Method for preparing zinc sulfide antireflection surface through femtosecond laser direct writing auxiliary wet etching

Using femtosecond laser direct writing assisted wet etching technology, a high depth-to-aspect ratio sub-wavelength microstructured anti-reflective surface is prepared, which solves the problem of difficulty in balancing manufacturing efficiency and anti-reflective performance in the existing technology, and achieves efficient and stable Light transmission anti-reflection effect.

CN118727157APending Publication Date: 2024-10-01SICHUAN UNIV

Patent Information

Application Number
CN202410965680.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing femtosecond laser direct writing technology cannot simultaneously meet high manufacturing efficiency and high anti-reflection performance, which limits its industrial application in detectors, flat panel displays, solar cells and other fields.

Method used

The femtosecond laser direct writing assisted wet etching method is used, which is converted into a Bessel beam through an axicon lens, focused on the lower surface of the zinc sulfide crystal for periodic grid scanning, and etched with 28% hydrogen peroxide and 30% ammonia. Ultrasonic wet etching is carried out in liquid to prepare a sub-wavelength microstructured anti-reflective surface with high aspect ratio.

Benefits of technology

A high-efficiency, low-cost preparation process is achieved, and the generated microstructure exhibits good anti-reflection effects in a wide spectral range, is structurally stable, and can withstand high temperature, high pressure, and corrosion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

The invention discloses a method for preparing a zinc sulfide antireflection surface through femtosecond laser direct writing assisted wet etching. The method specifically comprises the steps that periodic scanning modification is conducted on the lower surface of a zinc sulfide crystal through Bessel ultrafast laser, and then ultrasonic wet etching is conducted on a sample through etching liquid; the zinc sulfide anti-reflection surface with the high aspect ratio microstructure array is prepared, and the good anti-reflection effect can be achieved in the wide spectral range.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of optical components, and in particular relates to a femtosecond laser micro-nano precision processing technology and a preparation method. Background Art

[0002] Fresnel reflection on the surface of materials leads to a decrease in light transmission efficiency. How to reduce energy loss during light transmission is of great significance in fields such as detectors, flat-panel displays, and solar cells. Femtosecond laser direct writing technology has become a promising method for manufacturing anti-reflective microstructures due to its advantages such as high processing accuracy, no need for masks, and wide applicability to materials. However, the current femtosecond laser direct writing technology for preparing infrared anti-reflective surfaces generally cannot meet both high manufacturing efficiency and high anti-reflective performance at the same time, and cannot meet the needs of industrial applications.

[0003] At present, there have been studies on the use of femtosecond laser direct writing to prepare subwavelength structures and apply them to infrared anti-reflection designs, achieving anti-reflection in broadband mid-infrared. For example, Sikun Zhou et al. (Photonics, 2023, 10, 479.) used femtosecond lasers to prepare periodic hole arrays on the surface of zinc selenide, and the maximum single-sided transmittance reached 82% (the limit value is 82.3%). For example, Haoran Wang et al. (Optics and Laser Technology, 149, (2022), 107931.) used femtosecond lasers to prepare moth-eye microstructures on the surface of zinc sulfide by rapid scanning, and prepared an anti-reflection surface based on the moth-eye structure. The transmittance of the prepared double-sided anti-reflection surface reached 87%. In the recent patent application CN116425431A, "Anti-reflection structure on the surface of a chalcogenide glass and its preparation method", a femtosecond laser is used to directly ablate conical-shaped elongated micropores on the surface of a chalcogenide glass sample, thereby obtaining an anti-reflection microstructure. Although the preparation efficiency is relatively high, a large number of nano-scale particle structures will exist on the surface of the microstructure, resulting in poor anti-reflection effect. The above method can use a femtosecond laser to prepare an anti-reflection structure on the surface of a material, but it cannot simultaneously meet high manufacturing efficiency and high anti-reflection performance, which limits its practical application. Summary of the invention

[0004] The technical problem to be solved by the present invention is to propose a method for preparing a zinc sulfide anti-reflection surface by wet etching of femtosecond laser direct writing corrosion in view of the shortcomings of the prior art. The method has low cost, simple process, high efficiency, and the prepared microstructure array has a high aspect ratio, a uniform structural period, good anti-reflection and anti-reflection effect, and can show a good anti-reflection effect in a wide spectral range.

[0005] In order to achieve the above-mentioned purpose, the present invention adopts the technical solution composed of the following technical measures to achieve it.

[0006] The preparation method based on femtosecond laser direct writing assisted wet etching of the present invention has the following process steps:

[0007] (1) The femtosecond laser is converted into a Bessel beam through a conical lens, and the ultrafast laser is beam-contracted through a 4f system.

[0008] (2) The double-sided polished zinc sulfide crystal material is fixed on an electrically controlled translation stage, and a femtosecond laser beam is focused onto the lower surface of the material for periodic grid scanning modification.

[0009] (3) The zinc sulfide sample modified by direct writing is placed in an etching solution prepared by a certain ratio of 28% hydrogen peroxide and 30% ammonia water, and the modified sample is subjected to ultrasonic wet etching. After the etching is completed, it is washed with clean water to obtain a sample of the zinc sulfide anti-reflection surface.

[0010] The femtosecond laser parameters in step (1) of the above method are: laser wavelength of 1030nm, average power of 100-500mW, pulse width of 0.2-6ps, and repetition frequency of 100-500kHz.

[0011] The base angle of the conical lens in step (1) of the above method is 2°, and the 4f system is composed of a plano-convex lens with a focal length of 150 mm and a 100x microscope objective lens with an equivalent focal length of 2 mm.

[0012] The lower surface of the material described in step (2) of the above method also includes the lower surface after direct writing once and then flipping over.

[0013] The processing speed in step (2) of the above method is 0.1-0.5 mm / s.

[0014] In the above method, the ratio of hydrogen peroxide in step (3) is 1:1-5:1.

[0015] The wet etching time in step (3) of the above method is 1-3 hours.

[0016] The aspect ratio of the periodic microstructure prepared in step (3) of the above method is between 0.5 and 5.

[0017] The period of the periodic microstructure prepared in step (3) of the above method is 1-5 μm.

[0018] The sample of the zinc sulfide anti-reflection surface in step (3) of the above method can be single-sided or double-sided.

[0019] Compared with the related art, the method for preparing zinc sulfide anti-reflection surface by femtosecond laser direct writing assisted wet etching provided by the present invention has the following beneficial effects:

[0020] The present invention adopts Bessel femtosecond laser to modify the lower surface of zinc sulfide crystal, and then ultrasonically etches the sample. It is not necessary to design a complex motion path, which greatly simplifies the process and has high processing efficiency. The reason why the present invention designs and chooses to modify the lower surface of zinc sulfide is that when the femtosecond laser passes through the crystal, a nonlinear effect is generated, and a modified area with a high aspect ratio is induced on the lower surface, that is, only the refractive index is changed, and no structural damage is generated. At the same time, the microstructure induced by the femtosecond laser when it is focused on the upper surface is avoided to scatter the incident light, resulting in difficulty in forming a high aspect ratio structure. The anti-reflection surface designed by the present invention has a sub-wavelength microstructure on the surface of the crystal, which has stable physical and chemical properties, can withstand high temperature and high pressure, is not sensitive to external corrosion and pollution, and has a damage threshold equivalent to the material substrate, and the service life is greatly improved. The present invention generates a periodically arranged sub-wavelength microstructure on the surface of the zinc sulfide crystal, designs and manufactures an anti-reflection surface, and lays a foundation for the research and development of femtosecond laser preparation of anti-reflection surfaces. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention will be further described in detail below with reference to the accompanying drawings, in which:

[0022] Figure 1 This is a schematic diagram of the femtosecond laser direct writing optical path of the present invention;

[0023] Figure 2 is a microscopic structure diagram of the anti-reflection surface of the present invention;

[0024] Figure 3 This is a transmission spectrum test chart of the anti-reflection surface of the present invention. DETAILED DESCRIPTION

[0025] The preferred embodiments of the present invention will be described in detail below in conjunction with the accompanying drawings; it should be understood that the preferred embodiments are only for illustrating the present invention rather than for limiting the protection scope of the present invention.

[0026] (1) Femtosecond laser direct writing modification: The ultrafast laser 13 pulse is transmitted through the reflector 1, half-wave plate 2, beam splitter 3 and mechanical shutter 5, and then through the quarter-wave plate 6. After being reflected by the conical lens 7 (bottom angle is 2°), lens 8 (plano-convex lens with focal length of 150 mm) and reflector 9 to the microscope objective 10 (100 times microscope objective with equivalent focal length of 2 mm, NA = 0.8), it is focused on the lower surface of the sample 11. The sample is fixed on the three-dimensional electric control platform 12. The irradiation process is monitored by the CCD camera 14, and the power meter 4 is used to detect the real-time laser power. Take a zinc sulfide sample with a size of 10 mm × 10 mm × 1 mm and polished on both sides, clean it and fix it on the three-dimensional electric control platform; when the ultrafast laser is directly written on the surface of the zinc sulfide sample, the pulse width is 400 fs, the central wavelength is 1030 nm, and the repetition frequency is 25 kHz; the average power of the femtosecond laser is 350 mW, and the scanning speed is 0.4 mm / s.

[0027] (2) Wet etching: The zinc sulfide crystal modified by femtosecond laser direct writing is placed in an etching solution prepared by mixing 28% hydrogen peroxide and 30% ammonia water in a ratio of 3:1, and ultrasonic wet etching is performed for 2 hours. After the etching is completed, it is washed with water to obtain a sample with an anti-reflective surface microstructure. The anti-reflective surface microstructure is as follows: Figure 2 shown.

[0028] (3) Anti-reflection surface test: Use Fourier infrared spectrometer to test and analyze the anti-reflection surface. The test transmittance spectrum is Figure 3 As shown, the transmission spectrum in the wavelength range of 3-13μm was tested, where Curve 1 is the transmittance curve of the original unprocessed bulk crystal, and Curve 2 is the zinc sulfide sample with a single-sided anti-reflection microstructure prepared by the invention method, which achieves anti-reflection in the range of 6-13μm, with a maximum of 85.6%. Compared with the transmittance of 73% of the original unprocessed surface, the transmittance is increased by 12.6%.

[0029] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Obviously, those skilled in the art may make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. A method for preparing zinc sulfide anti-reflection surface by femtosecond laser direct writing assisted wet etching, characterized in that: The specific steps of this method are as follows: (1) Configuring a femtosecond laser processing system: placing an aconic lens in the femtosecond laser processing optical path, allowing the laser beam to pass through the center of the aconic lens, be reduced by a 4f system, and be tightly focused by a microscope objective lens; (2) Fix the zinc sulfide crystal on the displacement platform, keep the laser incident direction perpendicular to the optical axis of the zinc sulfide crystal, and focus on the lower surface of the crystal material sample along the direction of the optical axis; turn on the femtosecond laser preparation system for laser direct writing. During the laser direct writing process, a CCD camera can be used to observe the direct writing of the femtosecond laser in real time; (3) immersing the sample after the above treatment in a wet etching solution and performing ultrasonic wet etching to obtain a high aspect ratio periodic microstructure array, and then washing the crystal material after wet etching with clean water to obtain a zinc sulfide anti-reflection surface sample with a microstructure array; The femtosecond laser direct writing processing parameters described in the steps of the above method are: laser wavelength of 1030nm, average power of 100-500mW, pulse width of 50-600fs, repetition frequency of 10-500kHz; processing speed of 0.05-1mm / s.

2. The method for preparing zinc sulfide anti-reflection surface by femtosecond laser direct writing assisted wet etching according to claim 1, characterized in that: The focusing on the modification of the lower surface of the material also includes the lower surface after flipping.

3. The method for preparing zinc sulfide anti-reflection surface by femtosecond laser direct writing assisted wet etching according to claim 1, characterized in that: The prepared zinc sulfide anti-reflection surface includes single-sided and double-sided structures.

4. The method for preparing zinc sulfide anti-reflection surface by femtosecond laser direct writing assisted wet etching according to claim 1, characterized in that: The wet etching solution is composed of hydrogen peroxide and ammonia water.

5. The method for preparing zinc sulfide anti-reflection surface by femtosecond laser direct writing assisted wet etching according to claim 1, characterized in that: The aspect ratio of the prepared periodic microstructure is between 0.5 and 5.

6. The method for preparing zinc sulfide anti-reflection surface by femtosecond laser direct writing assisted wet etching according to claim 1, characterized in that: The period of the prepared periodic microstructure is 1-5 μm.

Citation Information

Patent Citations

  • Chalcogenide glass surface antireflection structure and preparation method thereof

    CN116425431A

Cited By

  • Design and manufacturing method of medium-long wave infrared anti-reflection microstructure window

    CN119148374A

  • Method for preparing antireflection surface on metal copper surface

    CN120460884A