Corrosion inhibitor and preparation method and application thereof

The corrosion inhibitor composed of citric acid, alanine and benzimidazole solves the corrosion problem of iron-based containers caused by chloride ions in the production of ammonium paratungstate, achieves container protection and improves product quality, and is low-cost and environmentally friendly.

CN118726982APending Publication Date: 2024-10-01HUBEI GREEN TUNGSTEN CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410711304.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-04
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

In the production process of ammonium paratungstate, chloride ions easily corrode iron-based containers, and existing corrosion inhibitors are ineffective and affect product quality.

Method used

A corrosion inhibitor composed of citric acid, alanine and benzimidazole is prepared by dispersing it in deionized water in a constant temperature water bath. It is used to protect tungstate production containers and use chemical adsorption to cover chloride ion corrosion.

Benefits of technology

It effectively extends the service life of the iron-based container and prevents new impurities from entering the tungstate solution. It is low-priced and environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004874111170000041
    Figure BDA0004874111170000041
Patent Text Reader

Abstract

The invention discloses a corrosion inhibitor as well as a preparation method and application thereof, which are used for solving the problem that chloride ions in a contact solution easily corrode an iron-based container in the production process of ammonium paratungstate. The invention relates to a corrosion inhibitor, which is composed of 2-5 mg / L of citric acid, 1-3 mg / L of alanine and 0.1-1 mg / L of benzimidazole, and a solvent is deionized water. The invention also provides a preparation method of the corrosion inhibitor, which comprises the following steps: sequentially dispersing the citric acid, the alanine and the benzimidazole in the deionized water under a constant-temperature water bath condition, and cooling to obtain the corrosion inhibitor. According to the corrosion inhibitor, after the citric acid, the alanine and the ammonium tungstate are compounded, a slow release effect is easily generated, chemical adsorption of the benzimidazole can effectively cover a container to isolate the corrosion effect of chloride ions, meanwhile, the composition does not bring new impurities into a tungstate solution, and the composition is low in price and small in environmental pollution.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of corrosion prevention, and in particular relates to a corrosion inhibitor and a preparation method and application thereof. Background Art

[0002] At present, in the process of preparing ammonium paratungstate products, hydrochloric acid is often used as an acidifying agent, and a large amount of chloride ions remain in the solution. Due to the small ion radius of chloride ions, they have a strong corrosion penetration effect on iron-based containers and are prone to pitting corrosion. Therefore, in order to improve the service life of iron-based containers in contact with the solution on the ammonium paratungstate product production line, it is necessary to protect the containers in contact with tungstate solutions. The corrosion inhibitors currently used cannot play a good protective role. At the same time, the addition of corrosion inhibitors leads to a decrease in the quality of ammonium paratungstate products. Summary of the invention

[0003] The invention aims to solve the problem that chloride ions in a contact solution are prone to corrode an iron-based container during the production of ammonium paratungstate, and provides a corrosion inhibitor, a preparation method and an application thereof.

[0004] In the first aspect, a corrosion inhibitor adopts the following technical solution:

[0005] A corrosion inhibitor, wherein the corrosion inhibitor components consist of 2-5 mg / L of citric acid, 1-3 mg / L of alanine and 0.1-1 mg / L of benzimidazole, and the solvent is deionized water.

[0006] Furthermore, the corrosion inhibitor component consists of 2 mg / L citric acid, 3 mg / L alanine and 1 mg / L benzimidazole, and the solvent is deionized water.

[0007] Furthermore, the corrosion inhibitor component consists of 5 mg / L citric acid, 1 mg / L alanine and 0.1 mg / L benzimidazole, and the solvent is deionized water.

[0008] Furthermore, the corrosion inhibitor component consists of 4 mg / L citric acid, 2 mg / L alanine and 0.5 mg / L benzimidazole, and the solvent is deionized water.

[0009] Preferably, the corrosion inhibitor component consists of 3 mg / L citric acid, 2 mg / L alanine and 0.3 mg / L benzimidazole, and the solvent is deionized water.

[0010] In the second aspect, a method for preparing a corrosion inhibitor adopts the following technical solution:

[0011] A method for preparing a corrosion inhibitor comprises the following steps: dispersing citric acid, alanine and benzimidazole in deionized water in sequence under a constant temperature water bath condition, and cooling to obtain the corrosion inhibitor.

[0012] Preferably, the constant temperature water bath temperature is 55-65°C.

[0013] In the third aspect, an application of a corrosion inhibitor adopts the following technical solution:

[0014] An application of a corrosion inhibitor, wherein any of the above-mentioned corrosion inhibitors is applied to container protective materials produced by tungstate.

[0015] Beneficial effects of the present invention:

[0016] The corrosion inhibitor provided by the present invention can easily produce a slow-release effect after compounding citric acid, alanine and ammonium tungstate, and the chemical adsorption of benzimidazole can effectively cover the corrosion effect of isolating chloride ions in the container. At the same time, the composition will not introduce new impurities into the tungstate solution, is low in price, and has little environmental pollution. DETAILED DESCRIPTION

[0017] The following is a further detailed description of a corrosion inhibitor, a preparation method and an application thereof described in the present invention in conjunction with the examples. For the sake of simplicity of description, this document cannot enumerate all alternative technical features and implementation schemes contained in the present invention. Therefore, those skilled in the art should know that any technical features and implementation schemes in this embodiment do not limit the scope of protection of the present invention, which includes any alternative technical features and implementation schemes adopted by all those skilled in the art without creative labor. Specifically, the implementation schemes obtained by replacing any technical feature in the present invention or combining any two or more technical features provided by the present invention should be within the scope of protection of the present invention.

[0018] If no specific techniques and conditions are specified in the examples, the procedures are carried out according to the techniques and conditions described in the literature in the art or according to the product instructions. If no manufacturer is specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0019] Example

[0020] Example 1

[0021] Example 1 provides a corrosion inhibitor, the corrosion inhibitor components consist of 2 mg / L citric acid, 3 mg / L alanine and 1 mg / L benzimidazole, and the solvent is deionized water.

[0022] Example 1 also provides a method for preparing a corrosion inhibitor, comprising the following steps: dispersing citric acid, alanine and benzimidazole in deionized water in sequence under a constant temperature water bath at 60° C., and cooling to room temperature to obtain the corrosion inhibitor.

[0023] Example 2

[0024] Example 2 provides a corrosion inhibitor, the corrosion inhibitor components consist of 5 mg / L citric acid, 1 mg / L alanine and 0.1 mg / L benzimidazole, and the solvent is deionized water.

[0025] The method for preparing a corrosion inhibitor provided in Example 2 is the same as that in Example 1.

[0026] Example 3

[0027] Example 3 provides a corrosion inhibitor, the corrosion inhibitor components consist of 4 mg / L citric acid, 2 mg / L alanine and 0.5 mg / L benzimidazole, and the solvent is deionized water.

[0028] The method for preparing a corrosion inhibitor provided in Example 3 is the same as that in Example 1.

[0029] Example 4

[0030] Example 4 provides a corrosion inhibitor, the corrosion inhibitor components consist of 3 mg / L citric acid, 2 mg / L alanine and 0.3 mg / L benzimidazole, and the solvent is deionized water.

[0031] The method for preparing a corrosion inhibitor provided in Example 4 is the same as that in Example 1.

[0032] Comparative Example

[0033] Comparative Example 1

[0034] Comparative Example 1 provides a corrosion inhibitor, the corrosion inhibitor component is 6.5 mg / L of citric acid, and the solvent is deionized water.

[0035] Comparative Example 2

[0036] Comparative Example 2 provides a corrosion inhibitor, the corrosion inhibitor component is 6.5 mg / L of alanine, and the solvent is deionized water.

[0037] Comparative Example 3

[0038] Comparative Example 3 provides a corrosion inhibitor, the corrosion inhibitor component is 6.5 mg / L benzimidazole, and the solvent is deionized water.

[0039] Corrosion inhibition performance test

[0040] The material of the test piece is consistent with the 304 stainless steel commonly used in the ammonium paratungstate production line. The test piece is prepared according to the provisions of 4.7.5 "Test piece" in SY / T5273-2014 to perform the test.

[0041] The amount of medium used is per 1cm 2The surface area of ​​the test piece is 20 ml of tungstate solution for production. The corrosion inhibitors provided in Examples 1-4 and Comparative Examples 1-3 are added during the production of the tungstate solution. A control group (no corrosion inhibitor) is provided at the same time. The test temperature is 60+1°C and placed at a constant temperature for 7-14 days. The corrosion inhibition rate is calculated in accordance with 4.7.7.1 of SY / T5273-2014. The test results are shown in Table 1 below.

[0042] Table 1 Corrosion inhibitor test results of Examples 1-4 and Comparative Examples 1-3

[0043]

[0044] For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here, and the obvious changes or modifications derived from them are still within the scope of protection of the claims of the invention.

Claims

1. A corrosion inhibitor, characterized in that: The corrosion inhibitor component consists of 2-5 mg / L of citric acid, 1-3 mg / L of alanine and 0.1-1 mg / L of benzimidazole, and the solvent is deionized water.

2. A corrosion inhibitor according to claim 1, characterized in that: The corrosion inhibitor component consists of 2 mg / L citric acid, 3 mg / L alanine and 1 mg / L benzimidazole, and the solvent is deionized water.

3. A corrosion inhibitor according to claim 1, characterized in that: The corrosion inhibitor component consists of 5 mg / L citric acid, 1 mg / L alanine and 0.1 mg / L benzimidazole, and the solvent is deionized water.

4. A corrosion inhibitor according to claim 1, characterized in that: The corrosion inhibitor component consists of 4 mg / L citric acid, 2 mg / L alanine and 0.5 mg / L benzimidazole, and the solvent is deionized water.

5. A corrosion inhibitor according to claim 1, characterized in that: The corrosion inhibitor component consists of 3 mg / L citric acid, 2 mg / L alanine and 0.3 mg / L benzimidazole, and the solvent is deionized water.

6. A method for preparing a corrosion inhibitor, characterized in that: The following steps are involved: Under constant temperature water bath conditions, citric acid, alanine and benzimidazole are dispersed in deionized water in sequence and cooled to obtain the corrosion inhibitor.

7. The method for preparing a corrosion inhibitor according to claim 6, characterized in that: The temperature of the constant temperature water bath is 55-65℃.

8. An application of a corrosion inhibitor, characterized in that: The corrosion inhibitor described in any one of claims 1 to 5 is applied to container protective materials for tungstate production.

Citation Information

Patent Citations

  • Corrosion inhibitor composition and preparation method and application thereof

    CN108842154A

  • Amino acid vapor phase corrosion inhibitor as well as preparation method and application thereof

    CN116641056A

  • Improvements in and relating to corrosion inhibition

    GB1235468A

  • Mixture for inhibition of corrosion of metals

    US5785896A