Aluminum alloy powder, additive manufacturing aluminum alloy and preparation method of additive manufacturing aluminum alloy
By adjusting the mass ratio of Mg, Li, Ga, Si, Zn, Sn and other elements in the aluminum alloy powder, and using laser cladding technology, the problem of high ignition point and low combustion value of existing aluminum alloy materials in laser additive molding has been solved. solve the problem, realize the low ignition point and high combustion value characteristics of the aircraft fuel bracket, and support the reuse of fuel carriers.
Patent Information
- Application Number
- CN202410981886.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-10-01
AI Technical Summary
Existing aluminum alloy materials cannot meet the needs of low ignition point and high combustion value in laser additive molding, especially in the design of fuel propellant brackets and thruster recycling in the aerospace field.
Provide an aluminum alloy powder containing Mg, Li, Ga, Si, Zn, Sn and other elements. Through a specific mass ratio and preparation method, the strength and ductility of the material are improved, and the aluminum alloy powder is formed through laser cladding technology. Reduces ignition point and increases combustion value, suitable for laser additive manufacturing.
It realizes that the aluminum alloy powder is basically burned out after the aircraft is ignited, supports the repeated filling and use of aircraft fuel carriers, improves the combustion value and strength of the material, and meets the low ignition point requirements.
Smart Images

Figure CN118726804A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of alloys, and in particular to an aluminum alloy powder, an additively manufactured aluminum alloy and a preparation method thereof. Background Art
[0002] With the development of additive manufacturing applications, more and more difficult application problems have been solved. In the field of aerospace, the design of fuel propellant brackets plays a vital role in the combination diversity of fuel and the recycling and reuse of thrusters. The development of laser additive manufacturing technology provides a broader idea for the design side and provides a good solution for the liberation of design freedom.
[0003] Among the existing aluminum alloy materials, only some Al-Si and Al-Mg alloys can be used for laser additive manufacturing. Although they have excellent performance, none of the existing materials can meet the special requirements of combustion. Therefore, it is urgent to develop a printable aluminum alloy material with low ignition point and high combustion value. Summary of the invention
[0004] In view of the shortcomings of the prior art, the purpose of the present invention is to provide an aluminum alloy powder, an additively manufactured aluminum alloy and a preparation method thereof, aiming to solve the technical problem that Al-Si alloy and Al-Mg alloy formed by laser additive manufacturing in the prior art cannot meet the requirements of low ignition point and high combustion value.
[0005] The first aspect of the present invention is to provide an aluminum alloy powder, which comprises the following components by mass percentage:
[0006] Mg: 1.0wt%~4.0wt%, Li: 0.5wt%~2.0wt%, Ga: 0.8wt%~2.0wt%, Si: 0.3wt%~1.0wt%, Zn: 0.5wt%~1.0wt%, Sn: 0.8wt%~2.0wt%, the balance is Al;
[0007] Among them, the mass ratio of Mg to Li is (1-3):1.
[0008] Compared with the prior art, the beneficial effect of the present invention lies in that: the aluminum alloy powder provided by the present invention, specifically, the aluminum alloy powder comprises the following components by mass percentage: Mg: 1.0wt%~4.0wt%, Li: 0.5wt%~2.0wt%, Ga: 0.8wt%~2.0wt%, Si: 0.3wt%~1.0wt%, Zn: 0.5wt%~1.0wt%, Sn: 0.8wt%~2.0wt%, and the balance is Al; wherein the mass ratio of Mg to Li is (1~3):1, and the strength and ductility of the aluminum alloy are improved by setting the ratio of the aluminum alloy powder, and the material density and the ignition point are reduced, and the combustion value of the material is improved, and the fuel bracket printed and formed using the powder can be basically burned out after the aircraft is ignited, thereby realizing repeated filling and use of the aircraft fuel carrier, thereby solving the technical problem that the Al-Si alloy and Al-Mg alloy formed by laser additive manufacturing in the prior art cannot meet the requirements of low ignition point and high combustion value.
[0009] According to one aspect of the above technical solution, the raw material of the aluminum alloy powder includes an alloy rod made of any one or any combination of aluminum-magnesium alloy, aluminum-lithium alloy, aluminum-gallium alloy, aluminum-silicon alloy, aluminum-zinc alloy, and aluminum-tin alloy.
[0010] According to one aspect of the above technical solution, the size of the alloy rod is 300 mm to 600 mm.
[0011] A second aspect of the present invention is to provide a method for preparing an aluminum alloy powder, wherein the method is used to prepare the above-mentioned aluminum alloy powder, and the method comprises:
[0012] Weighing alloy rods of a preset ratio, dividing the alloy rods into first alloy rods of a first preset ratio and second alloy rods of a second preset ratio, placing the first alloy rods in a smelting device, introducing inert gas to atmospheric pressure when the vacuum degree reaches below the preset vacuum degree, and preheating at a preheating temperature for a preset time;
[0013] At the preset melting temperature, the alloy droplets are melted and dripped vertically into the central liquid guide tube of the atomizing disk. Under the action of the atomizing gas pressure, they are ejected at high speed from the annular gap of the atomizing disk and broken into metal droplets.
[0014] The metal droplets are cooled and solidified to form original powder, and the original powder is classified and dried to obtain primary powder;
[0015] The second alloy rod is crushed and ball-milled into a second spherical alloy powder, and then the second spherical alloy powder is laser-clad on the primary powder to obtain aluminum alloy powder.
[0016] According to one aspect of the above technical solution, the preset vacuum degree is 60Pa, the preheating temperature is 300°C to 450°C, the preset time is 20min to 40min, the preset melting temperature is 750°C to 950°C, and the atomizing gas is an inert gas.
[0017] According to one aspect of the above technical solution, the annular seam air outlet angle of the atomizing disk is less than 37°.
[0018] According to one aspect of the above technical solution, the alloy rod of the first preset ratio includes: Mg: 1.0wt% to 4.0wt%, Li: 0.5wt% to 2.0wt%, Ga: 0.8wt% to 2.0wt%, Si: 0.3wt% to 1.0wt%, Zn: 0.1wt% to 0.5wt%, Sn: 0.8wt% to 2.0wt%;
[0019] The alloy rod of the second preset ratio includes: Zn: 0.2wt% to 0.7wt%.
[0020] A third aspect of the present invention is to provide an additively manufactured aluminum alloy, wherein the additively manufactured aluminum alloy comprises the above-mentioned aluminum alloy powder.
[0021] A fourth aspect of the present invention is to provide a method for preparing an additively manufactured aluminum alloy, wherein the method for preparing an additively manufactured aluminum alloy is used to prepare the above-mentioned additively manufactured aluminum alloy, and the method comprises:
[0022] Aluminum alloy powder is used as printing material and input into the preset fiber laser SLM printer. After printing, annealing, wire cutting and surface treatment, additively manufactured aluminum alloy is obtained.
[0023] According to one aspect of the above technical solution, the preheating temperature of the fiber laser SLM printer is 10°C to 75°C, the laser power is 150W to 220W, the scanning speed of the fiber laser SLM printer is 800mm / s to 1300mm / s, the scanning spacing is 0.15mm to 0.5mm, the scanning layer thickness is 0.03mm to 0.06mm, and the area overlap is set to 0.19mm. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0025] Figure 1 The present invention is a flow chart of the method for preparing aluminum alloy powder. DETAILED DESCRIPTION
[0026] In order to make the purpose, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the accompanying drawings. Several embodiments of the present invention are shown in the accompanying drawings. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thorough and comprehensive.
[0027] It should be noted that when an element is referred to as being "fixed to" another element, it may be directly on the other element or there may be a central element. When an element is considered to be "connected to" another element, it may be directly connected to the other element or there may be a central element at the same time. The terms "vertical", "horizontal", "left", "right", "upper", "lower" and similar expressions used herein are for illustrative purposes only and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as limiting the present invention.
[0028] In the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be internal communication between two components. For those of ordinary skill in the art, the specific meanings of the above terms in the present invention can be understood according to the specific circumstances. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0029] The present invention provides an aluminum alloy powder, which comprises the following components by mass percentage:
[0030] Mg: 1.0wt%~4.0wt%, Li: 0.5wt%~2.0wt%, Ga: 0.8wt%~2.0wt%, Si: 0.3wt%~1.0wt%, Zn: 0.5wt%~1.0wt%, Sn: 0.8wt%~2.0wt%, the balance is Al;
[0031] Preferably, the mass percentage of Mg is 1.0wt% to 4.0wt%, for example, 1.0wt%, 1.5wt%, 2.0wt%, 2.5wt%, 3.0wt%, 3.5wt% or 4.0wt%, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0032] Preferably, the mass percentage of Li is 0.5wt% to 2.0wt%, for example, 0.5wt%, 1.0wt%, 1.5wt% or 2.0wt%, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0033] Preferably, the mass percentage of Ga is 0.8wt% to 2.0wt%, for example, it can be 0.8wt%, 1.0wt%, 1.2wt%, 1.4wt%, 1.6wt%, 1.8wt% or 2.0wt%, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0034] Preferably, the mass percentage of Si is 0.3wt% to 1.0wt%, for example, it can be 0.3wt%, 0.4wt%, 0.5wt%, 0.6wt%, 0.7wt%, 0.8wt%, 0.9wt% or 1.0wt%, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0035] Preferably, the mass percentage of Zn is 0.5wt% to 1.0wt%, for example, 0.5wt%, 0.6wt%, 0.7wt%, 0.8wt%, 0.9wt% or 1.0wt%, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0036] Preferably, the mass percentage of Sn is 0.8wt% to 2.0wt%, for example, 0.8wt%, 1.0wt%, 1.2wt%, 1.4wt%, 1.6wt%, 1.8wt% or 2.0wt%, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0037] Furthermore, the mass ratio of Mg to Li is (1-3): 1. For example, it can be 1: 1, 2: 1 or 3: 1, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0038] It should be noted that by setting the ratio of aluminum alloy powder, the strength and ductility of aluminum alloy are improved, the material density is reduced, the ignition point is reduced, the combustion value of the material is improved, and the fuel bracket printed by using the powder can be basically burned out after the aircraft is ignited, so that the aircraft fuel carrier can be repeatedly loaded and used. The excellent performance of the material is mainly achieved by rapid cooling during the material forming process to break through the solid solution limit of the material, and the purpose of stable material forming and reduced ignition point is achieved by the combination of multiple strengthening phases such as Mg2Si, Al3Li, AlZn2, Al3Ga5, and AlSn2.
[0039] In addition, the present invention provides a method for preparing aluminum alloy powder, which is used to prepare the above-mentioned aluminum alloy powder. The preparation method comprises: steps S10-S13,
[0040] Step S10, weighing alloy rods of a preset ratio, dividing the alloy rods into first alloy rods of a first preset ratio and second alloy rods of a second preset ratio, placing the first alloy rods in a smelting device, introducing inert gas to atmospheric pressure when the vacuum degree reaches below the preset vacuum degree, and preheating at a preheating temperature for a preset time;
[0041] Among them, the preheating temperature is 300℃~450℃, and the preset time is 20min~40min. Generally, the density and physical properties of the materials are different. When they are melted at the preset high temperature in an instant, large gaps will be formed between the materials, making it difficult to form uniform molten metal droplets by subsequent atomization. Therefore, it is necessary to preheat the first alloy rod for a preset time to reduce the resistance between the materials and the gaps, thereby increasing the density of the molten metal droplets and improving the uniformity.
[0042] Step S11, melting alloy droplets at a preset melting temperature, vertically dripping into the central liquid guide tube of the atomizing disk, and ejecting them from the annular gap of the atomizing disk at high speed under the action of the atomizing gas pressure, breaking into metal droplets;
[0043] Step S12, cooling and solidifying the metal droplets to form original powder, and classifying and drying the original powder to obtain primary powder;
[0044] Step S13, crushing and ball-milling the second alloy rod into second spherical alloy powder, and then laser cladding the second spherical alloy powder on the primary powder to obtain aluminum alloy powder.
[0045] Preferably, the preset vacuum degree is 60 Pa, the preset melting temperature is 750° C. to 950° C., and the atomizing gas is an inert gas.
[0046] Preferably, the annular gap gas outlet angle of the atomizing disk is less than 37°, so that the metal molten droplets are broken into smaller and finer ones, thereby improving the performance of the aluminum alloy powder.
[0047] Further, the alloy rod of the first preset ratio includes: Mg: 1.0wt% to 4.0wt%, Li: 0.5wt% to 2.0wt%, Ga: 0.8wt% to 2.0wt%, Si: 0.3wt% to 1.0wt%, Zn: 0.1wt% to 0.5wt%, Sn: 0.8wt% to 2.0wt%;
[0048] The alloy rod of the second preset ratio includes: Zn: 0.2wt% to 0.7wt%.
[0049] It should be noted that by adding the Zn element separately, the thermal cracking tendency of the aluminum alloy powder caused by the increase of the Zn element content is effectively suppressed, so that the performance of the aluminum alloy powder is improved.
[0050] Furthermore, the present invention also provides an additively manufactured aluminum alloy, which includes the above-mentioned aluminum alloy powder.
[0051] In addition, the present invention also provides a method for preparing an additively manufactured aluminum alloy, which is used to prepare the above-mentioned additively manufactured aluminum alloy, and the preparation method comprises:
[0052] Aluminum alloy powder is used as printing material and input into the preset fiber laser SLM printer. After printing, annealing, wire cutting and surface treatment, additively manufactured aluminum alloy is obtained.
[0053] Furthermore, the preheating temperature of the fiber laser SLM printer is 10°C to 75°C, for example, 10°C, 20°C, 30°C, 40°C, 50°C, 60°C, 70°C or 75°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0054] Furthermore, the laser power of the fiber laser SLM printer is 150W to 220W, for example, 150W, 160W, 170W, 180W, 190W, 200W, 210W or 220W, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0055] Furthermore, the scanning speed of the fiber laser SLM printer is 800 mm / s to 1300 mm / s, for example, 800 mm / s, 900 mm / s, 1000 mm / s, 1100 mm / s, 1200 mm / s or 1300 mm / s, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0056] Furthermore, the scanning pitch of the fiber laser SLM printer is 0.15 mm to 0.5 mm, for example, 0.15 mm, 0.2 mm, 0.25 mm, 0.3 mm, 0.35 mm, 0.4 mm, 0.45 mm or 0.5 mm, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0057] Preferably, the scanning layer thickness of the fiber laser SLM printer is 0.03 mm to 0.06 mm, for example, 0.03 mm, 0.04 mm, 0.05 mm or 0.06 mm, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0058] Preferably, the area overlap of the fiber laser SLM printer is set to 0.19 mm.
[0059] Among them, the addition of low-melting-point components forms a strengthening phase with the aluminum matrix to ensure the material's forming performance; a large number of low-melting-point components are free in the matrix, which greatly reduces the material's ignition point while increasing the material's combustion value, making it combustible and burnable. In addition, the interaction of various elements in the multi-element alloy is achieved through the 3D printing method, and the rapid cooling technology is fully utilized to increase the material's solid solution limit, providing a lightweight solution for a combustible complex structure fuel bracket, which can greatly improve the energy efficiency of the fuel tank.
[0060] The present invention is further described below with specific embodiments:
[0061] Embodiment 1
[0062] The aluminum alloy powder provided in the first embodiment of the present invention comprises the following components by mass percentage:
[0063] Mg: 1.0wt%~4.0wt%, Li: 0.5wt%~2.0wt%, Ga: 0.8wt%~2.0wt%, Si: 0.3wt%~1.0wt%, Zn: 0.5wt%~1.0wt%, Sn: 0.8wt%~2.0wt%, the balance is Al;
[0064] Among them, the mass ratio of Mg to Li is (1-3):1.
[0065] Preferably, the mass ratio of Mg to Li is 2:1.
[0066] Preferably, Mg: 3.0wt%, Li: 1.5wt%, Ga: 1.0wt%, Si: 0.5wt%, Zn: 0.7wt%, Sn: 1.5wt%, and the balance is Al.
[0067] Also, see Figure 1 , which is a method for preparing an aluminum alloy powder provided by the present invention. The method for preparing an aluminum alloy powder is used to prepare the above-mentioned aluminum alloy powder. The preparation method comprises: steps S10-S13,
[0068] Step S10, weighing alloy rods of a preset ratio, dividing the alloy rods into first alloy rods of a first preset ratio and second alloy rods of a second preset ratio, placing the first alloy rods in a smelting device, introducing inert gas to atmospheric pressure when the vacuum degree reaches below the preset vacuum degree, and preheating at a preheating temperature for a preset time;
[0069] Preferably, the preheating temperature is 400° C. and the preset time is 30 minutes.
[0070] Step S11, melting alloy droplets at a preset melting temperature, vertically dripping into the central liquid guide tube of the atomizing disk, and ejecting them from the annular gap of the atomizing disk at high speed under the action of the atomizing gas pressure, breaking into metal droplets;
[0071] Step S12, cooling and solidifying the metal droplets to form original powder, and classifying and drying the original powder to obtain primary powder;
[0072] Step S13, crushing and ball-milling the second alloy rod into second spherical alloy powder, and then laser cladding the second spherical alloy powder on the primary powder to obtain aluminum alloy powder.
[0073] The alloy rod of the first preset ratio includes: Mg: 3.0wt%, Li: 1.5wt%, Ga: 1.0wt%, Si: 0.5wt%, Zn: 0.3wt%, Sn: 1.5wt%, Al: 91.0wt%.
[0074] The alloy rod of the second preset ratio includes: Zn: 0.4wt%, Al: 0.8wt%.
[0075] Preferably, the preset vacuum degree is 60 Pa, the preset melting temperature is 750° C., and the atomizing gas is an inert gas.
[0076] Preferably, the annular gap of the atomizing disk has an air outlet angle less than 37°.
[0077] Furthermore, this embodiment also provides an additively manufactured aluminum alloy, wherein the additively manufactured aluminum alloy includes the above-mentioned aluminum alloy powder.
[0078] In addition, this embodiment also provides a method for preparing an additively manufactured aluminum alloy, which is used to prepare the above-mentioned additively manufactured aluminum alloy, and the preparation method comprises:
[0079] Aluminum alloy powder is used as printing material and input into the preset fiber laser SLM printer. After printing, annealing, wire cutting and surface treatment, additively manufactured aluminum alloy is obtained.
[0080] Furthermore, the preheating temperature of the fiber laser SLM printer is 10° C., the laser power is 180 W, the scanning speed is 800 mm / s, the scanning pitch is 0.5 mm, the scanning layer thickness is 0.03 mm, and the area overlap is set to 0.19 mm.
[0081] Embodiment 2
[0082] The second embodiment of the present invention provides an aluminum alloy powder. The aluminum alloy powder in this embodiment is different from the aluminum alloy powder in the first embodiment in that:
[0083] The mass ratio of Mg to Li is 1:1.
[0084] Among them, Mg: 3.0wt%, Li: 3.0wt%, Ga: 1.0wt%, Si: 0.5wt%, Zn: 0.7wt%, Sn: 1.5wt%, and the balance is Al.
[0085] Embodiment 3
[0086] The third embodiment of the present invention provides an aluminum alloy powder. The aluminum alloy powder in this embodiment is different from the aluminum alloy powder in the first embodiment in that:
[0087] The mass ratio of Mg to Li is 3:1.
[0088] Among them, Mg: 3.0wt%, Li: 1.0wt%, Ga: 1.0wt%, Si: 0.5wt%, Zn: 0.7wt%, Sn: 1.5wt%, and the balance is Al.
[0089] Embodiment 4
[0090] The fourth embodiment of the present invention provides an aluminum alloy powder. The aluminum alloy powder in this embodiment is different from the aluminum alloy powder in the first embodiment in that:
[0091] Mg: 3.0wt%, Li: 1.5wt%, Ga: 2.0wt%, Si: 1.0wt%, Zn: 1.0%, Sn: 2.0wt%, and the balance is Al.
[0092] Embodiment 5
[0093] The fifth embodiment of the present invention provides an aluminum alloy powder. The aluminum alloy powder in this embodiment is different from the aluminum alloy powder in the first embodiment in that:
[0094] Mg: 3.0wt%, Li: 1.5wt%, Ga: 0.8wt%, Si: 0.3wt%, Zn: 0.5%, Sn: 0.8wt%, and the balance is Al.
[0095] Embodiment 6
[0096] The sixth embodiment of the present invention provides an aluminum alloy powder. The aluminum alloy powder in this embodiment is different from the aluminum alloy powder in the first embodiment in that:
[0097] Mg: 3.0wt%, Li: 1.5wt%, Ga: 1.5wt%, Si: 0.7wt%, Zn: 0.9%, Sn: 1.0wt%, and the balance is Al.
[0098] Embodiment 7
[0099] The seventh embodiment of the present invention provides a method for preparing an aluminum alloy by additive manufacturing. The method for preparing an aluminum alloy by additive manufacturing in this embodiment is different from the method for preparing an aluminum alloy by additive manufacturing in the first embodiment in that:
[0100] The preheating temperature of the fiber laser SLM printer is 40°C.
[0101] Embodiment 8
[0102] The eighth embodiment of the present invention provides a method for preparing an aluminum alloy by additive manufacturing. The method for preparing an aluminum alloy by additive manufacturing in this embodiment is different from the method for preparing an aluminum alloy by additive manufacturing in the first embodiment in that:
[0103] The preheating temperature of the fiber laser SLM printer is 75°C.
[0104] Embodiment 9
[0105] The ninth embodiment of the present invention provides a method for preparing an aluminum alloy by additive manufacturing. The method for preparing an aluminum alloy by additive manufacturing in this embodiment is different from the method for preparing an aluminum alloy by additive manufacturing in the first embodiment in that:
[0106] The laser power is 150W.
[0107] Embodiment 10
[0108] The tenth embodiment of the present invention provides a method for preparing an aluminum alloy by additive manufacturing. The method for preparing an aluminum alloy by additive manufacturing in this embodiment is different from the method for preparing an aluminum alloy by additive manufacturing in the first embodiment in that:
[0109] The laser power is 220W.
[0110] Embodiment 11
[0111] The eleventh embodiment of the present invention provides a method for preparing an aluminum alloy by additive manufacturing. The method for preparing an aluminum alloy by additive manufacturing in this embodiment is different from the method for preparing an aluminum alloy by additive manufacturing in the first embodiment in that:
[0112] The scanning speed is 1000mm / s.
[0113] Embodiment 12
[0114] The twelfth embodiment of the present invention provides a method for preparing an aluminum alloy by additive manufacturing. The method for preparing an aluminum alloy by additive manufacturing in this embodiment is different from the method for preparing an aluminum alloy by additive manufacturing in the first embodiment in that:
[0115] The scanning speed is 1300mm / s.
[0116] Embodiment 13
[0117] The thirteenth embodiment of the present invention provides a method for preparing an aluminum alloy by additive manufacturing. The method for preparing an aluminum alloy by additive manufacturing in this embodiment is different from the method for preparing an aluminum alloy by additive manufacturing in the first embodiment in that:
[0118] The scanning interval is 0.15 mm.
[0119] Embodiment 14
[0120] The fourteenth embodiment of the present invention provides a method for preparing an aluminum alloy by additive manufacturing. The method for preparing an aluminum alloy by additive manufacturing in this embodiment is different from the method for preparing an aluminum alloy by additive manufacturing in the first embodiment in that:
[0121] The scanning interval is 0.3 mm.
[0122] Embodiment 15
[0123] The fifteenth embodiment of the present invention provides a method for preparing an aluminum alloy by additive manufacturing. The method for preparing an aluminum alloy by additive manufacturing in this embodiment is different from the method for preparing an aluminum alloy by additive manufacturing in the first embodiment in that:
[0124] The scanning layer thickness is 0.06 mm.
[0125] Please refer to the following Table 1, which shows the parameters corresponding to the above-mentioned Embodiments 1 to 15 of the present invention.
[0126] Table 1
[0127]
[0128]
[0129]
[0130] Combined with the data of Example 1 to Example 15, it can be seen that the addition of low-melting point components forms a strengthening phase with the aluminum matrix to ensure the material's forming performance; a large number of low-melting point components are free in the matrix, which greatly reduces the material's ignition point while improving the material's combustion value, making it combustible and burnable. In addition, the interaction of the elements in the multi-element alloy is achieved through the 3D printing method, and the rapid cooling technology is fully utilized to improve the solid solution limit of the material, providing a combustible complex structure fuel bracket lightweight solution, which can greatly improve the fuel tank energy efficiency.
[0131] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.
[0132] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that, for those of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. An aluminum alloy powder, characterized in that: Calculated by mass percentage, it includes the following components: Mg: 1.0wt%~4.0wt%, Li: 0.5wt%~2.0wt%, Ga: 0.8wt%~2.0wt%, Si: 0.3wt%~1.0wt%, Zn: 0.5wt%~1.0wt%, Sn: 0.8wt%~2.0wt%, the balance is Al; Among them, the mass ratio of Mg to Li is (1-3):
1.
2. The aluminum alloy powder according to claim 1, characterized in that The raw material of the aluminum alloy powder includes an alloy rod made of any one or any combination of aluminum-magnesium alloy, aluminum-lithium alloy, aluminum-gallium alloy, aluminum-silicon alloy, aluminum-zinc alloy, and aluminum-tin alloy.
3. The aluminum alloy powder according to claim 2, characterized in that The size of the alloy rod is 300 mm to 600 mm.
4. A method for preparing aluminum alloy powder, characterized in that: The preparation method is used to prepare the aluminum alloy powder according to any one of claims 1 to 3, and the preparation method comprises: Weighing alloy rods of a preset ratio, dividing the alloy rods into first alloy rods of a first preset ratio and second alloy rods of a second preset ratio, placing the first alloy rods in a smelting device, introducing inert gas to atmospheric pressure when the vacuum degree reaches below the preset vacuum degree, and preheating at a preheating temperature for a preset time; At the preset melting temperature, the alloy droplets are melted and dripped vertically into the central liquid guide tube of the atomizing disk. Under the action of the atomizing gas pressure, they are ejected at high speed from the annular gap of the atomizing disk and broken into metal droplets. The metal droplets are cooled and solidified to form original powder, and the original powder is classified and dried to obtain primary powder; The second alloy rod is crushed and ball-milled into a second spherical alloy powder, and then the second spherical alloy powder is laser-clad on the primary powder to obtain aluminum alloy powder.
5. The method for preparing aluminum alloy powder according to claim 4, characterized in that: The preset vacuum degree is 60 Pa, the preheating temperature is 300° C. to 450° C., the preset time is 20 min to 40 min, the preset melting temperature is 750° C. to 950° C., and the atomizing gas is an inert gas.
6. The method for preparing aluminum alloy powder according to claim 4, characterized in that: The annular seam gas outlet angle of the atomizing disk body is less than 37°.
7. The method for preparing aluminum alloy powder according to claim 4, characterized in that: The alloy rod of the first preset ratio includes: Mg: 1.0wt% to 4.0wt%, Li: 0.5wt% to 2.0wt%, Ga: 0.8wt% to 2.0wt%, Si: 0.3wt% to 1.0wt%, Zn: 0.1wt% to 0.5wt%, Sn: 0.8wt% to 2.0wt%; The alloy rod of the second preset ratio includes: Zn: 0.2wt% to 0.7wt%.
8. An additively manufactured aluminum alloy, characterized in that: The additively manufactured aluminum alloy comprises the aluminum alloy powder described in any one of claims 1-3.
9. A method for preparing an aluminum alloy by additive manufacturing, characterized in that: The method for preparing the additively manufactured aluminum alloy is used to prepare the additively manufactured aluminum alloy according to claim 8, and the method comprises: Aluminum alloy powder is used as printing material and input into the preset fiber laser SLM printer. After printing, annealing, wire cutting and surface treatment, additively manufactured aluminum alloy is obtained.
10. The method for preparing aluminum alloy by additive manufacturing according to claim 9, characterized in that: The preheating temperature of the fiber laser SLM printer is 10°C to 75°C, the laser power is 150W to 220W, the scanning speed of the fiber laser SLM printer is 800mm / s to 1300mm / s, the scanning spacing is 0.15mm to 0.5mm, the scanning layer thickness is 0.03mm to 0.06mm, and the area overlap is set to 0.19mm.