440MPa grade aluminum-silicon coating plated steel for automobiles and preparation method of 440MPa grade aluminum-silicon coating plated steel

Through the combination of low-cost component design and process of 440MPa grade aluminized silicon-coated automotive steel, the existing technology problems of high cost, difficult production and poor surface quality of automotive exterior steel are solved, achieving high mechanical properties and Automotive exterior steel plates with high surface quality have excellent formability and strong plasticity.

CN118726844AActive Publication Date: 2024-10-01ANGANG STEEL CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410854079.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-01
Estimated Expiration
2044-06-28

AI Technical Summary

Technical Problem

Existing steel for automobile exterior panels has problems such as high cost, difficulty in production, and poor surface quality in terms of lightweighting and performance improvement. Especially when developing high-strength products, it is difficult to balance mechanical properties and surface quality.

Method used

Using the preparation method of 440MPa grade aluminum-silicon coated automotive steel, through low-cost component design and combination of continuous annealing and aluminum-silicon plating process, the chemical composition and heat treatment process are controlled to form a steel plate with excellent mechanical properties, including C, Mn, Alloy design of Cu, P, Si, Nb, Al and Si, and achieve high strength and high surface quality through hot rolling, cold rolling, pickling, continuous annealing aluminized silicon and finishing processes.

Benefits of technology

It achieves an improvement in the high yield strength, tensile strength and plastic strain ratio of the steel plate, while ensuring high surface quality and low-cost production, reducing high-temperature overaging processes, and improving the formability and strong plasticity of the steel plate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004917588420000051
    Figure BDA0004917588420000051
  • Figure BDA0004917588420000061
    Figure BDA0004917588420000061
Patent Text Reader

Abstract

The invention relates to 440 MPa grade aluminum-silicon coating plated automobile steel and a preparation method thereof. The preparation method comprises the steps of steelmaking continuous casting, hot rolling, acid pickling, cold rolling, continuous annealing aluminum-silicon plating and finishing. The continuous annealing aluminum and silicon plating method comprises the following steps: (1) the isothermal annealing temperature is 810-880 DEG C, and the annealing time is 40-100 seconds; (2) the slow cooling rate is 2-10 DEG C / s, and the slow cooling temperature is 650-720 DEG C; and 3) aluminum-silicon plating: after slow cooling, carrying out isothermal treatment at 650-720 DEG C for 5-20 seconds, and then carrying out aluminum-silicon plating, the temperature of an aluminum-silicon plating solution is 650-720 DEG C, the difference value between the temperature of the aluminum-silicon plating solution and the slow cooling isothermal temperature of the steel plate is less than or equal to 10 DEG C, and after the steel plate is subjected to the slow cooling isothermal temperature, the steel plate enters the aluminum-silicon plating solution to obtain a surface plating layer. And 4) cooling the steel plate to room temperature at a rapid cooling rate of not less than 20 DEG C / s. Through low-cost component design and process design combining continuous annealing and aluminum-silicon plating, the 440MPa-grade steel for the outer plate of the new energy automobile, which is excellent in mechanical property, high in concavity resistance and high in surface quality, is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of automobile steel manufacturing, and in particular relates to a 440MPa grade aluminum-silicon coated automobile steel and a preparation method thereof. Background Art

[0002] The rapid development of the automobile industry has brought convenience to people, but it has also brought social problems such as energy, environment and safety. Therefore, the development direction of modern automobiles is energy saving, emission reduction, emission reduction and improved safety performance. In order to achieve the above goals, the automobile industry has proposed a solution of lightweighting automobiles, and appropriate material selection is one of the important ways to achieve lightweighting. At present, steel materials are still the main materials used in automobiles, accounting for more than 60% of the total vehicle consumption, and the amount of steel used in automobile outer panels accounts for the largest proportion. Therefore, considering the requirements of lightweighting and performance improvement, the strength grade of steel used in automobile outer panels is also constantly improving, and high-strength interstitial atomic steel (IF) is applied.

[0003] High-strength IF steel is developed on the basis of traditional IF steel. Due to its composition characteristics and internal structure without interstitial atoms, it has excellent deep drawing performance, and has the characteristics of high strength and no aging. 440MPa grade high-strength IF steel is currently the most important product in the high-strength series of IF steel. It is the main steel for automobile outer panels and one of the cutting-edge products in the field of automobile steel. With the continuous advancement of automobile lightweighting in various countries, the development of high-strength automobile outer panel products is very necessary for the application of steel materials in the automotive industry. Summary of the invention

[0004] The present invention provides a 440MPa grade aluminum-silicon coated automobile steel and a preparation method thereof. Through low-cost component design and a process design combining continuous annealing and aluminum-silicon plating, a 440MPa grade new energy automobile outer panel steel with excellent mechanical properties, high dent resistance and high surface quality is achieved.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions:

[0006] 440MPa grade aluminum-silicon coated automobile steel, the chemical composition of the substrate is as follows by weight percentage: C 0.005%~0.010%, Mn 0.7%~1.5%, Cu 0.3%~0.7%, P 0.04%~0.08%, Si 0.03%~0.06%, Nb0.06%~0.13%, N≤0.003%, Al 0.02%~0.05%, S≤0.006%, and the balance is Fe and unavoidable impurities.

[0007] The steel plate has a yield strength of 260-360 MPa, a tensile strength of ≥440 MPa, an elongation after fracture of more than 34%, a plastic strain ratio r of more than 1.9, and a strain hardening exponent n of more than 0.2.

[0008] The steel plate structure includes ferrite, NbC precipitation phase and Cu-rich phase.

[0009] The reasons for the alloy design of the present invention are as follows:

[0010] C: C is an important element in the present invention. As an interstitial solid solution atom in steel, C has a pinning effect on dislocations, etc., which seriously limits the improvement of the formability of the steel plate. However, if the C content is too low, it is easy to cause difficulties in steelmaking and greatly increase the cost of steelmaking. In addition, an appropriate amount of C in steel can be fixed with microalloying elements such as Ti or Nb, and its product can improve the strength of the steel by precipitation strengthening without increasing too much cost and having a significant impact on plasticity. Therefore, the present invention requires that the C content is 0.005% to 0.010%.

[0011] Mn: Mn element achieves the purpose of solid solution strengthening by replacing atoms. This element is the main element for the automobile outer plate in the present invention to obtain a strength of 440MPa. However, excessive Mn addition is easy to cause segregation in the steel and easy to produce MnS inclusions, which seriously damages the formability of the steel plate. Therefore, the present invention requires the Mn content to be 0.7% to 1.5%.

[0012] Cu: Cu is the main element of the present invention. Cu exists in the steel in the form of Cu-rich phase. During the aging stage, Cu atoms are segregated in the matrix phase to form a Cu-rich phase. The precipitation size is usually nanometer-scale and does not combine with elements such as C and N, playing a role of precipitation strengthening. The limited Cu content can make the steel plate have dispersed and fine Cu-rich phases. Too much will make the Cu-rich phase coarse, and too little will affect the precipitation amount of the Cu-rich phase, both of which are unfavorable to the strength of the steel plate. Therefore, the present invention requires the Cu content to be 0.3% to 0.7%.

[0013] P: P is one of the important elements in the present invention, and it is also a solid solution strengthening element in steel. Adding P can significantly improve the strength of the steel plate, but this element is very easy to precipitate at the grain boundary and make the grain boundary embrittled, thereby affecting the plasticity and forming properties of the steel plate. The present invention comprehensively considers the addition amount of Mn and P, and requires the P element content to be 0.04% to 0.08%.

[0014] Si: Si is also a solid solution strengthening element in the present invention. A proper amount of Si can improve the strength of the steel plate, but too much Si affects the surface quality and plastic toughness of the steel plate. Therefore, based on the comprehensive consideration of solid solution strengthening elements, the present invention requires that the Si content be 0.03% to 0.06%.

[0015] Nb: Nb element is an important element in the present invention. Nb and interstitial atoms C fix C atoms in the form of strain-induced precipitation during the hot rolling stage and serve to refine the grains. At the same time, some Nb atoms are solid dissolved in the matrix phase to refine the grains by the dragging effect of solute atoms, thereby promoting the formability and strength of the steel plate. Taking into account the effects of C atoms and their solute atom dragging effect on the microstructure and properties in steel, the present invention requires the Nb content to be 0.06% to 0.13%.

[0016] N: N is an impurity element in steel. This element exists in the matrix phase in the form of interstitial solid solution atoms, which deteriorates the plasticity and toughness of the steel plate. Therefore, the lower its content, the better. The present invention requires that the N element content is ≤ 0.003%.

[0017] Al: Al is mainly used as a deoxidizer. It combines with N atoms to form AlN, thereby removing interstitial N atoms and helping to improve the formability of the steel plate. However, excessive addition of this element increases costs and increases the difficulty of steelmaking. Therefore, the present invention requires that the Al content be 0.02% to 0.05%.

[0018] S: S is an impurity element in steel, and is easy to form inclusions and precipitation with elements such as Mn, which is not good for the formability of the steel plate. Therefore, the present invention requires that the S element content is ≤ 0.006%.

[0019] A method for preparing 440MPa grade aluminum-silicon coated automobile steel, comprising steelmaking and continuous casting, hot rolling, pickling, cold rolling, continuous annealing, aluminum-silicon coating and skin-finishing processes;

[0020] Steelmaking and continuous casting: The alloy is smelted through a converter and refining outside the furnace to obtain the component alloy within the required range of the present invention, and then cast into a slab.

[0021] The hot rolling process comprises the following method:

[0022] 1) The heating temperature is between 1200 and 1300 °C, and the furnace time is ≥ 120 min, which can ensure the uniform distribution of alloy elements in the steel plate, thus facilitating the uniformity of the final microstructure.

[0023] 2) The starting rolling temperature is between 1100 and 1150°C, and the final rolling temperature is required to be ≥910°C to ensure rolling in the recrystallization range, which is conducive to the dynamic recrystallization behavior of austenite grains.

[0024] 3) The coiling temperature is controlled between 630 and 700 °C, so that NbC precipitates to completely fix the interstitial atomic C, which is beneficial for pinning the grain boundaries and improving the subsequent cold rolling deformation energy storage.

[0025] Pickling: Remove the surface oxide scale formed on the steel plate during the hot rolling stage to improve the surface quality of the steel plate.

[0026] The cold rolling has a cold rolling reduction rate of 75% to 85%. The purpose of ensuring a reduction rate of more than 75% is to make the steel plate reach the target thickness of the steel plate and to ensure the cold rolling structure is fibrotic, so that it has high deformation energy storage, thereby providing power for the recrystallization of ferrite in the subsequent continuous annealing stage. However, too much reduction will lead to excessive deformation resistance, and the cold rolling equipment capacity requirements are too high, making it difficult to achieve the target thickness, so the pressure rate is required not to be greater than 85%.

[0027] The continuous annealing aluminum silicon plating process comprises the following method:

[0028] 1) Annealing isothermal temperature is 810~880℃, annealing time is 40~100s; the temperature and time in this limited range are to ensure that the cold rolled deformation structure of the steel plate is effectively recrystallized and the ferrite grain size is suitable and uniform, and at the same time promote <111> / / ND oriented grains nucleate and grow in this process, thus forming a strong <111> / / ND texture.

[0029] 2) The slow cooling rate is 2-10℃ / s, the slow cooling temperature is 650-720℃, and the slow cooling isothermal time is 5-20s. The slow cooling stage can ensure that the dissolved NbC can be effectively precipitated, ensuring low solid solution carbon in the steel, thereby ensuring the final performance of the steel plate; at the same time, during this stage, the Cu-rich phase in the steel plate is precipitated, and this temperature and time can ensure that the Cu-rich phase is dispersed in the matrix, which promotes the strength.

[0030] 3) Aluminum silicon plating, after slow cooling and isothermal treatment, the steel plate enters the plating solution. The temperature of the aluminum silicon plating solution is 650-720℃, and the temperature difference between it and the slow cooling temperature of the steel plate is ≤10℃. The aluminum silicon plating time is 3-10s. The limited temperature and time can effectively ensure the fluidity of the aluminum silicon plating solution, enhance the adhesion of the coating, and make the coating surface smooth. At the same time, the small temperature difference between the aluminum silicon plating and the slow cooling stage can also ensure the full precipitation of NbC and Cu-rich phases in the steel plate, reduce the content of solid solution C in the steel, and at the same time, the precipitated phase plays a role in precipitation strengthening to ensure the strength of the steel plate. In addition, if the temperature of the steel plate is too high, the plating solution temperature will increase, which will increase the Fe solid solubility in the plating solution and cause the Fe content to increase; when the temperature of the steel plate is low, the plating solution temperature will be reduced to affect the fluidity, and a large number of Fe-Al alloy particles will be formed due to the reduction of the Fe solid solubility in the plating solution, thereby affecting the coating quality of the steel plate.

[0031] 4) After the aluminum-silicon coating is completed, the steel plate is cooled to room temperature at a rapid cooling rate of ≥20℃ / s. This rate can control the thickness of the coating and make the steel strip structure uniform, while preventing obvious crystal formation on the surface of the steel plate.

[0032] In the polishing process, the polishing elongation is 0.5% to 1.5%, and the shape of the steel plate is adjusted.

[0033] The composition of the aluminum silicon plating solution is as follows: Si 7% to 12%, Fe ≤ 2%, and the rest is Al and inevitable impurity elements. The limited content of Si element can improve the fluidity of the plating solution and reduce the temperature of aluminum plating. At the same time, Si can inhibit the Fe-Al reaction to form an alloy phase, effectively reducing the thickness of the alloy layer, which is beneficial to the plating forming performance. Fe in the plating solution is an inevitable impurity element, which is generated when the steel plate enters the plating solution and causes the Fe element to diffuse into the plating solution. Excessive Fe content increases the viscosity of the plating solution and affects the thickness of the coating. It also reacts with the Al element to form alloy particles suspended in the plating solution, causing the steel plate to leak plating and other phenomena, affecting the quality of the coating.

[0034] The final microstructure of the 440MPa grade aluminum-silicon coated automobile outer panel of the present invention is composed of ferrite, NbC precipitation phase and Cu-rich phase, and the steel plate texture is strong. <111> / / ND γ texture, and the steel plate surface is aluminum silicon coating. The present invention adopts a new hot coating process combined with a heat treatment process, and the aluminum silicon coated automobile outer panel has a yield strength of 260-360MPa, a tensile strength of ≥440MPa, an elongation after fracture of more than 34%, a plastic strain ratio r of more than 1.9, and a strain hardening index n of more than 0.2.

[0035] Compared with the prior art, the present invention has the following beneficial effects:

[0036] 1) The steel plate of the present invention mainly contains Mn, Cu, P and a small amount of Nb as main elements, and the C content is 0.005% to 0.010%, which is beneficial to the production of the steel plate, especially the control of C at the steelmaking end.

[0037] 2) The present invention adopts aluminum-silicon plating to make the steel plate obtain a coating structure, and combines the aluminum-silicon plating process with the slow cooling section of the heat treatment process. It is more commonly used hot-dip galvanizing, reduces the high-temperature over-aging process, ensures high efficiency and makes the steel plate have excellent surface quality.

[0038] 3) The present invention achieves excellent formability and strong plasticity of the steel plate through low-cost alloy design and novel process design. DETAILED DESCRIPTION

[0039] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the specific implementation methods of the present invention are further described below in conjunction with embodiments. The following embodiments are used to specifically illustrate the contents of the present invention. These embodiments are only general descriptions of the contents of the present invention and do not limit the contents of the present invention.

[0040] Table 1 lists the chemical composition of the example steel, Table 2 lists the process parameters of hot rolling and cold rolling of the example steel, Table 3 lists the process parameters of continuous annealing and aluminum silicon plating of the example steel, and Table 4 gives the mechanical properties of the example steel.

[0041] Table 1 Chemical composition of the example steel, wt%

[0042] No. C Mn Cu P Si Nb N Al S 1 0.0071 1.08 0.43 0.045 0.037 0.065 0.0015 0.035 0.0030 2 0.0063 0.92 0.35 0.056 0.032 0.072 0.0012 0.032 0.0026 3 0.0082 0.87 0.51 0.061 0.045 0.063 0.0014 0.042 0.0035 4 0.0078 0.79 0.67 0.052 0.046 0.080 0.0010 0.027 0.0031 5 0.0068 0.95 0.41 0.063 0.051 0.090 0.0009 0.030 0.0026 6 0.0091 1.10 0.56 0.058 0.048 0.095 0.0010 0.040 0.0020 7 0.0085 1.02 0.31 0.067 0.035 0.082 0.0016 0.029 0.0017 8 0.0074 0.97 0.36 0.070 0.049 0.074 0.0013 0.045 0.0032

[0043] Table 2 Hot rolling and cold rolling process of example steel

[0044]

[0045] Table 3 Example steel annealing and aluminum silicon plating process

[0046]

[0047] Table 4 Mechanical properties of example steel

[0048] Example <![CDATA[R p0.2 / Mpa]]> <![CDATA[R m / Mpa]]> <![CDATA[A 50 / %]]> Plastic strain ratio r Strain hardening exponent n Coating surface 1 275 450 35 2.0 0.21 Crystalless Flower 2 262 465 34 2.0 0.22 Crystalless Flower 3 269 457 36 2.2 0.20 Crystalless Flower 4 272 448 37 2.1 0.21 Crystalless Flower 5 273 457 36 2.3 0.23 Crystalless Flower 6 267 452 35 2.2 0.2 Crystalless Flower 7 272 449 36 2.1 0.24 Crystalless Flower 8 263 460 38 2.2 0.23 Crystalless Flower

[0049] It can be seen from the above embodiments that by using elements such as Mn and P for solid solution strengthening and precipitation strengthening of the Cu-rich phase, combined with Nb element fixing interstitial atoms and fine grain strengthening, and innovatively matching the aluminum-silicon plating process with the continuous annealing and slow cooling stage in the heat treatment, aluminum-silicon-plated automobile outer panel steel with excellent mechanical properties and high surface quality is prepared, and its yield strength is 260-360MPa, tensile strength is ≥440MPa, elongation after fracture is more than 34%, plastic strain ratio r is more than 1.9, and strain hardening exponent n is more than 0.2.

Claims

1. 440MPa grade aluminum-silicon coated automobile steel, characterized in that: The chemical composition of the substrate is calculated by weight percentage: C 0.005% to 0.010%, Mn 0.7% to 1.5%, Cu 0.3% to 0.7%, P 0.04% to 0.08%, Si 0.03% to 0.06%, Nb 0.06% to 0.13%, N≤0.003%, Al 0.02% to 0.05%, S≤0.006%, and the balance is Fe and unavoidable impurities.

2. The 440MPa grade aluminum-silicon coated automobile steel according to claim 1, characterized in that: The steel plate has a yield strength of 260-360 MPa, a tensile strength of ≥440 MPa, an elongation after fracture of more than 34%, a plastic strain ratio r of more than 1.9, and a strain hardening exponent n of more than 0.

2.

3. The 440MPa grade aluminum-silicon coated automobile steel according to claim 1, characterized in that: The steel plate structure includes ferrite, NbC precipitation phase and Cu-rich phase.

4. The method for preparing 440MPa grade aluminum-silicon coated automobile steel according to any one of claims 1 to 3, characterized in that: It includes steelmaking and continuous casting, hot rolling, pickling, cold rolling, continuous annealing, aluminum silicon plating and skin finishing processes; the continuous annealing, aluminum silicon plating process includes the following method: 1) The annealing isothermal temperature is 810-880°C and the annealing time is 40-100s; 2) The slow cooling rate is 2-10°C / s, the slow cooling temperature is 650-720°C, and the slow cooling isothermal time is 5-20s; 3) Aluminum silicon plating, after slow cooling and isothermal treatment, aluminum silicon plating is performed to obtain a coating, the aluminum silicon plating solution temperature is 650-720°C, the aluminum silicon plating time is 3-10s, and the difference between the plating solution temperature and the slow cooling temperature of the steel plate is ≤10°C; 4) After the aluminum-silicon coating is completed, the steel plate is cooled to room temperature at a rapid cooling rate of ≥20℃ / s.

5. The method for preparing 440MPa grade aluminum-silicon coated automobile steel according to claim 4, characterized in that: The hot rolling process comprises the following method: 1) The heating temperature is between 1200 and 1300°C, and the furnace time is ≥ 120 minutes; 2) The starting rolling temperature is between 1100 and 1150°C, and the final rolling temperature is required to be ≥910°C; 3) The coiling temperature is controlled between 630 and 700°C.

6. The method for preparing 440MPa grade aluminum-silicon coated automobile steel according to claim 4, characterized in that: In the cold rolling process, the cold rolling reduction rate is 75% to 85%.

7. The method for preparing 440MPa grade aluminum-silicon coated automobile steel according to claim 4, characterized in that: In the polishing process, the polishing elongation is 0.5% to 1.5%.

8. The method for preparing 440MPa grade aluminum-silicon coated automobile steel according to claim 4, characterized in that: The aluminum silicon plating solution comprises, by mass percentage, 7% to 12% Si, ≤2% Fe, and the rest Al and unavoidable impurity elements.

Citation Information

Patent Citations

  • 440MPa grade niobium-containing high-strength IF steel and manufacturing method thereof

    CN101348884A

  • High-strength cold-rolled hot-galvanized dual-phase steel plate and manufacture method thereof

    CN102719751A

  • 800MPa-grade high-strength high-plasticity low-carbon medium-manganese steel and manufacturing method thereof

    CN104630641A

  • Photovoltaic high-strength structural grade coated steel plate and manufacturing method thereof

    CN116288025A

  • 1200MPa-grade DH steel plate of aluminum-silicon coating and manufacturing method of 1200MPa-grade DH steel plate