the arc stabilizing current are gradually reduced, and a titanium ingot is obtained; optionally, the titanium ingot is subjected to surface machining treatment. By accurately controlling the smelting current, voltage, arc stabilizing current and the like of each stage, the yield and ingot casting quality of titanium ingots prepared by the vacuum consumable smelting method are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of titanium alloy smelting, and in particular relates to a vacuum consumable smelting method for improving the yield rate of titanium ingots. Background Art

[0002] At present, the smelting methods of titanium alloys mainly include five methods: vacuum consumable arc furnace smelting (VAR), non-consumable vacuum arc furnace smelting (NC), cold hearth smelting (CHM), cold crucible smelting (CCM), and electroslag smelting (ESR). In recent years, the VAR method has made significant progress and has become the mainstream technology for the preparation of titanium alloy ingots. It has the advantages of low power consumption, fast melting speed and good quality reproducibility. The smelted ingots have good crystal structure and uniform chemical composition. Modern VAR furnaces are characterized by large-scale, automation and precision control, and can produce large ingots with a diameter of 1.5 meters and a weight of 32 tons. At the same time, the full coaxial power input technology and advanced electronic control system realize constant speed smelting, further improving the quality of the ingots.

[0003] Although VAR technology occupies an important position in titanium alloy production, it still faces some technical challenges. The complexity of electrode preparation, the uniformity of raw materials, and the segregation and inclusion problems during the smelting process are the main difficulties in the current technological development. In addition, how to further improve the yield rate, composition uniformity and surface quality of ingots by adjusting process parameters is also a key issue that VAR technology needs to solve.

[0004] Invention CN107502784B discloses a method for producing TC4 titanium alloy round ingots / flat ingots, which uses a plasma welder to weld electrode blocks into long electrodes, and uses a VAR furnace to melt them into primary ingots, and then uses a 7-gun cold cathode EB furnace to melt the primary ingot melted in the VAR furnace for a second time, so as to obtain ultra-large specifications and high-quality TC4 titanium alloy round ingots / flat ingots. Although the invention uses a 7-gun cold cathode EB furnace to melt the primary ingot melted by VAR for a second time to obtain a high-quality TC4 titanium alloy ingot, the use of multiple equipment for melting increases the production steps and costs of TC4 titanium alloy, and the yield rate is not significantly improved.

[0005] Invention CN117535539A discloses a smelting method for improving the production efficiency and yield rate of titanium alloy ingots, including the following steps: 1) preparing electrodes; 2) primary smelting; 3) primary ingot processing; 4) secondary smelting or tertiary smelting; 5) processing, sampling and analysis; the invention strictly controls the relevant parameters of each step, especially the parameters of the final arc closure of the primary smelting by adjusting the parameters, specifically requiring the smelting current to be reduced by 1KA per minute, the voltage to be reduced by 1V, and the arc stabilization current to be reduced by 1A, four times in total, until the smelting is completed, and the arc stabilization adopts AC mode when closure, and the stirring cycle is 15s to 30s. However, the smelting equipment size and process parameter control of the invention are still insufficient, the production size of titanium ingot products is limited, and the yield rate is still insufficient.

[0006] Therefore, how to provide a vacuum consumable melting method for TC4 titanium ingots with uniform microstructure, few segregation and inclusion defects, optional ingot size, good quality and high yield rate by accurately controlling the process parameters such as melting voltage, melting current, arc stabilization current, cooling water, etc. in each melting stage in vacuum arc remelting is an urgent problem to be solved by technical personnel in this field. Summary of the invention

[0007] In view of the defects existing in the above-mentioned prior art, the present invention provides a titanium alloy vacuum consumable smelting method for improving the yield rate of titanium ingots. The titanium ingots produced by this method have uniform microstructure, few segregation and inclusion defects, more size selectivity, good ingot quality and high yield rate.

[0008] In a first aspect, the present invention provides a titanium alloy vacuum consumable melting method for improving the yield of titanium ingots, which uses a vacuum consumable arc furnace to melt a titanium alloy consumable electrode, comprising: (1) Preparation of titanium alloy consumable electrodes; (2) First smelting: vacuum degree in the furnace ≤1Pa, gas leakage rate ≤0.7Pa / min, smelting current 13-17kA, smelting voltage 31-34V, arc stabilization current 10-16A, and cooling after smelting to obtain a primary ingot; (3) Second smelting: vacuum degree in the furnace ≤ 0.8Pa, gas leakage rate ≤ 0.7Pa / min, smelting current 23-26KA, smelting voltage 31.5-33.5V, arc stabilization current 10-16A, cooling after smelting to obtain secondary ingots, total loss rate of secondary smelting ≤ 4%; (4) Entering the stage of arc supplement and arc closure, the melting current, arc voltage and arc stabilization current are gradually reduced to obtain a titanium ingot.

[0009] Optionally, the titanium ingot is subjected to surface processing.

[0010] Preferably, after the second smelting, a third smelting is also included, the vacuum degree in the furnace is ≤0.5Pa, the leakage rate is ≤0.6Pa / min, the smelting current is 25-26KA, the smelting voltage is 32-34V, the arc stabilization current is 10-16A, and the smelting is followed by cooling to obtain three ingots; the total loss rate of the three smeltings is ≤5%.

[0011] Preferably, in each smelting, before the stable smelting stage, an arc starting stage from 0 to t2+tx is also included: (1) When 0<t≤t1, the arc is struck with an arc starting current of 2kA~5kA, where t1 is 2~5min; (2) When t1<t≤t2, increase the current to the pre-melting current at a rate of 0.5~3kA / min, where t2 is 15~30min and the pre-melting current is 110~120% of the melting current; (3) When t2<t≤t2+tx, the pre-melting current is reduced to the melting current, and the arc starting stage enters the stable melting stage, and tx is 1 to 15 minutes.

[0012] The melting current is one of the parameters that has a significant impact on the melting process and product quality in the vacuum consumable melting method. In order to avoid affecting the quality of the ingot, a reasonable melting current must be selected. First, a small current is used to start the arc to quickly establish a molten pool. After the metal molten pool is formed, the melting rate is increased to raise the current to 110% to 120% of the melting current in the stable melting stage, and after maintaining it for a certain period of time, it is reduced to the normal melting current for stable melting. The normal melting current is based on the minimum current from the molten pool to the edge. Secondly, the current should not be too large during the melting process, because the larger the current, the deeper the molten pool. A too deep molten pool is not conducive to the floating removal of non-metallic inclusions, and the melting current is too large, exceeding the tolerance threshold of the consumable electrode, and the electrode is easy to fall off, resulting in an accident. If the melting current is too small, the molten pool is poor to the edge, and the subsequent peeling loss rate is too large, which reduces the yield rate. Therefore, the melting current is preferably increased slowly during the melting process.

[0013] Melting voltage is another main parameter in vacuum consumable arc melting. The arc length is controlled by adjusting the voltage to further stabilize the melting speed. The arc cannot be too long, otherwise the arc heat is not concentrated, the heat loss of the molten pool is large, and it is easy to produce side arcs and damage the crystallizer. Short arc operation is adopted in production, and the voltage can be controlled within a certain range through intelligent control or manual operation. On the other hand, if the melting voltage is too high, the molten pool will be poor to the edge and the yield rate will be reduced. If the melting voltage is too low, short circuit is easy to occur due to the close distance between the auxiliary electrode and the consumable electrode.

[0014] The arc stabilization current is a key factor in ensuring arc stability, and has a direct impact on the melting speed, molten pool morphology, and the final quality of the ingot. If the arc stabilization current is too small, stirring will not be possible, the molten pool will not reach the edge, and the yield rate will be low. If the arc stabilization current is too large, the consumable electrode will easily shake, posing a safety hazard.

[0015] Preferably, step (1) comprises: 1.1. Batching and mixing: Batching and mixing the raw material components of titanium alloy according to the proportion; 1.2. Electrode pressing and welding: Press a single electrode block, and use a non-tungsten electrode argon shielded plasma welding box to weld the pressed electrode block into a titanium alloy consumable electrode. The weight of the titanium alloy consumable electrode is 1000-6000kg, and the diameter d0 is 40cm≤d0≤73cm; The obtained titanium alloy consumable electrode comprises the following components by weight percentage: Al 5.5~6.5% V 3.5~4.5% Fe 0.1~0.2% The total amount of C, H, O and N is ≤0.3%, preferably ≤0.2%, more preferably ≤0.15%, and the balance is titanium.

[0016] The batching and mixing of materials is preferably carried out by an automatic mixing system according to the various raw material components to perform automatic electronic weighing batching and mixing to obtain a uniformly mixed raw material composition for the electrode block to be pressed. If necessary, the raw materials, such as sponge titanium, are pre-dried.

[0017] The welding is vacuum plasma welding. Before welding, argon gas is filled in the vacuum plasma welding box. The flow rate of argon gas is 4L / min~7L / min, and the pressure of argon gas is maintained at 20000~30000Pa.

[0018] The welding adopts a non-uniform speed welding method. In the range of 1 / 4 to 1 / 3 of the front section of the welding line, a welding speed of 50 to 60 mm / min is adopted, a welding current of 400A to 700A, and a voltage of 50V to 58V is adopted; in the range of 1 / 3 to 1 / 2 of the middle section, a welding speed of 80 to 90 mm / min is adopted, a welding current of 400A to 700A, and a voltage of 55V to 65V is adopted; in the range of 1 / 4 to 1 / 3 of the rear section, a welding speed of 100 to 120 mm / min is adopted, a welding current of 500A to 800A, and a voltage of 60V to 70V is adopted. The cooling time after welding is 25 to 60 minutes. After cooling, the weld presents a silvery white metallic luster, and the weld pool is full, the upper and lower parts are in a molten adhesion state, and the welding quality is good. The welding method of the present invention ensures welding quality while taking into account welding efficiency.

[0019] Among them, in step 1.1, the raw material components are mixed using a single block mixing method, and then pressed into a single electrode block, and then 25-35 electrode blocks are welded into a titanium alloy consumable electrode.

[0020] Preferably, a non-tungsten electrode argon shielded plasma welding box is used to butt-weld an auxiliary electrode made of the same grade of titanium alloy with the titanium alloy consumable electrode made in step (1), and the auxiliary electrode is installed on the pneumatic head of the electrode rod. The auxiliary electrode moves up and down to drive the titanium alloy consumable electrode to move up and down, and the diameter df of the auxiliary electrode satisfies: 0.25d0≤df≤0.75d0. Preferably, the outer chamfer of the lower end of the auxiliary electrode satisfies (4mm~6mm)×(45°±1°). After the consumable electrode and the auxiliary electrode are welded, the weld nodules are cleaned after cooling for 30~60 minutes, and the furnace is sealed and evacuated after cleaning. The butt welding conditions can refer to the electrode block welding conditions and be slightly adjusted according to factors such as the size of the welding object. The above-mentioned size and chamfer setting of the auxiliary electrode are conducive to the overflow of the weld molten pool to the outer edge of the lower end surface of the auxiliary electrode during the welding process, further increasing the contact area of ​​the weld and improving the stability of the weld quality.

[0021] Preferably, in step (2), the titanium alloy consumable electrode obtained in step (1) is first smelted in a first crucible, and the diameter D1 of the first crucible is 55 to 78 cm; the surface of the first ingot is cleaned; In step (3), the treated primary ingot is melted for a second time in a second crucible, wherein the diameter D2 of the second crucible is 65 to 85 cm; the secondary ingot is flattened, peeled and polished; After step (3), the treated secondary ingot is smelted for the third time in a third crucible, wherein the diameter D3 of the third crucible is 70-95 cm; and the tertiary ingot is subjected to skinning and polishing treatment.

[0022] Preferably, the primary ingot is strictly cleaned after the first smelting, preferably by ultrasonic-assisted stainless steel brushing, to remove impurities such as oxides, chlorides, carbides on the surface of the primary ingot, to avoid the defect of the electric arc furnace that solid impurities are difficult to remove, and to prevent the subsequent smelting resulting in multiple ingots with many pores, excessive amount of peeling material, and other losses.

[0023] The titanium alloy vacuum consumable smelting method of the present invention can be used to manufacture titanium ingots with a large diameter range, with good ingot composition and structural uniformity, high titanium ingot yield rate, low impurity content, and greatly reduced titanium ingot preparation cost.

[0024] Preferably, in the first smelting and the second smelting, the cooling water flow rate is controlled at 1100-1300 L / min, the water inlet temperature is 20°C-30°C, and the cooling time after smelting is not less than 5 hours; During the third smelting, the cooling water flow rate is controlled at 1300-1500 L / min, the inlet water temperature is 20°C-30°C, and the cooling time after smelting is not less than 7 hours.

[0025] Preferably, when the weight of the remaining unmelted electrode accounts for 2-6% of the initial weight, the process proceeds to step (4) of feeding and arc closure, which includes the following steps: 4.1 Primary feeding stage: melting current C1 is 20-25kA, arc voltage V1 is 30V-32V, arc stabilization current I1 is 8-14A, maintain for 1-2min; 4.2 Secondary feeding stage: melting current C2 is (60%~90%)×C1, arc voltage V2 is (80%~95%)×V1, arc stabilization current is 7~9A, maintain for 1~2min; 4.3 Three-level shrinkage feeding stage: the melting current C3 is maintained at (30%~70%)×C2 for 1~2 minutes, and then maintained at 2~5A until the melting is complete; the arc voltage V3 is maintained at (80%~95%)×V2 until the melting is complete; the arc stabilizing current is maintained at 5~7A until the melting is complete to obtain a semi-finished titanium alloy ingot.

[0026] For example, according to the composition and size of the tertiary ingots and based on the parameters of the first-level feeding stage in 4.1, the preferred second-level feeding stage is 4.2: the melting current is 14kA~20kA, the arc voltage is 28V~30V, and the arc-stabilizing current is 7~9A, which are maintained for 1~2min; 4.3 the third-level feeding stage: the melting current is 6kA~14kA for 1~2min, and then maintained at 2~5A until the melting is completed; the arc voltage is maintained at 25V~28V until the melting is completed; the arc-stabilizing current is maintained at 5~7A until the melting is completed, to obtain a semi-finished titanium alloy ingot.

[0027] Preferably, in the primary feeding stage and the secondary feeding stage, the cooling water flow rate is controlled at 500-700 L / min, the inlet water temperature is 20°C-30°C, and the return water temperature is 40°C-45°C; During the third-level feeding stage, the cooling water flow rate is controlled at 400-600L / min, the inlet water temperature is 20℃-30℃, the return water temperature is 35℃-40℃, and the feeding time is not less than 2.5 hours; thereafter, the water flow rate is maintained at 300-500L / min, the inlet water temperature is 20℃-30℃, the return water temperature is 25℃-35℃, and the cooling time is not less than 6 hours.

[0028] Preferably, after the shrinkage and arc closing stages, the end face of the titanium ingot riser is cut off, and the cutting amount is 40 to 90 mm.

[0029] By finely controlling the parameters of current, voltage, and arc-stabilizing current of titanium alloy ingots in the arc starting stage, smelting stage, and arc-closing and shrinking stage, the quality of the consumable electrode reserved for arc-closing and shrinking, the process parameters such as cooling water, and the cleaning process of the primary ingot, the infiltration of volatiles and impurities can be effectively prevented, which not only avoids the local accumulation of these substances on the end face of the ingot, but also prevents the formation of metallurgical defects such as low-density inclusions during the subsequent forming process. In addition, defects such as large surface pores and poor quality caused by uneven shrinkage are reduced. According to non-destructive testing, the titanium ingot riser of the present invention is relatively shallow, with a depth of about 40 to 90 mm, and only a small amount of cutting is required, or basically no cutting is required. This shallow riser is left at the end of the strip after forging and then cut off, which not only improves the overall yield rate, but also saves a process, reducing production time and manufacturing costs.

[0030] During the VAR smelting process, the smelting and cooling parameters of the VAR smelting equipment are controlled, the temperature gradient is expanded, a strong and stable cooling method is adopted, the solidification rate is increased, the molten pool depth is reduced, the alloy solidification time is shortened, and the component segregation is reduced. This effectively ensures that the components of the titanium alloy ingot are fully alloyed and homogenized, effectively solves the problem of component segregation of large-size titanium alloy ingots, and is suitable for large-scale industrial production.

[0031] The present invention provides at least the following beneficial effects: (1) The present invention adopts a vacuum consumable arc furnace to perform secondary or tertiary smelting of titanium alloy consumable electrodes, and accurately controls the current, voltage, water volume, water temperature and other factors in each arc starting stage, smelting stage, shrinkage and arc closing stage and cooling link, thereby improving the uniformity of ingot composition and structure, reducing impurity content, and increasing the titanium ingot yield rate from the traditional 90% to more than 96%, preferably more than 97%, greatly reducing the preparation cost of titanium ingots, and being suitable for the production of titanium ingots of various diameters and sizes, with good promotion and application value.

[0032] (2) The present invention strictly cleans the primary ingot after the primary smelting to remove impurities such as oxides, chlorides, carbides, etc. on the surface of the primary ingot, thereby reducing the defect of the arc furnace that solid impurities are difficult to remove and preventing the ingot from being brought into the subsequent smelting and causing losses such as multiple ingots with many pores and excessive amount of peeled material.

[0033] (3) In the present invention, when the remaining amount of the consumable electrode is 2-6% after the second or third smelting, the ingot enters the shrinkage compensation and arc closure stage, and the smelting current, arc voltage and arc stabilization current are gradually reduced, and the cooling water flow and temperature are strictly controlled to reduce the holes, defects and riser size formed due to shrinkage during the cooling process of the ingot, improve the integrity and yield rate of the casting, and reduce the coarse grains and segregation phenomena, thereby improving the uniformity and performance of the material.

[0034] (4) In the preparation of titanium alloy consumable electrodes, the present invention adopts a non-uniform speed welding method for the front, middle and rear sections of the welding line to ensure welding strength and quality while taking into account welding efficiency. The auxiliary electrode with a specific size and chamfer design is designed to facilitate the overflow of the weld pool to the outer edge of the lower end surface of the auxiliary electrode during the welding process with the consumable electrode, further increasing the contact area of ​​the weld and improving the stability of the weld quality. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 This is a schematic diagram of a titanium ingot according to the present invention; Figure 2 A schematic diagram of a crucible of the present invention; Figure 3 This is a schematic diagram of a finished titanium ingot after the riser is removed according to the present invention; Figure 4 Schematic diagram of the sample of Comparative Example 1. DETAILED DESCRIPTION

[0036] In order to better understand the above technical solution, the above technical solution will be described in detail below in conjunction with specific implementation methods. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0037] The terms used in the embodiments of the present invention are only for the purpose of describing specific embodiments, and are not intended to limit the present invention. The singular forms "a", "said" and "the" used in the embodiments of the present invention and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings, and "multiple" generally includes at least two.

[0038] It should also be noted that the term "includes", "comprising" or any other variation thereof is intended to cover non-exclusive inclusion, so that a commodity or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such commodity or device. In the absence of more restrictions, the elements defined by the sentence "comprising a ..." do not exclude the existence of other identical elements in the commodity or device including the elements.

[0039] Reference Figures 1 to 3 The titanium alloy vacuum consumable melting method for improving the yield of titanium ingots of the present invention adopts a vacuum consumable arc furnace to perform secondary or tertiary melting of the titanium alloy consumable electrode, comprising: (1) A titanium alloy consumable electrode is prepared, wherein the consumable electrode comprises the following components in terms of weight percentage: Al 5.5~6.5% V 3.5~4.5% Fe 0.1~0.2% The total amount of C, H, O and N is ≤0.3%, preferably ≤0.2%, more preferably ≤0.15%, and the balance is titanium.

[0040] Among them, the titanium is preferably grade 0 sponge titanium with a particle size of 0.83-25.4 mm, the particle size of aluminum vanadium alloy is 1-6 mm, the particle size of aluminum beans is 5-11 mm, the particle size of titanium iron alloy is 1-6 mm, and the particle size of titanium dioxide is ≤45 μm.

[0041] The titanium alloy consumable electrode has a weight of 1000-6000 kg and a diameter d0 of 40 cm ≤ d0 ≤ 73 cm; The titanium alloy consumable electrode preparation steps include: 1.1. Batching and mixing: Use the automatic mixing system to batch the raw material components of the titanium alloy according to the proportion, and mix them using the single-block mixing method; 1.2. Electrode pressing and welding: Press a single electrode block, and use a non-tungsten electrode argon shielded plasma welding box to weld 25 to 35 pressed electrode blocks into a titanium alloy consumable electrode.

[0042] The auxiliary electrode made of the same grade of titanium alloy is butt-welded with the titanium alloy consumable electrode made in step (1) by using a non-tungsten electrode argon shielded plasma welding box, and the auxiliary electrode is installed on the pneumatic head of the electrode rod. The auxiliary electrode moves up and down to drive the titanium alloy consumable electrode to move up and down. The diameter d of the auxiliary electrode satisfies: 0.25d0≤d f ≤0.75d0, the chamfer of the lower end of the auxiliary electrode meets (4mm~6mm)×(45°±1°). The auxiliary electrode is made of the same grade of titanium alloy, which can ensure effective welding and fusion between the auxiliary electrode and the consumable electrode, and ensure convenient and stable connection between the consumable electrode and the electrode rod pneumatic head.

[0043] The aforementioned electrode blocks are welded into titanium alloy consumable electrodes, and the auxiliary electrode and the titanium alloy consumable electrode are butt-welded by vacuum plasma welding. Before welding, argon gas is filled in the vacuum plasma welding box. The flow rate of argon gas is 4L / min~7L / min, and the pressure of argon gas is maintained at 20000~30000Pa.

[0044] The welding adopts non-uniform speed welding method. In the front 1 / 4 to 1 / 3 range of the welding line, the welding speed is 50-60mm / min, the welding current is 400A-700A, and the voltage is 50V-58V; in the middle 1 / 3 to 1 / 2 range, the welding speed is 80-90mm / min, the welding current is 400A-700A, and the voltage is 55V-65V; in the rear 1 / 4 to 1 / 3 range, the welding speed is 100-120mm / min, the welding current is 500A-800A, and the voltage is 60V-70V. The cooling time after welding is 25-60min, which ensures the welding quality while taking into account the welding efficiency.

[0045] Check the quality of the weld after cooling. The weld has a silvery white metallic luster, the weld molten pool is full, the upper and lower parts are in a molten adhesion state, the effective welding adhesion area at the weld is ≥95%, preferably ≥98%, and more preferably 100%. After longitudinal sectioning, check that the effective welding area inside the weld is ≥90%, preferably ≥92%, and more preferably ≥95%.

[0046] (2) First smelting: using a first crucible to perform a first vacuum smelting on the titanium alloy consumable electrode obtained in step (1); the diameter D1 of the first crucible is 55 to 78 cm, the vacuum degree in the furnace is ≤1 Pa, and the gas leakage rate is ≤0.7 Pa / min; 2.1 The first arc starting stage: (2.1.1) When 0<t≤t1, the arc is struck with an arc starting current of 2kA~5kA, where t1 is 2~5min; (2.1.2) When t1<t≤t2, increase the current to the pre-melting current at a rate of 0.5~3kA / min, where t2 is 15~30min and the pre-melting current is 110~120% of the melting current; (2.1.3) When t2<t≤t2+tx, the pre-melting current is reduced to the melting current, and the arc starting stage enters the stable melting stage, and tx is 1 to 15 minutes.

[0047] 2.2 Stable smelting stage: the smelting current is 13-17kA, the smelting voltage is 31-34V, the arc stabilization current is 10-16A, and a primary ingot is obtained; during the smelting process, the cooling water flow rate is controlled at 1100-1300L / min, the inlet water temperature is 20°C-30°C, and the cooling time is not less than 5 hours, preferably not less than 6 hours; The surface of the primary ingot is cleaned to remove impurities such as carbides and chlorides, and the primary smelting loss is ≤1%, preferably ≤0.5%; the surface cleaning of the primary ingot is preferably carried out by ultrasonic-assisted cleaning, which specifically includes: a. Place the primary ingot on a cleaning rack with multiple rotating rollers, which can rotate the primary ingot; b. Use a brushing unit to brush the surface of the primary ingot; c. A cleaning unit, which cleans the surface of the primary ingot; preferably, the cleaning unit performs secondary brushing and cleaning on the primary ingot, and more preferably, an ultrasonic auxiliary unit is provided on the cleaning unit.

[0048] Among them, the dirt brushing unit and the cleaning unit can be respectively arranged on both sides of the cleaning rack, or the dirt brushing unit and the cleaning unit can be arranged on both sides of the cleaning rack, and the cleaning unit is arranged on the side of the dirt brushing unit, and the dirt brushing unit and the cleaning unit can move longitudinally along the cleaning rack to cover the entire length of the titanium ingot. The dirt brushing unit and the cleaning unit both include at least two roller brush groups abutting against the surface of the titanium ingot, the first roller brush group of the dirt brushing unit is connected to the first cleaning liquid inlet pipe, and the second roller brush group is connected to the first water inlet pipe; the third roller brush group of the cleaning unit is connected to the second cleaning liquid inlet pipe, and the fourth roller brush group is connected to the second water inlet pipe. The cleaning liquid inlet pipe and the water inlet pipe connected to the dirt brushing unit and the cleaning unit can have the same source or different sources, so as to prepare different cleaning liquid components according to the cleaning needs. Each roller brush group includes at least one stainless steel roller brush, and each roller brush is driven to rotate by a driving unit. Preferably, the third roller brush group of the cleaning unit is configured with an ultrasonic auxiliary unit for fine cleaning, and a pressurizing device is added between the fourth roller brush group of the cleaning unit and the water inlet pipe to increase the water inlet pressure to complete thorough cleaning. By driving the titanium ingot to rotate through rotating rollers, the brushing unit and the cleaning unit move longitudinally along the cleaning rack, and ultrasonic-assisted secondary brushing and cleaning treatment, the surface of the titanium ingot can be comprehensively and thoroughly cleaned to provide high-quality primary ingots for subsequent smelting, which is beneficial to improving the comprehensive mechanical, chemical, processing and other properties of the titanium ingot product.

[0049] Particularly preferably, a sewage collection tank is provided at the bottom of the cleaning rack, and the collected sewage can be sent to the first water inlet pipe for the dirt-brushing unit through a water pump after being filtered and purified at multiple stages, so as to achieve the purpose of recycling and reusing the purified water, thereby improving the utilization rate of water resources, reducing production costs and improving environmental benefits. The above surface cleaning method can also be used for subsequent ingots and finished products.

[0050] (3) Second smelting: Use a second crucible to carry out a second vacuum consumable smelting of the first ingot; the diameter D2 of the second crucible is 65 to 85 cm, the vacuum degree in the furnace is ≤0.8 Pa, and the leakage rate is ≤0.7 Pa / min; 3.1 The second arc starting stage: (3.1.1) When 0<t≤t1, the arc is struck with an arc starting current of 2kA~5kA, where t1 is 2~5min; (3.1.2) When t1<t≤t2, increase the current to the pre-melting current at a rate of 0.5~3kA / min, where t2 is 15~30min and the pre-melting current is 110~120% of the melting current; (3.1.3) When t2<t≤t2+tx, the pre-melting current is reduced to the melting current, and the arc starting stage enters the stable melting stage, and tx is 1 to 15 minutes.

[0051] 3.2 Stable smelting stage: the smelting current is 23-26KA, the smelting voltage is 31.5-33.5V, the arc stabilization current is 10-16A, and the secondary ingot is obtained; during the smelting process, the cooling water flow rate is controlled at 1100-1300L / min, the inlet water temperature is 20°C-30°C, and the cooling time is not less than 6 hours, preferably not less than 7 hours; Optionally, the secondary ingot is brushed to remove black carbides, chlorides, etc., and the head is flattened, peeled and polished; the total loss rate of secondary smelting is ≤4%, preferably ≤3%; The preferred third smelting: the third crucible is used to perform the third vacuum consumable smelting on the secondary ingot; the diameter D3 of the third crucible is 70-95 cm, the vacuum degree in the furnace is ≤0.5 Pa, and the gas leakage rate is ≤0.6 Pa / min; A. The third arc starting stage: (a1) When 0<t≤t1, the arc is struck with an arc starting current of 2kA~5kA, where t1 is 2~5min; (a2) When t1<t≤t2, the current is increased to the pre-melting current at a rate of 0.5~3kA / min, where t2 is 15~30min and the pre-melting current is 110~120% of the melting current; (a3) When t2<t≤t2+tx, the pre-melting current is reduced to the melting current, and the arc starting stage enters the stable melting stage, and tx is 1 to 15 minutes.

[0052] B. Stable smelting stage: smelting current 25-26KA, smelting voltage 32-34V, arc stabilization current 10-16A; during the smelting process, the cooling water flow rate is controlled at 1300-1500L / min, the inlet water temperature is 15°C-25°C, and the cooling time is not less than 7 hours, preferably not less than 8 hours; Optionally, the three ingots are subjected to skinning and polishing treatment; the total loss rate of the three smeltings is ≤5%, preferably ≤4%; When the weight of the remaining unmelted electrode accounts for 2-6% of the initial weight, proceed to step (4): (4) In the multi-stage compensation and arc closing stage, the argon filling pressure is set to 500-2000 Pa, which specifically includes the following steps: 4.1 Primary feeding stage: melting current C1 is 20-25kA, arc voltage V1 is 30V-32V, arc stabilization current is 9-14A, maintained for 1-2min; cooling water flow is controlled at 500-700L / min, inlet water temperature is 20℃-30℃, and return water temperature is 40℃-45℃; 4.2 Secondary feeding stage: melting current C2 is (60%-90%)×C1, preferably 14kA-20kA, arc voltage V2 is (80%-95%)×V1, preferably 28V-30V, arc stabilization current is 7-9A, maintained for 1-2min; cooling water flow rate is controlled at 500-700L / min, inlet water temperature is 20℃-30℃, and return water temperature is 40℃-45℃; 4.3 Three-stage shrinkage compensation stage: smelting current C3 is (30%~70%)×C2, preferably 6kA~14kA, maintained for 1~2min, and then maintained at 2~5A until complete melting; arc voltage V3 is (80%~95%)×V2, preferably 25V~28V, maintained until complete melting; arc stabilization current is maintained at 5~7A until complete melting; cooling water flow rate is controlled at 400~600L / min, inlet water temperature is 20℃~30℃, return water temperature is 35℃~40℃, and shrinkage compensation time is not less than 2.5 hours; then maintain the water flow rate at 300L / min~500L / min, inlet water temperature is 20℃~30℃, return water temperature is 25℃~35℃, cooling time is not less than 6 hours, and a titanium ingot is obtained.

[0053] Optionally, the titanium ingot is subjected to surface processing to obtain a high-quality titanium ingot product, preferably including but not limited to, performing a riser end face cutting operation, see attached Figure 3 The finished titanium ingot with the riser cut off has a cutting amount of 40 to 90 mm.

[0054] Example 1 The titanium alloy vacuum consumable melting method of Example 1 uses a vacuum consumable arc furnace to perform secondary melting on the titanium alloy consumable electrode, comprising: (1) Preparation of titanium alloy consumable electrode: 1.1 Use an automatic mixing system to mix titanium sponge with aluminum vanadium, aluminum beans, ferrotitanium and titanium dioxide in proportion, and use a single-block mixing method to mix; In terms of weight percentage, the consumable electrode comprises the following raw material composition: Al 6.2%, V 4.3%, Fe 0.12%, the total amount of C, H, O, and N is ≤0.15%, and the balance is titanium.

[0055] 1.2 After mixing the ingredients, the materials are pressed into a single electrode block by a hydraulic press, and the 30 pressed electrode blocks are welded into a titanium alloy consumable electrode by a non-tungsten electrode argon shielded plasma welding box in a non-uniform speed welding manner. The titanium alloy consumable electrode weighs 5010 kg and has a diameter d0 of 65 cm.

[0056] 1.3 Use a non-tungsten electrode argon shielded plasma welding box to weld the auxiliary electrode made of the same grade of titanium alloy to the titanium alloy consumable electrode in a non-uniform speed welding mode, and install the auxiliary electrode on the pneumatic head of the electrode rod, and drive the titanium alloy consumable electrode to move up and down through the auxiliary electrode. The diameter d of the auxiliary electrode f The chamfer angle of the lower end of the auxiliary electrode is 5mm×45°.

[0057] (2) First melting: using a first crucible with a diameter D1 of 72 cm to perform the first vacuum melting of the titanium alloy consumable electrode obtained in step (1), the vacuum degree in the furnace is ≤1 Pa, and the leakage rate is ≤0.7 Pa / min; 2.1 The first arc starting stage: (2.1.1) Stir the arc for 3 minutes at an arc starting current of 3.5 kA; (2.1.2) After arcing is completed, the current is increased to a pre-melting current of 20.3 kA at a rate of 1.4 kA / min between the 3rd and 15th minutes, and pre-melting is performed at a pre-melting current of 20.3 kA between the 15th and 20th minutes; (2.1.3) Within 5 minutes after the 20th minute, the pre-melting current of 20.3kA is reduced to the melting current of 17kA, and the arc starting stage enters the stable melting stage, and the stable melting stage is entered; 2.2 Stable smelting stage: vacuum degree in the furnace ≤1Pa, gas leakage rate ≤0.7Pa / min, smelting current 17kA, smelting voltage 34V, arc stabilization current 16A, and a primary ingot is obtained; during the smelting process, the cooling water flow rate is controlled at 1300L / min, the water inlet temperature is 25℃, and the cooling time is 6 hours; the carbides and chlorides on the surface of the primary ingot are thoroughly cleaned, and the loss of the primary smelting is about 0.35%; (3) Second smelting: Use a second crucible with a diameter D2 of 80 cm to carry out a second vacuum consumable smelting of the first ingot, the vacuum degree in the furnace is ≤0.8 Pa, and the leakage rate is ≤0.7 Pa / min; 3.1 The second arc starting stage: (3.1.1) Start the arc with an arc starting current of 4kA for 3 minutes; (3.1.2) After arcing is completed, the current is increased to a pre-melting current of 29.5 kA at a rate of 1.7 kA / min between the 3rd and 18th minutes, and pre-melting is performed at a pre-melting current of 29.5 kA between the 18th and 20th minutes; (3.1.3) Within 5 minutes after the 20th minute, the pre-melting current of 29.5kA is reduced to the melting current of 26kA, and the arc starting stage enters the stable melting stage, and enters the stable melting stage; 3.2 Stable smelting stage: the smelting current is 26KA, the smelting voltage is 33.5V, the arc stabilization current is 16A, and the secondary ingot is obtained; during the smelting process, the cooling water flow is controlled at 1300L / min, the water inlet temperature is 20℃, and the cooling time is 7h; the secondary ingot is flattened, peeled and polished, and the total loss of the secondary smelting is about 1.9%; When the weight of the remaining unmelted electrode reaches 200 kg, the process enters step (4) of multi-stage feeding and arc closure, and the argon filling pressure is set to 600 Pa, which specifically includes the following steps: 4.1 Primary feeding stage: melting current is 25kA, arc voltage is 31.5V, arc stabilization current is 14A, maintained for 1min, cooling water flow rate is controlled at 600L / min, and water inlet temperature is 42℃; 4.2 Secondary feeding stage: melting current is 20kA, arc voltage is 30V, arc stabilization current is 8.5A, maintained for 1min, cooling water flow rate is controlled at 600L / min, and water inlet temperature is 40℃; 4.3 Three-stage shrinkage compensation stage: the smelting current is maintained at 14kA for 1min and 4A until complete melting; the arc voltage is maintained at 27.5V until complete melting; the arc stabilizing current is maintained at 7A until complete melting, the cooling water flow rate is controlled at 500L / min, the inlet water temperature is 25℃, the return water temperature is 35℃, and the cooling time is 3 hours; then the water flow rate is maintained at 400L / min, the inlet water temperature is 20℃, the return water temperature is 30℃, and the cooling time is 6 hours to obtain a titanium ingot with a diameter of about 78±0.5cm and a yield rate of about 98.1%.

[0058] (5) Perform a cut operation on the end face of the riser, with a cut amount of 50 mm.

[0059] Example 2 The titanium alloy vacuum consumable melting method of Example 2 is mainly different from that of Example 1 in that a vacuum consumable arc furnace is used to melt the titanium alloy consumable electrode three times, specifically comprising: (1) First melting: Use the first crucible with a diameter D1 of 70 cm to perform the first vacuum melting of the titanium alloy consumable electrode with a diameter d0 of 65 cm. The vacuum degree in the furnace is ≤1Pa and the leakage rate is ≤0.7Pa / min. 1.1 The first arc starting stage: (1.1.1) Start the arc for 3 minutes with an arc starting current of 3.5 kA; (1.1.2) After arcing is completed, the current is increased to a pre-melting current of 20.3 kA at a rate of 1.4 kA / min between the 3rd and 15th minutes, and pre-melting is performed at a pre-melting current of 20.3 kA between the 15th and 20th minutes; (1.1.3) Within 5 minutes after the 20th minute, the pre-melting current of 20.3kA is reduced to the melting current of 17kA, and the arc starting stage enters the stable melting stage, and the stable melting stage is entered; 1.2 Stable smelting stage: the smelting current is 17kA, the smelting voltage is 33.5V, the arc stabilization current is 16A, and a primary ingot is obtained; during the smelting process, the cooling water flow rate is controlled at 1200L / min, the water inlet temperature is 25℃, and the cooling time is 6 hours; the carbides and chlorides on the surface of the primary ingot are thoroughly cleaned, and the primary smelting loss is about 0.3%; (2) Second smelting: Use a second crucible with a diameter D2 of 75 cm to carry out a second vacuum consumable smelting of the first ingot, the vacuum degree in the furnace is ≤0.8 Pa, and the leakage rate is ≤0.7 Pa / min; 2.1 The second arc starting stage: (2.1.1) Start the arc with an arc current of 4kA for 3 minutes; (2.1.2) After arcing is completed, the current is increased to a pre-melting current of 29.5 kA at a rate of 1.7 kA / min between the 3rd and 18th minutes, and pre-melting is performed at a pre-melting current of 29.5 kA between the 18th and 20th minutes; (2.1.3) Within 5 minutes after the 20th minute, the pre-melting current of 29.5kA is reduced to the melting current of 25kA, and the arc starting stage enters the stable melting stage, and enters the stable melting stage; 2.2 Stable smelting stage: the smelting current is 25KA, the smelting voltage is 33V, the arc stabilization current is 15A, and the secondary ingot is obtained; during the smelting process, the cooling water flow is controlled at 1200L / min, the water inlet temperature is 25℃, and the cooling time is 6h; the secondary ingot is flattened, peeled and polished, and the total loss of the secondary smelting is about 0.6%; (3) Third smelting: The third crucible is used to carry out the third vacuum consumable smelting of the secondary ingot; the diameter D3 of the third crucible is 80 cm, the vacuum degree in the furnace is ≤0.5 Pa, and the leakage rate is ≤0.6 Pa / min; 3.1 The third arc starting stage: (3.1.1) Stir the arc at an arc starting current of 3kA for 2 minutes; (3.1.2) After arcing is completed, the current is increased to a pre-melting current of 30.2 kA at a rate of 1.7 kA / min between the 2nd and 18th minutes, and pre-melting is performed at a pre-melting current of 30.2 kA between the 18th and 20th minutes; (3.1.3) Within 5 minutes after the 20th minute, the pre-melting current of 30.2kA is reduced to the melting current of 26.5kA, and the arc starting stage enters the stable melting stage, and enters the stable melting stage; 3.2 Stable smelting stage: smelting current is 26.5KA, smelting voltage is 33V, arc stabilization current is 15A, and three ingots are obtained; during the smelting process, the cooling water flow rate is controlled at 1400L / min, the water inlet temperature is 20℃, the cooling time is 7h, and the skinning treatment is carried out. The total loss of the three smeltings is 2.4%; The subsequent multi-stage shrinkage and arc closing processes are the same as those in Example 1, and finally a titanium ingot with a diameter of about 78±0.5 cm is obtained, and the yield rate is about 97.6%.

[0060] Example 3 The titanium alloy vacuum consumable melting method of Example 3 uses a vacuum consumable arc furnace to melt the titanium alloy consumable electrode three times, comprising: (1) Preparation of titanium alloy consumable electrode: 1.1 Use an automatic mixing system to mix titanium sponge with aluminum vanadium, aluminum beans, ferrotitanium and titanium dioxide in proportion, and use a single-block mixing method to mix; In terms of weight percentage, the consumable electrode comprises the following raw material composition: Al 6.3%, V 4.1%, Fe 0.14%, the total amount of C, H, O, and N is ≤0.15%, and the balance is titanium.

[0061] 1.2 After mixing the ingredients, the materials are pressed into a single electrode block by a hydraulic press, and the 30 pressed electrode blocks are welded into a titanium alloy consumable electrode by a non-tungsten electrode argon shielded plasma welding box in a non-uniform speed welding manner. The titanium alloy consumable electrode weighs 4110 kg and has a diameter d0 of 60 cm.

[0062] 1.3 Use a non-tungsten electrode argon shielded plasma welding box to weld the auxiliary electrode made of the same grade of titanium alloy to the titanium alloy consumable electrode in a non-uniform speed welding mode, and install the auxiliary electrode on the pneumatic head of the electrode rod, and drive the titanium alloy consumable electrode to move up and down through the auxiliary electrode. The diameter d of the auxiliary electrode f The chamfer angle of the lower end of the auxiliary electrode meets the requirements of 5mm×45°.

[0063] (2) First Melting: Using a first crucible with a diameter D1 of 65 cm, the titanium alloy consumable electrode obtained in step (1) is subjected to first vacuum consumable melting, with the vacuum degree in the furnace ≤1 Pa and the gas leakage rate ≤0.7 Pa / min; 2.1 The first arc starting stage: (2.1.1) Stir the arc for 3 minutes at an arc starting current of 3kA; (2.1.2) After arcing is completed, the current is increased to a pre-melting current of 12.6 kA at a rate of 0.8 kA / min between the 3rd and 15th minutes, and pre-melting is performed at a pre-melting current of 12.6 kA between the 15th and 20th minutes; (2.1.3) After the 20th minute, enter; (3.1.1) Start the arc with an arc starting current of 3kA for 3 minutes; (3.1.2) After arcing is completed, the current is increased to a pre-melting current of 17.4 kA at a rate of 1.2 kA / min between the 3rd and 15th minutes, and pre-melting is performed at a pre-melting current of 17.4 kA between the 18th and 20th minutes; (3.1.3) Within 5 minutes after the 20th minute, the pre-melting current of 17.4kA is reduced to the melting current of 15kA, and the arc starting stage enters the stable melting stage, and enters the stable melting stage; 2.2 Stable smelting stage: the smelting current is 15kA, the smelting voltage is 32.5V, the arc stabilization current is 13A, and a primary ingot is obtained; during the smelting process, the cooling water flow rate is controlled at 1200L / min, the water inlet temperature is 25℃, and the cooling time is 6 hours; the carbides and chlorides on the surface of the primary ingot are thoroughly cleaned, and the loss of the primary smelting is 0.32%; (3) Second smelting: Use a second crucible with a diameter D2 of 70 cm to carry out a second vacuum consumable smelting of the first ingot, the vacuum degree in the furnace is ≤0.8 Pa, and the leakage rate is ≤0.7 Pa / min; 3.1 The second arc starting stage: (3.1.1) Start the arc with an arc starting current of 4kA for 3 minutes; (3.1.2) After arcing is completed, the current is increased to a pre-melting current of 26.5 kA at a rate of 1.5 kA / min between the 3rd and 18th minutes, and pre-melting is performed at a pre-melting current of 26.5 kA between the 18th and 20th minutes; (3.1.3) Within 5 minutes after the 20th minute, the pre-melting current of 26.5kA is reduced to the melting current of 24kA, and the arc starting stage enters the stable melting stage, and enters the stable melting stage; 3.2 Stable smelting stage: the smelting current is 24KA, the smelting voltage is 32.5V, the arc stabilization current is 13A, and the secondary ingot is obtained; during the smelting process, the cooling water flow is controlled at 1200L / min, the water inlet temperature is 25℃, and the cooling time is 6h; the secondary ingot is flattened, peeled and polished, and the total loss of the secondary smelting is 0.65%; Third smelting: the third crucible is used to carry out the third vacuum consumable smelting of the secondary ingot; the diameter D3 of the third crucible is 75 cm, the vacuum degree in the furnace is ≤0.5 Pa, and the gas leakage rate is ≤0.6 Pa / min; A. The third arc starting stage: (a1) Stir the arc at an arc starting current of 3 kA for 2 min; (a2) After arcing is completed, the current is increased to a pre-melting current of 19.9 kA at a rate of 1.3 kA / min between the 2nd and 15th minutes, and pre-melting is performed at a pre-melting current of 19.9 kA between the 15th and 20th minutes; (a3) After the 20th minute, enter; (3.1.1) Stir the arc at an arc starting current of 3kA for 2 minutes; (3.1.2) After arcing is completed, the current is increased to a pre-melting current of 28.6 kA at a rate of 1.6 kA / min between the 2nd and 18th minutes, and pre-melting is performed at a pre-melting current of 28.6 kA between the 18th and 20th minutes; (3.1.3) Within 5 minutes after the 20th minute, the pre-melting current of 28.6kA is reduced to the melting current of 25kA, and the arc starting stage enters the stable melting stage, and enters the stable melting stage; B. Stable smelting stage: smelting current is 25KA, smelting voltage is 33V, arc stabilization current is 13A, and three ingots are obtained; during the smelting process, the cooling water flow rate is controlled at 1400L / min, the water inlet temperature is 20℃, the cooling time is 7h, and the skin is peeled. The total loss of the three smeltings is 2.7%; When the weight of the remaining unmelted electrode reaches 150 kg, proceed to step (4); (4) In the multi-stage compensation and arc closing stage, the argon filling pressure is set to 600Pa, which specifically includes the following steps: 4.1 Primary feeding stage: melting current is 23kA, arc voltage is 31V, arc stabilization current is 12KA, maintained for 1min, cooling water flow is controlled at 600L / min, and water inlet temperature is 42℃; 4.2 Secondary feeding stage: melting current is 17kA, arc voltage is 29V, arc stabilization current is 8KA, maintained for 1min, cooling water flow is controlled at 600L / min, and water inlet temperature is 40℃; 4.3 Three-stage shrinkage compensation stage: the smelting current is maintained at 10kA for 1min and 4kA until the melting is complete; the arc voltage is maintained at 26V until the melting is complete; the arc stabilizing current is maintained at 6KA until the melting is complete, the cooling water flow rate is controlled at 500L / min, the water inlet temperature is 35℃, and the cooling time is 3 hours; then the water flow rate is maintained at 400L / min, the water inlet temperature is 25℃, and the cooling time is 6 hours to obtain a titanium ingot with a diameter of about 73±0.5cm and a yield rate of about 97.3%.

[0064] (5) Perform a cut operation on the end face of the riser, with a cut amount of 55 mm.

[0065] Example 4 The titanium alloy vacuum consumable melting method of Example 4 uses a vacuum consumable arc furnace to melt the titanium alloy consumable electrode three times, comprising: (1) Preparation of titanium alloy consumable electrode: 1.1 Use an automatic mixing system to mix titanium sponge with aluminum vanadium, aluminum beans, ferrotitanium and titanium dioxide in proportion, and use a single-block mixing method to mix; In terms of weight percentage, the consumable electrode comprises the following raw material composition: Al 6.4%, V 4.0%, Fe 0.12%, the total amount of C, H, O, and N is ≤0.15%, and the balance is titanium.

[0066] 1.2 After mixing the ingredients, the materials are pressed into a single electrode block by a hydraulic press, and the 30 pressed electrode blocks are welded into a titanium alloy consumable electrode by a non-tungsten electrode argon shielded plasma welding box in a non-uniform speed welding manner. The titanium alloy consumable electrode weighs 1500 kg and has a diameter d0 of 45 cm.

[0067] 1.3 Use a non-tungsten electrode argon shielded plasma welding box to weld the auxiliary electrode made of the same grade of titanium alloy to the titanium alloy consumable electrode in a non-uniform speed welding mode, and install the auxiliary electrode on the pneumatic head of the electrode rod, and drive the titanium alloy consumable electrode to move up and down through the auxiliary electrode. The diameter d of the auxiliary electrode f The chamfer angle of the lower end of the auxiliary electrode is 5mm×45°.

[0068] (2) First melting: using a first crucible with a diameter D1 of 55 cm to perform the first vacuum melting of the titanium alloy consumable electrode obtained in step (1), the vacuum degree in the furnace is ≤1 Pa, and the leakage rate is ≤0.7 Pa / min; 2.1 The first arc starting stage: (2.1.1) Stir the arc for 3 minutes at an arc starting current of 3kA; (3.1.2) After arcing is completed, the current is increased to a pre-melting current of 16.2 kA at a rate of 1.1 kA / min between the 3rd and 15th minutes, and pre-melting is performed at a pre-melting current of 16.2 kA between the 15th and 20th minutes; (3.1.3) Within 5 minutes after the 20th minute, the pre-melting current of 16.2kA is reduced to the melting current of 14kA, and the arc starting stage enters the stable melting stage, and enters the stable melting stage; 2.2 Stable smelting stage: the smelting current is 14kA, the smelting voltage is 31V, the arc stabilization current is 13KA, and a primary ingot is obtained; during the smelting process, the cooling water flow rate is controlled at 1200L / min, the water inlet temperature is 25℃, and the cooling time is 6 hours; the carbides and chlorides on the surface of the primary ingot are thoroughly cleaned, and the primary smelting loss is 0.35%; (3) Second smelting: Use a second crucible with a diameter D2 of 65 cm to carry out a second vacuum consumable smelting of the first ingot, the vacuum degree in the furnace is ≤0.8 Pa, and the leakage rate is ≤0.7 Pa / min; 3.1 The second arc starting stage: (3.1.1) Start the arc with an arc starting current of 4kA for 3 minutes; (3.1.2) After arcing is completed, the current is increased to a pre-melting current of 26.5 kA at a rate of 1.5 kA / min between the 3rd and 18th minutes, and pre-melting is performed at a pre-melting current of 26.5 kA between the 18th and 20th minutes; (3.1.3) Within 5 minutes after the 20th minute, the pre-melting current of 26.5kA is reduced to the melting current of 23kA, and the arc starting stage enters the stable melting stage, and enters the stable melting stage; 3.2 Stable smelting stage: the smelting current is 23KA, the smelting voltage is 31.5V, the arc stabilization current is 12A, and the secondary ingot is obtained; during the smelting process, the cooling water flow is controlled at 1200L / min, the water inlet temperature is 25℃, and the cooling time is 6h; the secondary ingot is flattened, peeled and polished, and the total loss of the secondary smelting is 0.71%; Third smelting: the third crucible is used to carry out the third vacuum consumable smelting of the secondary ingot; the diameter D3 of the third crucible is 70 cm, the vacuum degree in the furnace is ≤0.5 Pa, and the gas leakage rate is ≤0.6 Pa / min; A. The third arc starting stage: (a1) Stir the arc at an arc starting current of 3 kA for 2 min; (a2) After arcing is completed, the current is increased to a pre-melting current of 28.6 kA at a rate of 1.6 kA / min between the 2nd and 18th minutes, and pre-melting is performed at a pre-melting current of 28.6 kA between the 18th and 20th minutes; (a3) Within 5 minutes after the 20th minute, the pre-melting current of 28.6 kA is reduced to the melting current of 25 kA, and the arc starting stage enters the stable melting stage; Stable smelting stage: smelting current is 25KA, smelting voltage is 32V, arc stabilization current is 11A, and three ingots are obtained; during the smelting process, the cooling water flow rate is controlled at 1400L / min, the water inlet temperature is 20℃, the cooling time is 7h, and the skin is peeled. The total loss of the three smeltings is 3.3%; When the weight of the remaining unmelted electrode reaches 60 kg, proceed to step (4); (4) In the multi-stage compensation and arc closing stage, the argon filling pressure is set to 600Pa, which specifically includes the following steps: 4.1 Primary feeding stage: melting current is 20kA, arc voltage is 30V, arc stabilization current is 10A, maintained for 1min, cooling water flow rate is controlled at 600L / min, and water inlet temperature is 42℃; 4.2 Secondary feeding stage: melting current is 15kA, arc voltage is 28V, arc stabilization current is 7A, maintained for 1min, cooling water flow rate is controlled at 600L / min, and water inlet temperature is 40℃; 4.3 Three-stage shrinkage compensation stage: the smelting current is maintained at 8kA for 1min and 4kA until the melting is complete; the arc voltage is maintained at 25V until the melting is complete; the arc stabilizing current is maintained at 5A until the melting is complete, the cooling water flow rate is controlled at 500L / min, the water inlet temperature is 35℃, and the cooling time is 3 hours; then the water flow rate is maintained at 400L / min, the water inlet temperature is 25℃, and the cooling time is 6 hours to obtain a titanium ingot with a diameter of about 68±0.5cm and a yield rate of about 96.7%.

[0069] (5) Perform a cut operation on the end face of the riser, with a cut amount of 55 mm.

[0070] Example 5 Based on Example 2, the smelting voltage, smelting current and arc stabilizing current in the first smelting, the second smelting and the third smelting are adjusted, and the other process step parameters are the same.

[0071] (1) First smelting: arc starting current 3.5kA, pre-melting current 15.5kA, melting current 13.5kA, melting voltage 31V, arc stabilization current 13A, cooling and cleaning to obtain a single ingot, the loss of a single smelting is about 0.42%; (2) Second smelting: arc starting current 4kA, pre-melting current 25kA, melting current 22KA, melting voltage 31.5V, arc stabilization current 12A, cooling, flattening, peeling and polishing treatment to obtain secondary ingots, the total loss of the secondary smelting is about 0.7%; (3) The third smelting: arc starting current 3kA, pre-melting current 28.6kA, melting current 25KA, melting voltage 32V, arc stabilization current 13A, three ingots were obtained by peeling, and the total loss of the three smeltings was 3.5%; The subsequent multi-stage shrinkage and arc closing processes are the same as those in Example 2, and finally a titanium ingot with a diameter of about 78±0.5 cm is obtained, and the yield rate is about 96.5%.

[0072] Example 6 Based on Example 2, the smelting voltage, smelting current and arc stabilizing current in the first smelting, the second smelting and the third smelting are adjusted, and the other process step parameters are the same.

[0073] (1) First smelting: arc starting current 3.5kA, pre-melting current 17.9kA, melting current 15.5kA, melting voltage 32V, arc stabilization current 15A, cooling and cleaning to obtain a single ingot, the loss of a single smelting is about 0.36%; (2) Second smelting: arc starting current 4kA, pre-melting current 28kA, melting current 24.5KA, melting voltage 32V, arc stabilization current 14A, cooling, flattening, peeling and polishing treatment to obtain secondary ingots, the total loss of the secondary smelting is about 0.65%; (3) The third smelting: arc starting current 3kA, pre-melting current 28.6kA, melting current 26KA, melting voltage 33V, arc stabilization current 14A, three ingots were obtained by peeling, and the total loss of the three smeltings was 3.0%; The subsequent multi-stage shrinkage and arc closing processes are the same as those in Example 2, and finally a titanium ingot with a diameter of about 78±0.5 cm is obtained, and the yield rate is about 97.0%.

[0074] Some parameters of Examples 1 to 6 are shown in Table 1.

[0075] Table 1:

[0076] Comparative Example 1 Based on Example 2, the difference is that the arc starting conditions in each smelting stage are different. In this comparative example, the current is increased to each smelting current at a rate of 2.5 kA / min, and the stable smelting stage is entered. Due to the short arc starting time and the hasty establishment of the molten pool, the surface quality of the titanium ingots obtained from each smelting was low (see Appendix Figure 4 The titanium ingot shown in the figure requires a lot of surface treatment, resulting in excessive material loss. The loss of the first smelting is about 2.1%, the total loss of the second smelting is about 3.5%, and the total loss of the third smelting is 7.7%. The overall yield rate is about 92.3%.

[0077] Comparative Example 2 Based on Example 2, the primary ingot was only cleaned with a stainless steel dry brush, and the carbides and chlorides on the surface of the primary ingot were not thoroughly cleaned. The impurities entered the subsequent smelting with the primary ingot, resulting in a large loss of subsequent ingots such as peeling. The total loss of the secondary smelting was about 1.9%, the total loss of the tertiary smelting was 5.8%, and the overall yield rate was about 94.2%.

[0078] Embodiments 7 to 9 Embodiments 7 and 8 are based on embodiment 2, except that the process parameters in the multi-stage feeding and arc closing stages are different, and the remaining process steps and parameters are the same.

[0079] Example 9 is based on Example 2, except that the process parameters of the three-stage feeding stage are different, and the remaining process steps and parameters are the same.

[0080] Table 2:

[0081] Test Method The ingot surfaces of Examples 1, 2, and 9 were sampled at three points in the longitudinal direction and the transverse specimens in the middle of the ingots were sampled at nine points in the transverse direction to analyze the composition uniformity of the entire ingot. The test results are shown in Tables 3-4.

[0082] Table 3 Chemical composition at three points in the longitudinal direction of the ingots of Examples 1, 2 and 9 (wt%)

[0083] Table 4 Chemical composition of nine points in the middle of the ingots of Examples 1, 2, and 9 (wt%)

[0084] As can be seen from Tables 1 to 4, the ingot yield rate of Example 1 using secondary smelting is higher than that of Examples 2-6 using tertiary smelting, but under the same material composition, the uniformity of the titanium ingot composition of Example 2 using tertiary smelting is better than that of Example 1. Secondly, although the process parameters in the multi-stage feeding and arc closing stages of Example 2 and Examples 7-8 are different, the difference in the uniformity of the titanium ingot composition is not large, and the uniformity of the titanium ingot of Example 9 using only a single cooling method for the three-stage feeding is slightly lower than that of Example 2.

[0085] Although the preferred embodiments of the present invention have been described, those skilled in the art may make additional changes and modifications to these embodiments once they are aware of the basic creative concepts. Therefore, the present invention is intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention, and these modifications and variations belong to the scope of the present invention and its equivalent technologies.

Claims

1. A vacuum consumable smelting method for improving the yield of titanium ingots, characterized in that: The titanium alloy consumable electrode is melted by a vacuum consumable arc furnace, including: (1) Preparation of titanium alloy consumable electrodes; (2) First smelting: vacuum degree in the furnace ≤1Pa, gas leakage rate ≤0.7Pa / min, smelting current 13-17kA, smelting voltage 31-34V, arc stabilization current 10-16A, and cooling after smelting to obtain a primary ingot; (3) Second smelting: vacuum degree in the furnace ≤ 0.8Pa, gas leakage rate ≤ 0.7Pa / min, smelting current 23-26KA, smelting voltage 31.5-33.5V, arc stabilization current 10-16A, cooling after smelting to obtain secondary ingots, total loss rate of secondary smelting ≤ 4%; (4) Entering the stage of arc supplementation and arc closure, the melting current, arc voltage and arc stabilization current are gradually reduced to obtain a titanium ingot.

2. The titanium alloy vacuum consumable melting method according to claim 1, characterized in that: Step (1) includes: 1.

1. Batching and mixing: Batching and mixing the raw material components of titanium alloy according to the proportion; 1.

2. Electrode pressing and welding: Press a single electrode block, and use a non-tungsten electrode argon shielded plasma welding box to weld the pressed electrode block into a titanium alloy consumable electrode. The weight of the titanium alloy consumable electrode is 1000-6000kg, and the diameter d0 is 40cm≤d0≤73cm; The obtained titanium alloy consumable electrode comprises the following components by weight percentage: Al 5.5~6.5% V 3.5~4.5% Fe 0.1~0.2% The total amount of C, H, O and N is ≤0.3%, and the balance is titanium.

3. The vacuum consumable melting method of high-purity titanium ingot according to claim 2, characterized in that: The auxiliary electrode made of the same grade of titanium alloy is butt-welded to the titanium alloy consumable electrode made in step (1) by using a non-tungsten electrode argon shielded plasma welding box, and the auxiliary electrode is mounted on the pneumatic head of the electrode rod. The titanium alloy consumable electrode is driven to move up and down by the auxiliary electrode moving up and down, and the diameter df of the auxiliary electrode satisfies: 0.25d0≤df≤0.75d0.

4. The titanium alloy vacuum consumable melting method according to any one of claims 1 to 3, characterized in that: After the second smelting, a third smelting is also included, the vacuum degree in the furnace is ≤0.5Pa, the gas leakage rate is ≤0.6Pa / min, the smelting current is 25-26KA, the smelting voltage is 32-34V, the arc stabilization current is 10-16A, and the smelting is followed by cooling to obtain a third ingot; The total loss rate of three smeltings is ≤5%.

5. The titanium alloy vacuum consumable melting method according to claim 4, characterized in that: In each smelting, before the stable smelting stage, there is also an arc starting stage from 0 to t2+tx: (1) When 0<t≤t1, the arc is struck with an arc starting current of 2kA~5kA, where t1 is 2~5min; (2) When t1<t≤t2, increase the current to the pre-melting current at a rate of 0.5~3kA / min, where t2 is 15~30min and the pre-melting current is 110~120% of the melting current; (3) When t2<t≤t2+tx, the pre-melting current is reduced to the melting current, and the arc starting stage enters the stable melting stage, and tx is 1 to 15 minutes.

6. The titanium alloy vacuum consumable melting method according to claim 5, characterized in that: In step (2), the titanium alloy consumable electrode obtained in step (1) is first smelted in a first crucible, wherein the diameter D1 of the first crucible is 55 to 78 cm; and the surface of the primary ingot is cleaned; In step (3), the treated primary ingot is melted for a second time in a second crucible, wherein the diameter D2 of the second crucible is 65 to 85 cm; the secondary ingot is flattened, peeled and polished; After step (3), the treated secondary ingot is smelted for the third time in a third crucible, wherein the diameter D3 of the third crucible is 70-95 cm; and the tertiary ingot is subjected to skinning and polishing treatment.

7. The titanium alloy vacuum consumable melting method according to claim 6, characterized in that: During the first and second smelting, the cooling water flow rate is controlled at 1100-1300 L / min, the inlet water temperature is 20℃-30℃, and the cooling time after smelting is not less than 5 hours; During the third smelting, the cooling water flow rate is controlled at 1300-1500 L / min, the inlet water temperature is 20°C-30°C, and the cooling time after smelting is not less than 7 hours.

8. The titanium alloy vacuum consumable melting method according to claim 6 or 7, characterized in that: When the weight of the remaining unmelted electrode accounts for 2-6% of the initial weight, the process proceeds to step (4) of shrinkage and arc closure, which includes the following steps: 4.1 Primary feeding stage: melting current C1 is 20-25kA, arc voltage V1 is 30V-32V, arc stabilization current is 8-14A, maintain for 1-2min; 4.2 Secondary feeding stage: melting current C2 is (60%~90%)×C1, arc voltage V2 is (80%~95%)×V1, arc stabilization current is 7~9A, maintain for 1~2min; 4.3 Three-level shrinkage feeding stage: the melting current C3 is maintained at (30%~70%)×C2 for 1~2 minutes, and then maintained at 2~5A until the melting is complete; the arc voltage V3 is maintained at (80%~95%)×V2 until the melting is complete; the arc stabilizing current is maintained at 5~7A until the melting is complete to obtain a semi-finished titanium alloy ingot.

9. The titanium alloy vacuum consumable melting method according to claim 8, characterized in that: In the primary and secondary feeding stages, the cooling water flow rate is controlled at 500-700L / min, the inlet water temperature is 20℃-30℃, and the return water temperature is 40℃-45℃; During the third-level feeding stage, the cooling water flow rate is controlled at 400-600L / min, the inlet water temperature is 20℃-30℃, the return water temperature is 35℃-40℃, and the feeding time is not less than 2.5 hours; thereafter, the water flow rate is maintained at 300-500L / min, the inlet water temperature is 20℃-30℃, the return water temperature is 25℃-35℃, and the cooling time is not less than 6 hours.

10. The titanium alloy vacuum consumable melting method according to claim 8, characterized in that: After the shrinkage and arc closing stages, the end face of the titanium ingot riser is cut off with a cutting amount of 40 to 90 mm.

Citation Information

Patent Citations

  • A method for producing TC4 titanium alloy round / flat ingots

    CN107502784B

  • Smelting method for improving titanium alloy cast ingot production efficiency and yield

    CN117535539A

Cited By

  • Method for eliminating arc striking of crucible wall in titanium alloy VAR smelting process and application

    CN121575233A

  • Method for eliminating arc striking on crucible wall in VAR melting process of titanium alloy and application

    CN121575233B