Aluminum alloy material and preparation method thereof

By adding modified mixed reinforcements of single-walled carbon nanotubes, silicon nitride and silicon carbide into the aluminum alloy matrix, combined with vacuum ball milling and hot rolling and cold rolling processes, the difficulty of balancing the strength and plasticity of aluminum matrix composites is solved. solve the problem and prepare aluminum alloy materials with excellent strength and plasticity, which expands its application prospects.

CN118726799APending Publication Date: 2024-10-01GUANGDONG YAN ALUMINUM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410664911.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-27
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

When preparing aluminum-based composite materials in the prior art, it is difficult to balance strength and plasticity. Especially when the content of graphene increases, the elongation decreases and the shaping is poor, which affects its application in the market.

Method used

A mixed reinforcement of modified single-walled carbon nanotubes, silicon nitride and silicon carbide is added to the aluminum alloy matrix. Through vacuum ball milling, ultrasonic dispersion, stirring and hot rolling and cold rolling processes, a composite material with excellent strength and plasticity is prepared. aluminum alloy material.

Benefits of technology

Through the uniform dispersion of the modified reinforcements in the aluminum alloy matrix, the strength and plasticity of the material are significantly improved, and its application prospects are expanded. The process is simple, the equipment requirements are low, and the operability is strong.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004860798130000091
    Figure BDA0004860798130000091
Patent Text Reader

Abstract

The invention discloses an aluminum alloy material and a preparation method thereof, and belongs to the field of aluminum alloy material preparation. According to the aluminum alloy material and the preparation method thereof, the reinforcements are added into the aluminum alloy matrix, so that the prepared aluminum alloy material has excellent strength and plasticity, further the prepared aluminum alloy material has a wider application prospect, and in addition, the preparation process is simple, the requirement for invested equipment is low, and operability is high. Besides, the single-walled carbon nanotubes, the silicon nitride and the silicon carbide are compounded and then subjected to modification treatment, it is guaranteed that the components are evenly dispersed in an aluminum alloy matrix, the strength of the aluminum alloy matrix is obviously enhanced, and by means of the hot rolling and cold rolling combined mode, the strength of the aluminum alloy material is guaranteed, and meanwhile the strength of the aluminum alloy material is improved. The excellent plasticity is also realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of aluminum alloy preparation, and in particular to an aluminum alloy material and a preparation method thereof. Background Art

[0002] With the advancement of science and technology, human beings' requirements for material properties are also increasing. In the field of metal preparation, the trade-off between strength and plasticity of traditional structural materials can no longer meet people's use needs in specific occasions, which makes composite materials extremely important in front-line research. Aluminum has the advantages of large reserves, low density, high specific strength, corrosion resistance, good conductivity, and low price. In particular, the automotive and aerospace industries have focused on reducing the weight of structures in order to improve fuel efficiency and reduce climate change and environmental damage, making the application of aluminum-based composite materials more and more extensive. In the prior art, in order to further improve the strength of aluminum and its alloys to further reduce the weight of structural components, it can be achieved by adding reinforcements. Commonly used reinforcements for aluminum-based composite materials include SiC, Al2O3, graphene, etc. However, when SiC and Al2O3 are directly added as reinforcements in the matrix, the processability of the prepared aluminum-based composite material is low; when graphene is directly added as reinforcement in the matrix, its strength and hardness are significantly improved, but the plasticity and elongation of the prepared aluminum-based composite material are not improved, especially when the content of graphene reaches a certain level, its elongation is reduced compared with the pure matrix, and the plasticity is poor. Therefore, there is a problem that strength and plasticity cannot be taken into account when preparing aluminum-based composite materials in the prior art, which affects its application in the market. Summary of the invention

[0003] Based on this, in order to solve the problem that strength and plasticity cannot be taken into account when preparing aluminum-based composite materials in the prior art, the present invention provides an aluminum alloy material and a preparation method thereof, and the specific technical solution is as follows:

[0004] An aluminum alloy material, comprising an aluminum alloy matrix and a reinforcement, wherein the aluminum alloy matrix comprises the following components in percentage by mass:

[0005] Si 0.1% to 0.6%, Cu 0.01% to 0.03%, Sr 0.1% to 0.5%, Zr 0.02% to 0.07%, Ti 0.03% to 0.2%, Mn 0.01% to 0.06%, Ni 0.1% to 0.3%, the balance is Al and unavoidable impurities;

[0006] According to the mass ratio, the reinforcement is prepared by mixing single-walled carbon nanotubes, silicon nitride and silicon carbide in a mass ratio of (1-7): (1-3): (2-5) and then undergoing a modification treatment; and the added amount of the reinforcement accounts for 0.01% to 15% of the mass percentage of the aluminum alloy material.

[0007] Furthermore, the modification treatment is as follows: single-walled carbon nanotubes, silicon nitride and silicon carbide are mixed, ball-milled at 500 r / min to 1200 r / min for 25 to 45 min, and then the mixture is added to olive, first ultrasonically dispersed, filtered and then the filter cake is added to polyvinyl alcohol, heated to 45°C to 55°C, stirred at a stirring speed of 800 r / min to 1500 r / min for 30 to 45 min, filtered and dried to obtain a reinforcement.

[0008] Furthermore, the solid-liquid ratio of the mixture to olive is (1-5) g / 10 mL.

[0009] Furthermore, the volume ratio of the filter cake to the polyvinyl alcohol is (1-5):(10-15).

[0010] Furthermore, the power of the first ultrasonic dispersion is 400W to 500W, and the time is 30min to 60min.

[0011] In addition, the present invention also provides a method for preparing an aluminum alloy material, the preparation method comprising the following steps:

[0012] The raw materials of the aluminum alloy matrix material and the reinforcement are added to a ball mill and vacuum milled for 1 h to 3 h. During the vacuum milling, the ball milling is performed for 0.5 h, then stopped for 0.5 h, and then the ball milling is continued, and this cycle is repeated to obtain a mixed powder.

[0013] The mixed powder is pre-pressed, sintered and heat-insulated to obtain a blank;

[0014] The billet is subjected to hot rolling and cold rolling to obtain an aluminum alloy material.

[0015] Furthermore, the raw materials are Al-Si alloy powder, Al-Cu alloy powder, Al-Sr alloy powder, Al-Zr alloy powder, Ti powder, Al-Mn alloy powder and Ni powder.

[0016] Furthermore, the sintering treatment is performed at a temperature of 700° C. to 750° C. and for a time of 1 h to 2 h.

[0017] Furthermore, the temperature of the heat preservation treatment is 500° C. to 550° C., and the time is 30 min to 50 min.

[0018] Furthermore, the temperature of the hot rolling treatment is 420° C. to 450° C., and the deformation amount of the hot pressing treatment is 30% to 50%.

[0019] In the above scheme, by adding a reinforcement to the aluminum alloy matrix, the prepared aluminum alloy material has excellent strength and plasticity, and thus the prepared aluminum alloy material has a wider application prospect. Moreover, the preparation process of the present invention is simple, the equipment requirements are low, and the operability is strong. In addition, the present application compounds single-walled carbon nanotubes, silicon nitride and silicon carbide, and then undergoes a modification treatment, which not only ensures the uniform dispersion of the components in the aluminum alloy matrix, but also has a significant strengthening effect on the strength of the aluminum alloy matrix, and through a combination of hot rolling and cold rolling, the aluminum alloy material has excellent plasticity while ensuring strength. DETAILED DESCRIPTION

[0020] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with its embodiments. It should be understood that the specific implementation methods described herein are only used to explain the present invention and do not limit the protection scope of the present invention.

[0021] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0022] An aluminum alloy material in an embodiment of the present invention includes an aluminum alloy matrix and a reinforcement, wherein the aluminum alloy matrix includes the following components in percentage by mass:

[0023] Si 0.1% to 0.6%, Cu 0.01% to 0.03%, Sr 0.1% to 0.5%, Zr 0.02% to 0.07%, Ti 0.03% to 0.2%, Mn 0.01% to 0.06%, Ni 0.1% to 0.3%, the balance is Al and unavoidable impurities;

[0024] According to the mass ratio, the reinforcement is prepared by mixing single-walled carbon nanotubes, silicon nitride and silicon carbide in a mass ratio of (1-7): (1-3): (2-5) and then undergoing a modification treatment; and the added amount of the reinforcement accounts for 0.01% to 15% of the mass percentage of the aluminum alloy material.

[0025] In one embodiment, the modification treatment is: single-walled carbon nanotubes, silicon nitride and silicon carbide are mixed, ball milled at 500r / min~1200r / min for 25min~45min, and then the mixture is added to olive, first ultrasonically dispersed, filtered and then the filter cake is added to polyvinyl alcohol, heated to 45°C~55°C, stirred at a stirring speed of 800r / min~1500r / min for 30min~45min, filtered and dried to obtain a reinforcement.

[0026] In one embodiment, the liquid ratio of the mixture to olive oil is (1-5) g / 10 mL. The van der Waals interaction between the surface groups of the modified reinforcement is reduced, which is helpful for its separation and dispersion in the aluminum alloy matrix. In addition, the surface modification of polyvinyl alcohol makes the carboxyl functionalized, has better compatibility, and significantly improves the overall mechanical properties.

[0027] In one embodiment, the volume ratio of the filter cake to the polyvinyl alcohol is (1-5): (10-15).

[0028] In one embodiment, the power of the first ultrasonic dispersion is 400W to 500W, and the time is 30min to 60min.

[0029] In addition, the present invention also provides a method for preparing an aluminum alloy material, the preparation method comprising the following steps:

[0030] The raw materials of the aluminum alloy matrix material and the reinforcement are added to a ball mill and vacuum milled for 1 h to 3 h. During the vacuum milling, the ball milling is performed for 0.5 h, then stopped for 0.5 h, and then the ball milling is continued, and this cycle is repeated to obtain a mixed powder.

[0031] The mixed powder is pre-pressed, sintered and heat-insulated to obtain a blank;

[0032] The billet is subjected to hot rolling and cold rolling to obtain an aluminum alloy material.

[0033] In one embodiment, the raw materials are Al-Si alloy powder, Al-Cu alloy powder, Al-Sr alloy powder, Al-Zr alloy powder, Ti powder, Al-Mn alloy powder and Ni powder.

[0034] In one embodiment, the ball-to-material ratio of the vacuum ball mill is 10:1.

[0035] In one embodiment, the rotation speed of the vacuum ball mill is 500 r / min to 1000 r / min.

[0036] In one embodiment, the sintering process is performed at a temperature of 700° C. to 750° C. and for a time of 1 h to 2 h.

[0037] In one embodiment, the temperature of the heat preservation treatment is 500° C. to 550° C., and the time is 30 min to 50 min.

[0038] In one embodiment, the temperature of the hot rolling treatment is 420° C. to 450° C., and the deformation amount of the hot pressing treatment is 30% to 50%.

[0039] In one embodiment, the deformation amount of the cold rolling process is 25% to 50%.

[0040] In the above scheme, by adding a reinforcement into the aluminum alloy matrix, the prepared aluminum alloy material has excellent strength and plasticity, and thus the prepared aluminum alloy material has a wider application prospect.

[0041] The embodiments of the present invention will be described in detail below with reference to specific examples.

[0042] Embodiment 1:

[0043] The aluminum alloy material of Example 1 includes an aluminum alloy matrix and a reinforcement, wherein the aluminum alloy matrix includes the following components in percentage by mass:

[0044] Si 0.5%, Cu 0.03%, Sr 0.3%, Zr 0.05%, Ti 0.08%, Mn 0.05%, Ni 0.2%, reinforcement 8%, the balance is Al and unavoidable impurities;

[0045] The method for preparing the aluminum alloy material in Example 1 comprises the following steps:

[0046] After mixing single-walled carbon nanotubes, silicon nitride and silicon carbide in a mass ratio of 7:3:2, ball milling was performed at 800 r / min for 30 min, and then the mixture was added to olive at 3 g / 10 mL, and the first ultrasonic dispersion was performed at a power of 400 W for 40 min. After filtration, the filter cake was added to polyvinyl alcohol at a volume ratio of 3:10, heated to 45°C, stirred at a stirring speed of 1000 r / min for 40 min, filtered and dried to obtain a reinforcement for standby use;

[0047] Al-Si alloy powder, Al-Cu alloy powder, Al-Sr alloy powder, Al-Zr alloy powder, Ti powder, Al-Mn alloy powder, Ni powder and the reinforcement are added into a ball mill, and the ball-to-material ratio in the ball mill is 10:1, and vacuum ball milling is performed at a speed of 600 r / min for 3 hours. During the vacuum ball milling, the powder is milled for 0.5 hours, stopped for 0.5 hours, and then the powder is continued, and a mixed powder is obtained by this cycle;

[0048] The mixed powder is pre-pressed, then sintered at 700° C. for 1 hour, and then heat-treated at 500° C. for 40 minutes to obtain a blank;

[0049] The billet is hot rolled at 420° C. with a deformation amount of 40%, and then cold rolled with a deformation amount of 30% to obtain an aluminum alloy material.

[0050] Embodiment 2:

[0051] The aluminum alloy material of Example 2 includes an aluminum alloy matrix and a reinforcement, wherein the aluminum alloy matrix includes the following components in percentage by mass:

[0052] Si 0.6%, Cu 0.02%, Sr 0.5%, Zr 0.06%, Ti 0.09%, Mn 0.04%, Ni 0.3%, reinforcement 10%, the balance is Al and unavoidable impurities;

[0053] The method for preparing the aluminum alloy material in Example 2 comprises the following steps:

[0054] After mixing single-walled carbon nanotubes, silicon nitride and silicon carbide in a mass ratio of 7:3:2, ball milling was performed at 900 r / min for 40 min, and then the mixture was added to olive at 3 g / 10 mL, and the first ultrasonic dispersion was performed at a power of 500 W for 30 min. After filtration, the filter cake was added to polyvinyl alcohol at a volume ratio of 3:10, heated to 45°C, stirred at a stirring speed of 1000 r / min for 45 min, filtered and dried to obtain a reinforcement for standby use;

[0055] Al-Si alloy powder, Al-Cu alloy powder, Al-Sr alloy powder, Al-Zr alloy powder, Ti powder, Al-Mn alloy powder, Ni powder and the reinforcement are added into a ball mill, and the ball-to-material ratio in the ball mill is 10:1, and vacuum ball milling is performed at a speed of 800 r / min for 3 hours, and during the vacuum ball milling process, the ball milling is performed for 0.5 hours, and then stopped for 0.5 hours, and then the ball milling is continued, and this cycle is repeated to obtain a mixed powder;

[0056] The mixed powder is pre-pressed, then sintered at 720° C. for 1 hour, and then heat-treated at 520° C. for 45 minutes to obtain a blank;

[0057] The billet is hot rolled at 450° C. with a deformation amount of 50%, and then cold rolled with a deformation amount of 30% to obtain an aluminum alloy material.

[0058] Embodiment 3:

[0059] The aluminum alloy material of Example 3 includes an aluminum alloy matrix and a reinforcement, wherein the aluminum alloy matrix includes the following components in percentage by mass:

[0060] Si 0.6%, Cu 0.03%, Sr 0.5%, Zr 0.07%, Ti 0.05%, Mn 0.06%, Ni 0.1%, reinforcement 12%, the balance is Al and unavoidable impurities;

[0061] The method for preparing the aluminum alloy material in Example 3 comprises the following steps:

[0062] After mixing single-walled carbon nanotubes, silicon nitride and silicon carbide in a mass ratio of 7:1:4, ball milling was performed at 800 r / min for 45 min, and then the mixture was added to olive at 3 g / 10 mL, and the first ultrasonic dispersion was performed at a power of 500 W for 50 min. After filtration, the filter cake was added to polyvinyl alcohol at a volume ratio of 3:10, heated to 55°C, stirred at a stirring speed of 800 r / min5 for 30 min, filtered and dried to obtain a reinforcement for standby use;

[0063] Al-Si alloy powder, Al-Cu alloy powder, Al-Sr alloy powder, Al-Zr alloy powder, Ti powder, Al-Mn alloy powder, Ni powder and the reinforcement are added into a ball mill, and the ball-to-material ratio in the ball mill is 10:1, and vacuum ball milling is performed at a speed of 1000 r / min for 3 hours, and during the vacuum ball milling process, the ball milling is performed for 0.5 hours, and then stopped for 0.5 hours, and then the ball milling is continued, and this cycle is repeated to obtain a mixed powder;

[0064] The mixed powder is pre-pressed, then sintered at 750° C. for 1 hour, and then heat-treated at 550° C. for 30 minutes to obtain a blank;

[0065] The billet is hot rolled at 450° C. with a deformation amount of 40%, and then cold rolled with a deformation amount of 40% to obtain an aluminum alloy material.

[0066] Comparative Example 1:

[0067] The difference between Comparative Example 1 and Example 3 is that no reinforcement is added in Comparative Example 1, and the rest is the same as Example 3.

[0068] Comparative Example 2:

[0069] The difference between Comparative Example 2 and Example 3 is that the reinforcement in Comparative Example 2 is not modified, and the rest is the same as Example 3.

[0070] Comparative Example 3:

[0071] The difference between Comparative Example 3 and Example 3 is that a single single-walled carbon nanotube is used in Comparative Example 3, and the rest is the same as Example 3.

[0072] Comparative Example 4:

[0073] The difference between Comparative Example 4 and Example 3 is that a single silicon nitride is used in Comparative Example 4, and the rest is the same as Example 3.

[0074] Comparative Example 5:

[0075] The difference between Comparative Example 5 and Example 3 is that a single silicon carbide is used in Comparative Example 5, and the rest is the same as Example 3.

[0076] Comparative Example 6:

[0077] The difference between Comparative Example 6 and Example 3 is that the reinforcement in Comparative Example 6 is a conventional carbon nanotube.

[0078] Comparative Example 7:

[0079] The difference between Comparative Example 7 and Example 3 is that the modification method in Comparative Example 7 is as follows, and the rest is the same as Example 3.

[0080] Single-walled carbon nanotubes, silicon nitride and silicon carbide were mixed in a mass ratio of 7:1:4, ball-milled at 800 r / min for 45 min, then directly added to polyvinyl alcohol at a volume ratio of 3:10, heated to 55°C, stirred at a stirring speed of 800 r / min for 30 min, filtered and dried to obtain a reinforcement for use.

[0081] Comparative Example 8:

[0082] The difference between Comparative Example 8 and Example 3 is that the amount of reinforcement added in Comparative Example 8 accounts for 20% of the aluminum alloy material, and the rest is the same as Example 3.

[0083] Comparative Example 9:

[0084] The difference between Comparative Example 9 and Example 3 is that Comparative Example 9 is not subjected to heat preservation treatment, and the rest is the same as Example 3.

[0085] Comparative Example 10:

[0086] The difference between Comparative Example 10 and Example 3 is that Comparative Example 10 is not subjected to hot rolling treatment, and the rest is the same as Example 3.

[0087] The samples of Examples 1 to 3 and the comparative samples of Comparative Examples 1 to 10 were subjected to performance tests, and the results are shown in Table 1. The tensile strength refers to the room temperature tensile test of metal materials in GB / T228-2002.

[0088] Table 1: Performance test results

[0089]

[0090]

[0091] From the data analysis of Table 1, it can be seen that the present application can obtain an aluminum alloy material with excellent tensile strength and elongation at break by optimizing the composition and component ratio of the reinforcement and modifying the reinforcement. From the comparative analysis of Comparative Examples 1 to 10 and Example 3, it can be seen that the present application not only has a positive effect on the technical effect in terms of composition and component ratio, but also promotes the acquisition of the high-strength and high-plasticity aluminum alloy material of the present application in terms of process.

[0092] In addition, the aluminum alloy material of the present application was die-cast into parts, and there were 100 experimental products with a pass rate of 100%. The surface was flat and crack-free, and generally, products with composite appearance quality requirements were obtained.

[0093] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0094] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. An aluminum alloy material, comprising an aluminum alloy matrix and a reinforcement, characterized in that: The aluminum alloy matrix includes the following components in percentage by mass: Si 0.1%~0.6%, Cu 0.01%~0.03%, Sr 0.1%~0.5%, Zr 0.02%~0.07%, Ti0.03%~0.2%, Mn 0.01%~0.06%, Ni 0.1%~0.3%, the balance is Al and unavoidable impurities; According to the mass ratio, the reinforcement is prepared by mixing single-walled carbon nanotubes, silicon nitride and silicon carbide in a mass ratio of (1-7): (1-3): (2-5) and then undergoing a modification treatment; and the added amount of the reinforcement accounts for 0.01% to 15% of the mass percentage of the aluminum alloy material.

2. The aluminum alloy material according to claim 1, characterized in that: The modification treatment is as follows: single-walled carbon nanotubes, silicon nitride and silicon carbide are mixed, ball-milled for 25 to 45 minutes at 500 to 1200 r / min, and then the mixture is added to olives, first subjected to ultrasonic dispersion, filtered, and then the filter cake is added to polyvinyl alcohol, heated to 45 to 55° C., stirred for 30 to 45 minutes at a stirring speed of 800 to 1500 r / min, filtered, and dried to obtain a reinforcement.

3. The aluminum alloy material according to claim 2, characterized in that: The solid-liquid ratio of the mixture to olive is (1-5) g / 10 mL.

4. The aluminum alloy material according to claim 2, characterized in that: The volume ratio of the filter cake to the polyvinyl alcohol is (1-5):(10-15).

5. The aluminum alloy material according to claim 2, characterized in that: The power of the first ultrasonic dispersion is 400W to 500W, and the time is 30min to 60min.

6. A method for preparing an aluminum alloy material, characterized in that: The preparation method is used to prepare the aluminum alloy material according to any one of claims 1 to 5, and the preparation method comprises the following steps: The raw materials of the aluminum alloy matrix material and the reinforcement are added to a ball mill and vacuum milled for 1 h to 3 h. During the vacuum milling, the ball milling is performed for 0.5 h, then stopped for 0.5 h, and then the ball milling is continued, and this cycle is repeated to obtain a mixed powder. The mixed powder is pre-pressed, sintered and heat-insulated to obtain a blank; The billet is subjected to hot rolling and cold rolling to obtain an aluminum alloy material.

7. The preparation method according to claim 6, characterized in that: The raw materials are Al-Si alloy powder, Al-Cu alloy powder, Al-Sr alloy powder, Al-Zr alloy powder, Ti powder, Al-Mn alloy powder and Ni powder.

8. The preparation method according to claim 6, characterized in that: The sintering treatment is carried out at a temperature of 700° C. to 750° C. and for a time of 1 h to 2 h.

9. The preparation method according to claim 6, characterized in that: The temperature of the insulation treatment is 500°C to 550°C, and the time is 30min to 50min.

10. The preparation method according to claim 6, characterized in that: The temperature of the hot rolling treatment is 420°C to 450°C, and the deformation amount of the hot pressing treatment is 30% to 50%.