Preparation method of lightweight aluminum alloy

Through the alloying of zinc, magnesium, nickel and other elements with aluminum ingots and the combination of reinforcements such as rare earths, combined with pressure forging of liquid metal and ultrasonic homogenization technology, the problem of balancing light weight and strength of aluminum alloy materials is solved. It achieves lighter aluminum alloy preparation and improves the economy and material performance of new energy vehicles.

CN118726863APending Publication Date: 2024-10-01HETIAN AUTOMOTIVE IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410719651.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-05
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing aluminum alloy materials have difficulties in achieving a balance between light weight and strength, especially in the low-temperature baking process. Their strength is not ideal and it is difficult to achieve balanced formability.

Method used

Zinc, magnesium, nickel, copper, titanium, zirconium, beryllium, chromium and other elements are smelted with aluminum ingots and recycled aluminum to form alloys, and passed through rare earths, alumina, titanium oxide, titanium boride, whiskers and boron nitride nanotubes The combination improves the crystal structure and mechanical properties of the alloy, and ensures high dispersion of the material and no casting defects through pressure liquid forging and ultrasonic homogenization technology.

Benefits of technology

It achieves a lighter weight with the same mechanical strength as ordinary aluminum alloys, improves the economy of new energy vehicles, saves costs through recycling, and avoids casting defects and oxidation problems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118726863A_ABST
    Figure CN118726863A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a lightweight aluminum alloy, and relates to the technical field of automobile production, and the preparation method comprises the following steps: preparing materials: zinc, magnesium, nickel, copper, titanium, zirconium, beryllium, strontium, chromium, rare earth, silicon carbide, aluminum oxide, titanium oxide, titanium boride, crystal whiskers, boron nitride nanotubes and aluminum ingots, and recovering aluminum; according to the aluminum alloy, aluminum ingots and recycled aluminum molten aluminum are used as matrixes and matched with zinc, magnesium, nickel, copper, titanium, zirconium, beryllium, strontium and chromium to form the alloy, the crystal structure and mechanical performance of the aluminum alloy are improved, rare earth plays a role in refining crystal grains during alloy crystallization, the strength and plasticity of the alloy are improved, aluminum oxide, titanium oxide, titanium boride and crystal whiskers are used as reinforcements, and the strength and plasticity of the alloy are improved. The mechanical property of the aluminum alloy is improved, the performance of the aluminum alloy is changed by refining crystal grains of the boron nitride nanotubes in the solidification process and changing the microstructure of metal, it is verified that the aluminum alloy is lighter under the same mechanical strength as common aluminum alloy, and the economical efficiency of new energy automobiles is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of automobile production, and in particular to a method for preparing a lightweight aluminum alloy. Background Art

[0002] In the context of the increasing difficulty of improving engine technology, new energy vehicles have become the trend of future development. At the same time, the automotive industry is booming all over the world, which has prompted the automotive industry to focus on energy and environmental protection as the core of sustainable development. Advanced automotive material technology dominated by lightweight vehicles is an important guarantee for achieving this goal. Therefore, lightweight new energy vehicles have become the main direction of future automotive technology development. Automobile materials are an important factor affecting automobile weight, and have a considerable impact on energy conservation and pollution improvement. When new energy technology is not yet mature, automobile weight reduction is undoubtedly the best way to reduce energy consumption and pollution. The use of lightweight materials is the simplest way to reduce automobile weight. The body weight accounts for about 40% of the total weight of the car. For the lightweight of the whole vehicle, the lightweight of the body plays a pivotal role. Specifically: use scientific methods and means to optimize the design of automobile products. Under the premise of ensuring the comprehensive performance indicators of the car, by using new materials, the weight of the automobile product itself is reduced as much as possible to achieve the comprehensive goals of weight reduction, consumption reduction, environmental protection and safety. Studies have shown that about 60% of the energy used by the car is consumed by the car's own weight. The weight of the car is reduced, and the energy consumption will also be reduced. Under the same output power, a lighter car is a lighter load for the engine, and the car's handling stability is also improved. Therefore, reducing the weight of the car body has a dual effect on reducing the power consumption of the engine and reducing the total weight of the car. As a lightweight material with multiple excellent properties, aluminum alloy has become the preferred material in the current development of automobile lightweight technology. Since the specific gravity of aluminum is about 1 / 3 of that of steel, aluminum alloy is recognized as an ideal material for automobile lightweighting. In addition, aluminum is highly recyclable, beautiful in appearance, energy-saving, good in heat dissipation, corrosion-resistant, and fatigue-resistant. It will become the first choice material to replace steel in the future logistics vehicle manufacturing industry. The aluminum alloys currently used on the market do not have ideal use strength, especially for the development of new 6 series alloys that can implement low-temperature baking paint technology, and the development of aluminum alloys with higher baking hardening performance. Overall, the comprehensive performance of the current 6 series aluminum alloy automobile plates is general. Low alloying is generally used to sacrifice part of the strength to obtain high forming performance, or high strength is obtained by sacrificing forming performance. It is difficult to achieve a balanced effect of light weight and other properties such as strength. Therefore, the present invention proposes a preparation method of a lightweight aluminum alloy to solve the problems existing in the prior art. Summary of the invention

[0003] In view of the above problems, the present invention proposes a method for preparing a lightweight aluminum alloy. The method for preparing a lightweight aluminum alloy can achieve a lighter weight under the same mechanical strength as ordinary aluminum alloy, which helps to improve the economy of new energy vehicles.

[0004] To achieve the purpose of the present invention, the present invention is implemented by the following technical scheme: A method for preparing a lightweight aluminum alloy comprises the following steps: S1: Prepare materials: zinc, magnesium, nickel, copper, titanium, zirconium, beryllium, strontium, chromium, rare earth, silicon carbide, aluminum oxide, titanium oxide, titanium boride, whiskers, boron nitride nanotubes and aluminum ingots, recycled aluminum; S2: Smelting and refining the recycled aluminum to recover the aluminum liquid, then melting the aluminum ingot into liquid and mixing it with the recovered aluminum liquid to obtain a mixed liquid; S3: adding zinc, magnesium, nickel, copper, titanium, zirconium, beryllium, strontium and chromium into a mixed liquid, stirring and melting the mixed liquid in a smelting furnace to form a liquid metal; S4: Cooling the liquid metal, waiting for the solid and liquid to coexist, introducing it into the pressure cavity for pressure application, liquid forging and pressure maintenance, and then heating it into liquid in the melting furnace; S5: adding a refining agent for refining, then standing to skim off the surface scum, and then performing ultrasonic homogenization; S6: Extend the feeding tube into the liquid metal, blow rare earth, silicon carbide, aluminum oxide, titanium oxide, and titanium boride into the liquid metal through the feeding tube with air pressure, and stir and homogenize; S7: Cooling the liquid metal again, waiting for the solid and liquid to coexist, introducing it into the pressure cavity for pressure application, liquid forging and pressure maintenance, and then heating it into liquid state into a melting furnace, adding whiskers and boron nitride nanotubes; S8: After cooling the liquid metal, press it into a mold, cool it to obtain a finished product, and perform an antioxidant treatment on the surface.

[0005] A further improvement is that in S1, materials are prepared according to the following mass ratios: 2-5 parts of zinc, 2-5 parts of magnesium, 2-5 parts of nickel, 2-5 parts of copper, 2-5 parts of titanium, 1-3 parts of zirconium, 1-3 parts of beryllium, 1-3 parts of strontium, 1-3 parts of chromium, 5-10 parts of rare earth, 0.5-1 parts of silicon carbide, 0.5-1 parts of aluminum oxide, 0.5-1 parts of titanium oxide, 0.5-1 parts of titanium boride, 0.2-0.5 parts of whiskers, 0.3-0.5 parts of boron nitride nanotubes, 40-60 parts of aluminum ingots, and 30-50 parts of recycled aluminum.

[0006] Further improvements are: the particle size of titanium oxide and titanium boride is 10 μm, the diameter of the whisker is 0.1-2 μm, the length is 20-200 μm, and the boron nitride nanotube is selected to have a diameter of 60 nm and a length of 20 μm.

[0007] A further improvement is that: S2 comprises the following steps: S21: Put the recycled aluminum into a smelting furnace, heat it to 700-750°C, and smelt it for 60-90 minutes to melt it; S22: Using inert gas nitrogen as a carrier, 1.0-1.5‰ granular refining agent is evenly blown into the aluminum liquid, and allowed to stand for 10-20 minutes to remove the internal hydrogen and floating oxide slag; S23: collecting the aluminum-containing slag floating on the liquid surface, performing rotary calcination in a rotary kiln to separate the ash and aluminum, and then recovering the aluminum liquid therein to a smelting furnace to obtain a total recovered aluminum liquid; S24: Then, the aluminum ingot is heated to 700-800° C. and smelted for 50-80 minutes to be melted into liquid, and the liquid is mixed with the recovered aluminum liquid to obtain a mixed liquid.

[0008] A further improvement is that: S3 comprises the following steps: S31: adding zinc, magnesium, nickel, copper, titanium, zirconium, beryllium, strontium and chromium into a mixed solution, and adjusting the temperature in the smelting furnace to 700-800°C; S32: Stirring for 10-20 minutes, and when all the materials in the smelting furnace are melted into liquid, stirring is stopped to obtain liquid metal.

[0009] A further improvement is that: said S4 comprises the following steps: S41: Prepare the die casting machine, apply lubricant in the pressure cavity, and preheat the pressure cavity to 280-380℃ for 2-3min; S42: Cooling the liquid metal to 60-70°C, waiting for the liquid metal to coexist in solid and liquid state, and then introducing the liquid metal into the pressurized cavity; S43: applying pressure to the pressure cavity, controlling the liquid forging pressure at 70-130 MPa, controlling the temperature at 550-600°C, and then maintaining the pressure for 30-45 seconds; S44: After completion, the mixture is introduced into a melting furnace and heated to 650-700°C to form a liquid.

[0010] The further improvement is that S5 comprises the following steps: S51: adding a refining agent to the liquid metal at 700-750°C for refining, standing for 5-10 minutes after refining, and skimming off the surface scum at 600-700°C; S52: Ultrasonic homogenization of liquid metal at a frequency of 40 kHz and a power density of 0.8 W / cm 2 Ultrasonic homogenization was performed for 1 min.

[0011] A further improvement is that: S6 comprises the following steps: S61: Extend the high temperature resistant feeding pipe into the liquid metal and connect it to the air pressure feeding pump; S62: Blowing rare earth, silicon carbide, aluminum oxide, titanium oxide, and titanium boride into the liquid metal through a feeding pipe with air pressure, and controlling the air pressure so that no sputtering occurs on the surface of the liquid metal; S63: Stir and homogenize simultaneously, and control the stirring speed to 50-120r / min.

[0012] A further improvement is that: said S7 comprises the following steps: S71: Cool the liquid metal to 55-65°C, wait for the liquid metal to coexist in solid and liquid, introduce it into the pressure cavity, apply pressure, control the liquid forging pressure at 70-120MPa, control the temperature during pressure application at 500-600°C, and then maintain the pressure for 20-30s; S72: then introducing the smelting furnace into a liquid state by heating at 700-750°C, and adding whiskers and boron nitride nanotubes; S73: Stir for 2-3 minutes at a rotation speed of 50-100 r / min.

[0013] A further improvement is that in S8, the liquid metal is cooled to between 580-650°C, injected into a mold preheated to 200-350°C at a speed of 1.5-2m / s, cooled to obtain a finished product, then acrylic emulsion is applied to the outside of the finished product, placed in an electrophoresis tank, connected to a power source to allow the emulsion to adhere, and heated and dried to obtain an antioxidant reinforced coating.

[0014] The beneficial effects of the present invention are: 1. The present invention uses aluminum ingots and recycled aluminum molten aluminum as a matrix, and combines zinc, magnesium, nickel, copper, titanium, zirconium, beryllium, strontium, and chromium to form an alloy, thereby improving the crystal structure and mechanical properties of the aluminum alloy. Rare earths refine the grains during alloy crystallization to improve the strength and plasticity of the alloy. Aluminum oxide, titanium oxide, titanium boride, and whiskers are used as reinforcements to improve the mechanical properties of the aluminum alloy. Boron nitride nanotubes refine the grains during solidification to change the microstructure of the metal, thereby changing its performance. It has been verified that the same mechanical strength as ordinary aluminum alloys can be achieved with a lighter weight, which helps to improve the economy of new energy vehicles.

[0015] 2. The base material of the present invention uses recycled aluminum, and the planned processing flow is conducive to recycling and cost saving.

[0016] 3. The present invention utilizes the characteristics of metal when it transitions from liquid to solid or from solid to liquid. By applying pressure, liquid forging and maintaining pressure twice under the coexistence of solid and liquid, the metal is crystallized and solidified under pressure and the shrinkage cavities and shrinkage formed by solidification shrinkage are forced to be eliminated to obtain a material without casting defects.

[0017] 4. The present invention uses a feeding pipe to blow rare earth, silicon carbide, aluminum oxide, titanium oxide, and titanium boride into the liquid metal with air pressure, and then stirs and homogenizes the material to make it highly dispersed, the particles are completely embedded in the metal matrix, and a suitable interface is formed, thereby improving the performance of the aluminum alloy. 5. The present invention applies acrylic emulsion on the outside of the finished product, connects to a power source to make the emulsion adhere, heats and dries to obtain an anti-oxidation reinforced coating, avoids oxidation of the aluminum alloy, and is convenient for storage. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 It is a flow chart of the present invention. DETAILED DESCRIPTION

[0019] In order to deepen the understanding of the present invention, the present invention will be further described in detail below in conjunction with examples. The examples are only used to explain the present invention and do not constitute a limitation on the protection scope of the present invention. Example 1

[0020] according to Figure 1 As shown, this embodiment proposes a method for preparing a lightweight aluminum alloy, comprising the following steps: Prepare materials according to the following mass ratio: 2 parts of zinc, 2 parts of magnesium, 2 parts of nickel, 2 parts of copper, 2 parts of titanium, 13 parts of zirconium, 1 part of beryllium, 1 part of strontium, 1 part of chromium, 5 parts of rare earth, 0.5 parts of silicon carbide, 0.5 parts of aluminum oxide, 0.5 parts of titanium oxide, 0.5 parts of titanium boride, 0.2 parts of whiskers, 0.3 parts of boron nitride nanotubes, 40 parts of aluminum ingots, and 30 parts of recycled aluminum; wherein the particle size of titanium oxide and titanium boride is 10 μm, the diameter of the whiskers is 0.1-2 um, and the length is 20-200 um, and the boron nitride nanotubes are selected to have a diameter of 60 nm and a length of 20 um; the boron nitride nanotubes are mixed with NanoBarb powder and metallic aluminum, and the BNNB powder is evenly dispersed in the aluminum to form aluminum-based master alloy reinforcement particles, and the boron nitride nanotubes reach the nanometer level, and the smaller the particles, the higher the possibility of improving the strength performance; The recycled aluminum is melted and refined to recover aluminum liquid, and then the aluminum ingot is melted into liquid, mixed with the recovered aluminum liquid to obtain a mixed liquid; specifically, the following steps are included: the recycled aluminum is placed in a smelting furnace, heated to 700-750°C, and smelted for 60-90 minutes to melt it; with inert gas nitrogen as a carrier, 1.0-1.5‰ granular refining agent is evenly blown into the aluminum liquid, and allowed to stand for 10-20 minutes to remove hydrogen and floating oxide inclusions inside; slag containing aluminum floating on the liquid surface is collected, and rotary calcined in a rotary kiln to separate ash and aluminum, and then the aluminum liquid therein is recovered into the smelting furnace to obtain total recovered aluminum liquid; then, the aluminum ingot is heated to 700-800°C, smelted for 50-80 minutes to melt it into liquid, and mixed with the recovered aluminum liquid to obtain a mixed liquid; Add zinc, magnesium, nickel, copper, titanium, zirconium, beryllium, strontium and chromium into a mixed liquid, and stir and melt the mixed liquid in a smelting furnace to form a liquid metal; specifically, the following steps are included: add zinc, magnesium, nickel, copper, titanium, zirconium, beryllium, strontium and chromium into the mixed liquid, and adjust the temperature in the smelting furnace to 700-800°C; stir for 10-20 minutes, and stop stirring when all the materials in the smelting furnace are melted into liquid to obtain liquid metal; The liquid metal is cooled down, and when the solid and liquid coexist, it is introduced into the pressure cavity for pressure, liquid forging and pressure maintenance, and then heated to liquid in a smelting furnace; the specific steps include: preparing a die-casting machine, applying lubricant to the pressure cavity, preheating the pressure cavity to 280-380°C for 2-3 minutes; cooling the liquid metal to 60-70°C, and when the liquid metal solid and liquid coexist, introducing it into the pressure cavity; pressurizing the pressure cavity, controlling the liquid forging pressure ratio at 70-130MPa, controlling the temperature during pressure to 550-600°C, and then maintaining the pressure for 30-45s; after completion, introducing it into a smelting furnace and heating it to 650-700°C to liquid; allowing the metal to crystallize and solidify under pressure and forcibly eliminating shrinkage cavities and shrinkage formed by solidification shrinkage to obtain a material without casting defects; The method comprises the following steps: adding a refining agent to the liquid metal for refining at 700-750°C, standing the liquid metal for 5-10 minutes after refining, and skimming the surface scum at 600-700°C; performing ultrasonic homogenization on the liquid metal at a frequency of 40 kHz and a power density of 0.8 W / cm 2 Ultrasonic homogenization was performed for 1 min under the following conditions; The feeding tube is extended into the liquid metal, and rare earth, silicon carbide, aluminum oxide, titanium oxide, and titanium boride are blown into the liquid metal through the feeding tube in combination with air pressure, and then stirred and homogenized. Specifically, the following steps are included: a high temperature resistant feeding tube is extended into the liquid metal, and an air pressure feeding pump is connected; rare earth, silicon carbide, aluminum oxide, titanium oxide, and titanium boride are blown into the liquid metal through the feeding tube in combination with air pressure, and the air pressure is controlled so that there is no sputtering on the surface of the liquid metal; stirring and homogenizing are performed simultaneously, and the stirring speed is controlled to be 50-120r / min; so that the material is highly dispersed, the particles are completely embedded in the metal matrix, and a suitable interface is formed, thereby improving the performance of the aluminum alloy; The liquid metal is cooled down again, and when the solid and liquid coexist, it is introduced into the pressure cavity for pressure, liquid forging and pressure maintenance, and then heated to liquid in the melting furnace, and whiskers and boron nitride nanotubes are added; the specific steps include: cooling the liquid metal to 55-65°C, and when the solid and liquid coexist, the liquid metal is introduced into the pressure cavity for pressure, and the liquid forging pressure is controlled at 70-120MPa, and the temperature during pressure is controlled at 500-600°C, and then the pressure is maintained for 20-30s, so that the metal crystallizes and solidifies under pressure and the shrinkage cavities and shrinkage formed by solidification shrinkage are forcibly eliminated to obtain a material without casting defects; then the liquid metal is introduced into the melting furnace and heated to 700-750°C for liquid, and whiskers and boron nitride nanotubes are added; stirring is carried out at a speed of 50-100r / min for 2-3min; The liquid metal is cooled to between 580-650℃, injected into a mold preheated to 200-350℃ at a speed of 1.5-2m / s, cooled to obtain the finished product, and then acrylic emulsion is applied to the outside of the finished product, placed in an electrophoresis tank, connected to a power source to allow the emulsion to adhere, and heated to dryness to obtain an antioxidant reinforced coating. Example 2

[0021] according to Figure 1 As shown, this embodiment proposes a method for preparing a lightweight aluminum alloy, comprising the following steps: Prepare materials according to the following mass ratio: 3 parts of zinc, 3 parts of magnesium, 3 parts of nickel, 3 parts of copper, 3 parts of titanium, 2 parts of zirconium, 2 parts of beryllium, 2 parts of strontium, 2 parts of chromium, 8 parts of rare earth, 0.8 parts of silicon carbide, 0.8 parts of aluminum oxide, 0.8 parts of titanium oxide, 0.8 parts of titanium boride, 0.3 parts of whiskers, 0.4 parts of boron nitride nanotubes, 50 parts of aluminum ingots, and 40 parts of recycled aluminum; wherein the particle size of titanium oxide and titanium boride is 10 μm, the diameter of the whiskers is 0.1-2 um, and the length is 20-200 um, and the boron nitride nanotubes are selected to have a diameter of 60 nm and a length of 20 um; the boron nitride nanotubes are mixed with NanoBarb powder and metallic aluminum, and the BNNB powder is evenly dispersed in the aluminum to form aluminum-based master alloy reinforced particles, and the boron nitride nanotubes reach the nanometer level, and the smaller the particles, the higher the possibility of improving the strength performance; The recycled aluminum is melted and refined to recover aluminum liquid, and then the aluminum ingot is melted into liquid, mixed with the recovered aluminum liquid to obtain a mixed liquid; specifically, the following steps are included: the recycled aluminum is placed in a smelting furnace, heated to 700-750°C, and smelted for 60-90 minutes to melt it; with inert gas nitrogen as a carrier, 1.0-1.5‰ granular refining agent is evenly blown into the aluminum liquid, and allowed to stand for 10-20 minutes to remove hydrogen and floating oxide inclusions inside; slag containing aluminum floating on the liquid surface is collected, and rotary calcined in a rotary kiln to separate ash and aluminum, and then the aluminum liquid therein is recovered into the smelting furnace to obtain total recovered aluminum liquid; then, the aluminum ingot is heated to 700-800°C, smelted for 50-80 minutes to melt it into liquid, and mixed with the recovered aluminum liquid to obtain a mixed liquid; Add zinc, magnesium, nickel, copper, titanium, zirconium, beryllium, strontium and chromium into a mixed liquid, and stir and melt the mixed liquid in a smelting furnace to form a liquid metal; specifically, the following steps are included: add zinc, magnesium, nickel, copper, titanium, zirconium, beryllium, strontium and chromium into the mixed liquid, and adjust the temperature in the smelting furnace to 700-800°C; stir for 10-20 minutes, and stop stirring when all the materials in the smelting furnace are melted into liquid to obtain liquid metal; The liquid metal is cooled down, and when the solid and liquid coexist, it is introduced into the pressure cavity for pressure, liquid forging and pressure maintenance, and then heated to liquid in a smelting furnace; the specific steps include: preparing a die-casting machine, applying lubricant to the pressure cavity, preheating the pressure cavity to 280-380°C for 2-3 minutes; cooling the liquid metal to 60-70°C, and when the liquid metal solid and liquid coexist, introducing it into the pressure cavity; pressurizing the pressure cavity, controlling the liquid forging pressure ratio at 70-130MPa, controlling the temperature during pressure to 550-600°C, and then maintaining the pressure for 30-45s; after completion, introducing it into a smelting furnace and heating it to 650-700°C to liquid; allowing the metal to crystallize and solidify under pressure and forcibly eliminating shrinkage cavities and shrinkage formed by solidification shrinkage to obtain a material without casting defects; The method comprises the following steps: adding a refining agent to the liquid metal for refining at 700-750°C, standing the liquid metal for 5-10 minutes after refining, and skimming the surface scum at 600-700°C; performing ultrasonic homogenization on the liquid metal at a frequency of 40 kHz and a power density of 0.8 W / cm 2 Ultrasonic homogenization was performed for 1 min under the following conditions; The feeding tube is extended into the liquid metal, and rare earth, silicon carbide, aluminum oxide, titanium oxide, and titanium boride are blown into the liquid metal through the feeding tube in combination with air pressure, and then stirred and homogenized. Specifically, the following steps are included: a high temperature resistant feeding tube is extended into the liquid metal, and an air pressure feeding pump is connected; rare earth, silicon carbide, aluminum oxide, titanium oxide, and titanium boride are blown into the liquid metal through the feeding tube in combination with air pressure, and the air pressure is controlled so that there is no sputtering on the surface of the liquid metal; stirring and homogenizing are performed simultaneously, and the stirring speed is controlled to be 50-120r / min; so that the material is highly dispersed, the particles are completely embedded in the metal matrix, and a suitable interface is formed, thereby improving the performance of the aluminum alloy; The liquid metal is cooled down again, and when the solid and liquid coexist, it is introduced into the pressure cavity for pressure, liquid forging and pressure maintenance, and then heated to liquid in the melting furnace, and whiskers and boron nitride nanotubes are added; the specific steps include: cooling the liquid metal to 55-65°C, and when the solid and liquid coexist, the liquid metal is introduced into the pressure cavity for pressure, and the liquid forging pressure is controlled at 70-120MPa, and the temperature during pressure is controlled at 500-600°C, and then the pressure is maintained for 20-30s, so that the metal crystallizes and solidifies under pressure and the shrinkage cavities and shrinkage formed by solidification shrinkage are forcibly eliminated to obtain a material without casting defects; then the liquid metal is introduced into the melting furnace and heated to 700-750°C for liquid, and whiskers and boron nitride nanotubes are added; stirring is carried out at a speed of 50-100r / min for 2-3min; The liquid metal is cooled to between 580-650℃, injected into a mold preheated to 200-350℃ at a speed of 1.5-2m / s, cooled to obtain the finished product, and then acrylic emulsion is applied to the outside of the finished product, placed in an electrophoresis tank, connected to a power source to allow the emulsion to adhere, and heated to dryness to obtain an antioxidant reinforced coating. Example 3

[0022] according to Figure 1 As shown, this embodiment proposes a method for preparing a lightweight aluminum alloy, comprising the following steps: Prepare materials according to the following mass ratio: 5 parts of zinc, 5 parts of magnesium, 5 parts of nickel, 5 parts of copper, 5 parts of titanium, 3 parts of zirconium, 3 parts of beryllium, 3 parts of strontium, 3 parts of chromium, 10 parts of rare earth, 1 part of silicon carbide, 1 part of aluminum oxide, 1 part of titanium oxide, 1 part of titanium boride, 0.5 parts of whiskers, 0.5 parts of boron nitride nanotubes, 60 parts of aluminum ingots, and 50 parts of recycled aluminum; wherein the particle size of titanium oxide and titanium boride is 10 μm, the diameter of the whiskers is 0.1-2 um, and the length is 20-200 um, and the boron nitride nanotubes are selected to have a diameter of 60 nm and a length of 20 um; the boron nitride nanotubes are a mixture of NanoBarb powder and metallic aluminum, and the BNNB powder is uniformly dispersed in the aluminum to form aluminum-based master alloy reinforcement particles, and the boron nitride nanotubes reach the nanometer level, and the smaller the particles, the higher the possibility of improving the strength performance; The recycled aluminum is melted and refined to recover aluminum liquid, and then the aluminum ingot is melted into liquid, mixed with the recovered aluminum liquid to obtain a mixed liquid; specifically, the following steps are included: the recycled aluminum is placed in a smelting furnace, heated to 700-750°C, and smelted for 60-90 minutes to melt it; with inert gas nitrogen as a carrier, 1.0-1.5‰ granular refining agent is evenly blown into the aluminum liquid, and allowed to stand for 10-20 minutes to remove hydrogen and floating oxide inclusions inside; slag containing aluminum floating on the liquid surface is collected, and rotary calcined in a rotary kiln to separate ash and aluminum, and then the aluminum liquid therein is recovered into the smelting furnace to obtain total recovered aluminum liquid; then, the aluminum ingot is heated to 700-800°C, smelted for 50-80 minutes to melt it into liquid, and mixed with the recovered aluminum liquid to obtain a mixed liquid; Add zinc, magnesium, nickel, copper, titanium, zirconium, beryllium, strontium and chromium into a mixed liquid, and stir and melt the mixed liquid in a smelting furnace to form a liquid metal; specifically, the following steps are included: add zinc, magnesium, nickel, copper, titanium, zirconium, beryllium, strontium and chromium into the mixed liquid, and adjust the temperature in the smelting furnace to 700-800°C; stir for 10-20 minutes, and stop stirring when all the materials in the smelting furnace are melted into liquid to obtain liquid metal; The liquid metal is cooled down, and when the solid and liquid coexist, it is introduced into the pressure cavity for pressure, liquid forging and pressure maintenance, and then heated to liquid in a smelting furnace; the specific steps include: preparing a die-casting machine, applying lubricant to the pressure cavity, preheating the pressure cavity to 280-380°C for 2-3 minutes; cooling the liquid metal to 60-70°C, and when the liquid metal solid and liquid coexist, introducing it into the pressure cavity; pressurizing the pressure cavity, controlling the liquid forging pressure ratio at 70-130MPa, controlling the temperature during pressure to 550-600°C, and then maintaining the pressure for 30-45s; after completion, introducing it into a smelting furnace and heating it to 650-700°C to liquid; allowing the metal to crystallize and solidify under pressure and forcibly eliminating shrinkage cavities and shrinkage formed by solidification shrinkage to obtain a material without casting defects; The method comprises the following steps: adding a refining agent to the liquid metal for refining at 700-750°C, standing the liquid metal for 5-10 minutes after refining, and skimming the surface scum at 600-700°C; performing ultrasonic homogenization on the liquid metal at a frequency of 40 kHz and a power density of 0.8 W / cm 2 Ultrasonic homogenization was performed for 1 min under the following conditions; The feeding tube is extended into the liquid metal, and rare earth, silicon carbide, aluminum oxide, titanium oxide, and titanium boride are blown into the liquid metal through the feeding tube in combination with air pressure, and then stirred and homogenized. Specifically, the following steps are included: a high temperature resistant feeding tube is extended into the liquid metal, and an air pressure feeding pump is connected; rare earth, silicon carbide, aluminum oxide, titanium oxide, and titanium boride are blown into the liquid metal through the feeding tube in combination with air pressure, and the air pressure is controlled so that there is no sputtering on the surface of the liquid metal; stirring and homogenizing are performed simultaneously, and the stirring speed is controlled to be 50-120r / min; so that the material is highly dispersed, the particles are completely embedded in the metal matrix, and a suitable interface is formed, thereby improving the performance of the aluminum alloy; The liquid metal is cooled down again, and when the solid and liquid coexist, it is introduced into the pressure cavity for pressure, liquid forging and pressure maintenance, and then heated to liquid in the melting furnace, and whiskers and boron nitride nanotubes are added; the specific steps include: cooling the liquid metal to 55-65°C, and when the solid and liquid coexist, the liquid metal is introduced into the pressure cavity for pressure, and the liquid forging pressure is controlled at 70-120MPa, and the temperature during pressure is controlled at 500-600°C, and then the pressure is maintained for 20-30s, so that the metal crystallizes and solidifies under pressure and the shrinkage cavities and shrinkage formed by solidification shrinkage are forcibly eliminated to obtain a material without casting defects; then the liquid metal is introduced into the melting furnace and heated to 700-750°C for liquid, and whiskers and boron nitride nanotubes are added; stirring is carried out at a speed of 50-100r / min for 2-3min; The liquid metal is cooled to between 580-650℃, injected into a mold preheated to 200-350℃ at a speed of 1.5-2m / s, cooled to obtain the finished product, and then acrylic emulsion is applied to the outside of the finished product, placed in an electrophoresis tank, connected to a power source to allow the emulsion to adhere, and heated to dryness to obtain an antioxidant reinforced coating.

[0023] According to Example 1, Example 2 and Example 3, it can be concluded that the aluminum alloy prepared in the present invention has better mechanical properties and lighter weight by using the following mass ratio components: 2-5 parts of zinc, 2-5 parts of magnesium, 2-5 parts of nickel, 2-5 parts of copper, 2-5 parts of titanium, 1-3 parts of zirconium, 1-3 parts of beryllium, 1-3 parts of strontium, 1-3 parts of chromium, 5-10 parts of rare earth, 0.5-1 parts of silicon carbide, 0.5-1 parts of aluminum oxide, 0.5-1 parts of titanium oxide, 0.5-1 parts of titanium boride, 0.2-0.5 parts of whiskers, 0.3-0.5 parts of boron nitride nanotubes, 40-60 parts of aluminum ingots, and 30-50 parts of recycled aluminum.

[0024] Verification example:

[0025] The present invention uses aluminum ingots and recycled aluminum molten aluminum liquid as a matrix, and cooperates with zinc, magnesium, nickel, copper, titanium, zirconium, beryllium, strontium, and chromium to form an alloy, improves the crystal structure and mechanical properties of the aluminum alloy, and rare earths play a role in grain refinement during alloy crystallization, improves the strength and plasticity of the alloy, and uses aluminum oxide, titanium oxide, titanium boride, and whiskers as reinforcements to improve the mechanical properties of the aluminum alloy. Grain refinement during solidification by boron nitride nanotubes changes the microstructure of the metal, thereby changing its performance. After verification, it is achieved that the same mechanical strength as ordinary aluminum alloy is achieved, and the weight is compared with the original structure weight, and the weight loss is 40%, which helps to improve the economy of new energy vehicles. And the matrix material of the present invention uses recycled aluminum, and the planned processing flow is conducive to recycling and cost saving. At the same time, the present invention utilizes the characteristics of the metal when it transitions from liquid to solid or solid to liquid, and pressurizes, liquid forging and pressure-maintaining under two solid-liquid coexistences, so that the metal is crystallized and solidified under pressure and forced to eliminate the shrinkage cavity and shrinkage formed by solidification shrinkage, so as to obtain a material without casting defects. In addition, the present invention blows rare earth, silicon carbide, aluminum oxide, titanium oxide, and titanium boride into the interior of the liquid metal through a feeding pipe in combination with air pressure, and stirs and homogenizes the materials, so that the materials are highly dispersed, the particles are completely embedded in the metal matrix, and a suitable interface is formed, thereby improving the performance of the aluminum alloy. Finally, the present invention applies acrylic emulsion on the outside of the finished product, connects a power source to make the emulsion adhere, heats and dries to obtain an anti-oxidation strengthening coating, avoids oxidation of the aluminum alloy, and is convenient for storage.

[0026] The above shows and describes the basic principles, main features and advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. A method for preparing a lightweight aluminum alloy, characterized in that: The following steps are involved: S1: Prepare materials: zinc, magnesium, nickel, copper, titanium, zirconium, beryllium, strontium, chromium, rare earth, silicon carbide, aluminum oxide, titanium oxide, titanium boride, whiskers, boron nitride nanotubes and aluminum ingots, recycled aluminum; S2: Smelting and refining the recycled aluminum to recover the aluminum liquid, then melting the aluminum ingot into liquid and mixing it with the recovered aluminum liquid to obtain a mixed liquid; S3: adding zinc, magnesium, nickel, copper, titanium, zirconium, beryllium, strontium and chromium into a mixed liquid, stirring and melting the mixed liquid in a smelting furnace to form a liquid metal; S4: Cooling the liquid metal, waiting for the solid and liquid to coexist, introducing it into the pressure cavity for pressure application, liquid forging and pressure maintenance, and then heating it into liquid in the melting furnace; S5: adding a refining agent for refining, then standing to skim off the surface scum, and then performing ultrasonic homogenization; S6: Extend the feeding tube into the liquid metal, blow rare earth, silicon carbide, aluminum oxide, titanium oxide, and titanium boride into the liquid metal through the feeding tube with air pressure, and stir and homogenize; S7: Cooling the liquid metal again, waiting for the solid and liquid to coexist, introducing it into the pressure cavity for pressure application, liquid forging and pressure maintenance, and then heating it into liquid state into a melting furnace, adding whiskers and boron nitride nanotubes; S8: After cooling the liquid metal, press it into a mold, cool it to obtain a finished product, and perform an antioxidant treatment on the surface.

2. The method for preparing a lightweight aluminum alloy according to claim 1, characterized in that: In S1, materials are prepared according to the following mass ratios: 2-5 parts of zinc, 2-5 parts of magnesium, 2-5 parts of nickel, 2-5 parts of copper, 2-5 parts of titanium, 1-3 parts of zirconium, 1-3 parts of beryllium, 1-3 parts of strontium, 1-3 parts of chromium, 5-10 parts of rare earth, 0.5-1 parts of silicon carbide, 0.5-1 parts of aluminum oxide, 0.5-1 parts of titanium oxide, 0.5-1 parts of titanium boride, 0.2-0.5 parts of whiskers, 0.3-0.5 parts of boron nitride nanotubes, 40-60 parts of aluminum ingots, and 30-50 parts of recycled aluminum.

3. The method for preparing a lightweight aluminum alloy according to claim 2, characterized in that: The particle size of the titanium oxide and titanium boride is 10 μm, the diameter of the whisker is 0.1-2 μm, and the length is 20-200 μm. The boron nitride nanotube has a diameter of 60 nm and a length of 20 μm.

4. The method for preparing a lightweight aluminum alloy according to claim 2, characterized in that: The S2 comprises the following steps: S21: Put the recycled aluminum into a smelting furnace, heat it to 700-750°C, and smelt it for 60-90 minutes to melt it; S22: Using inert gas nitrogen as a carrier, 1.0-1.5‰ granular refining agent is evenly blown into the aluminum liquid, and allowed to stand for 10-20 minutes to remove the internal hydrogen and floating oxide slag; S23: collecting the aluminum-containing slag floating on the liquid surface, performing rotary calcination in a rotary kiln to separate the ash and aluminum, and then recovering the aluminum liquid therein to a smelting furnace to obtain a total recovered aluminum liquid; S24: Then, the aluminum ingot is heated to 700-800° C. and smelted for 50-80 minutes to be melted into liquid, and the liquid is mixed with the recovered aluminum liquid to obtain a mixed liquid.

5. The method for preparing a lightweight aluminum alloy according to claim 4, characterized in that: The S3 comprises the following steps: S31: adding zinc, magnesium, nickel, copper, titanium, zirconium, beryllium, strontium and chromium into a mixed solution, and adjusting the temperature in the smelting furnace to 700-800°C; S32: Stirring for 10-20 minutes, and when all the materials in the smelting furnace are melted into liquid, stirring is stopped to obtain liquid metal.

6. The method for preparing a lightweight aluminum alloy according to claim 5, characterized in that: The S4 comprises the following steps: S41: Prepare the die casting machine, apply lubricant in the pressure cavity, and preheat the pressure cavity to 280-380℃ for 2-3min; S42: Cooling the liquid metal to 60-70°C, waiting for the liquid metal to coexist in solid and liquid state, and then introducing the liquid metal into the pressurized cavity; S43: applying pressure to the pressure cavity, controlling the liquid forging pressure at 70-130 MPa, controlling the temperature at 550-600°C, and then maintaining the pressure for 30-45 seconds; S44: After completion, the mixture is introduced into a melting furnace and heated to 650-700°C to form a liquid.

7. The method for preparing a lightweight aluminum alloy according to claim 6, characterized in that: The S5 comprises the following steps: S51: adding a refining agent to the liquid metal at 700-750°C for refining, standing for 5-10 minutes after refining, and skimming off the surface scum at 600-700°C; S52: Ultrasonic homogenization of liquid metal at a frequency of 40 kHz and a power density of 0.8 W / cm 2 Ultrasonic homogenization was performed for 1 min.

8. The method for preparing a lightweight aluminum alloy according to claim 7, characterized in that: The S6 comprises the following steps: S61: Extend the high temperature resistant feeding pipe into the liquid metal and connect it to the air pressure feeding pump; S62: Blowing rare earth, silicon carbide, aluminum oxide, titanium oxide, and titanium boride into the liquid metal through a feeding pipe with air pressure, and controlling the air pressure so that no sputtering occurs on the surface of the liquid metal; S63: Stir and homogenize simultaneously, and control the stirring speed to 50-120r / min.

9. The method for preparing a lightweight aluminum alloy according to claim 8, characterized in that: The S7 comprises the following steps: S71: Cool the liquid metal to 55-65°C, wait for the liquid metal to coexist in solid and liquid, introduce it into the pressure cavity, apply pressure, control the liquid forging pressure at 70-120MPa, control the temperature during pressure application at 500-600°C, and then maintain the pressure for 20-30s; S72: then introducing the smelting furnace to heat to 700-750°C to liquid state, adding whiskers and boron nitride nanotubes; S73: Stir for 2-3 minutes at a rotation speed of 50-100 r / min.

10. The method for preparing a lightweight aluminum alloy according to claim 9, characterized in that: In S8, the liquid metal is cooled to between 580-650°C, injected into a mold preheated at 200-350°C at a speed of 1.5-2m / s, cooled to obtain a finished product, and then acrylic emulsion is applied to the outside of the finished product, placed in an electrophoresis tank, connected to a power source to allow the emulsion to adhere, and heated to dry to obtain an antioxidant reinforced coating.