Marine cable manufacturing and processing technology
By mixing polypropylene resin, EPDM rubber, modified nano-silica and additives to form a marine cable, the problem of aging of traditional cables under ultraviolet light and sea water is solved, and the mechanical, light-aging resistance, and anti-aging properties of the cable are improved. Waterproof and corrosion resistant for high performance marine rope applications.
Patent Information
- Application Number
- CN202410876452.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-02
- Publication Date
- 2024-10-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Traditional ship cables age under the influence of ultraviolet light and seawater impact, resulting in reduced mechanical properties and lack of UV resistance, waterproofing and corrosion resistance, making them unable to meet higher technical demands for ship cables.
Using a mixing process of polypropylene resin, EPDM rubber, modified nano-silica and additives, and melting and blending spinning through a twin-screw extruder, a marine cable with high mechanical properties is formed. Silica and additives improve the cable's wear resistance, photoaging resistance, waterproofing and corrosion resistance.
The produced marine cable has excellent mechanical properties, abrasion resistance, photoaging resistance, waterproofing and corrosion resistance, has long-term and stable performance, and is suitable for use in the field of ship cables.
Smart Images

Figure BDA0004923200700000021 
Figure BDA0004923200700000031 
Figure BDA0004923200700000032
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of cables, and in particular relates to a manufacturing process for a ship cable. Background Art
[0002] Ship cables are safety ropes used on ships. They are multi-strand ropes used to tie ships together. They are also an important tool. They can tow and fix ships. Cables can also be used to fix various equipment. Therefore, ship cables often need to have high tensile strength. However, when ships are operating at sea, ship cables are often exposed to the outdoors, and traditional ship cables do not have UV resistance. When exposed to ultraviolet light for a long time, they are prone to aging, which reduces the mechanical properties of the cables and the service life of the cables. In addition, the impact and erosion of ship cables by seawater will also cause the performance of the cables to decline. Therefore, it is urgent to invent a cable with UV resistance, waterproofness and corrosion resistance to meet the higher demands in the field of ship cable technology. Summary of the invention
[0003] The purpose of the present invention is to overcome the defects of the prior art and provide a manufacturing process for a ship cable.
[0004] The purpose of the present invention can be achieved through the following technical solutions:
[0005] A ship cable manufacturing process, comprising the following steps:
[0006] The polypropylene resin, EPDM rubber, antioxidant, modified nano-silica, additives and initiator are mixed and added into a twin-screw extruder for melt blending and spinning. The filaments are formed into cable filaments through cooling and blowing, cooling, solidification, and winding. The marine cables are then woven into marine cables according to the requirements.
[0007] Furthermore, the raw materials are calculated in parts by weight as follows: 80-100 parts of polypropylene resin, 10-14 parts of ethylene propylene diene rubber, 4-6 parts of antioxidant, 12-16 parts of modified nano-silicon dioxide, 5-10 parts of auxiliary agent, and 0.1-0.3 parts of initiator.
[0008] Furthermore, the initiator is one of benzoyl peroxide and lauroyl peroxide.
[0009] Furthermore, the antioxidant is one of antioxidant 1010 and antioxidant 264.
[0010] The manufactured marine cable is based on polypropylene resin, which gives the cable higher mechanical properties and wear resistance; the addition of EPDM rubber improves the cable's aging resistance.
[0011] Furthermore, the modified nano-silicon dioxide is prepared by the following steps:
[0012] Disperse nano-silica in a three-necked flask filled with toluene, and after ultrasonic treatment for 10 minutes, add 3-aminopropyltrimethoxysilane (silane coupling agent KH-540), slowly heat to 75°C under strong mechanical stirring, react for 8 hours, cool to room temperature after the reaction, take the filter residue after suction filtration, wash it with anhydrous ethanol 3-4 times, and dry it in a vacuum oven at 60°C to obtain modified nano-silica; the ratio of nano-silica, toluene, and 3-aminopropyltrimethoxysilane is 10g:100mL:15g;
[0013] There are many -OH groups on the surface of nano-silica, which can be introduced into -NH2 active groups by reacting with KH-540 to obtain modified nano-silica. The specific reaction process is as follows:
[0014]
[0015] Nano-silica has good wear resistance. By modifying it and grafting organic molecular chains by chemical bonding, that is, forming an organic layer on its surface, the interfacial compatibility between the modified nano-silica and the matrix can be greatly improved, thereby promoting the uniform dispersion of the modified nano-silica in the matrix, so that the performance of the modified nano-silica can be fully exerted, and the wear resistance of the matrix can be greatly improved. In addition, nano-silica also acts as a reinforcement material to enhance the mechanical properties of the matrix.
[0016] Furthermore, the auxiliary agent is prepared by the following steps:
[0017] S1. In a three-necked flask equipped with a stirring device, vinyl acetic acid, 4-amino-3-fluorophenol, dicyclohexylcarbodiimide (DCC, a dehydrating agent) and toluene were mixed and stirred uniformly, and reacted for 3 hours under a 50° C. water bath condition. After the reaction was completed, the mixture was filtered and the solvent was removed by distillation under reduced pressure to obtain intermediate 1; the ratio of vinyl acetic acid, 4-amino-3-fluorophenol, dicyclohexylcarbodiimide and toluene was 8.6 g:12.7 g:20.6 g:75 mL;
[0018] The carboxyl group on vinyl acetic acid and the amino group on 4-amino-3-fluorophenol undergo an amidation reaction. Under the action of a dehydrating agent, the reaction can be carried out under relatively mild conditions to obtain intermediate 1. The specific reaction process is as follows:
[0019]
[0020] S2. In a three-necked flask equipped with a stirring device, 2,2,6,6-tetramethylpiperidinol, n-octane and molybdenum trioxide were mixed and stirred evenly, heated to 80°C, and tert-butyl hydroperoxide aqueous solution (mass fraction 18%) was added dropwise. After the addition was completed, the reaction was refluxed for 9 hours. After the reaction was completed, the filtrate was filtered, activated carbon was added to the filtrate and stirred for 1 hour, allowed to stand, filtered, the filtrate was taken, and n-octane was removed by vacuum distillation to obtain intermediate 2; the ratio of 2,2,6,6-tetramethylpiperidinol, n-octane, molybdenum trioxide and tert-butyl hydroperoxide aqueous solution was 15.7 g:50 mL:0.4 g:15 mL;
[0021] Under the catalysis of molybdenum trioxide and the oxidation of tert-butyl hydroperoxide, 2,2,6,6-tetramethylpiperidinol and n-octane undergo a free radical coupling reaction; n-octane participates in the reaction process as a reactant and also acts as a reaction solvent, which can reduce the formation of by-products to obtain intermediate 2; the specific reaction process is as follows:
[0022]
[0023] S3, in a three-necked flask equipped with a stirring device, the intermediate 1, trimesoyl chloride and toluene were mixed and stirred uniformly, and then dicyclohexylcarbodiimide (dehydrating agent) was added, and the temperature was raised to 65°C for reaction for 5 hours. Stirring was continued during the reaction. After the reaction was completed, the mixture was filtered, and part of the solvent was removed by rotary evaporation. The mixture was purified by column chromatography (the eluent was a mixed solvent of benzene / ethyl acetate in a volume ratio of 3:2), and the eluent was removed by rotary evaporation to obtain intermediate 3; the ratio of the amount of intermediate 1, trimesoyl chloride, toluene and dicyclohexylcarbodiimide was 38.9 g:28.8 g:150 mL:41.2 g;
[0024] Under the action of dicyclohexylcarbodiimide, intermediate 1 and trimesoyl chloride undergo acylation reaction, and intermediate 3 is obtained by controlling the molar ratio of the two to be close to 2:1 and the trimesoyl chloride to be slightly excessive. The specific reaction process is as follows:
[0025]
[0026] S4. In a three-necked flask equipped with a stirring device, the intermediate 3, the intermediate 2 and toluene are mixed and stirred uniformly, and then dicyclohexylcarbodiimide (dehydrating agent) is added, and the reaction temperature is controlled to 70°C, and the reaction is carried out for 6 hours. Stirring is continued during the reaction. After the reaction is completed, the mixture is filtered, and distilled under reduced pressure. Then, the mixture is purified by column chromatography (the eluent is a mixed solvent of benzene / ethyl acetate, and the volume ratio of the two is 3:4), and the eluent is removed by rotary evaporation to obtain an auxiliary agent; the ratio of the amount of intermediate 1, intermediate 2, toluene and dicyclohexylcarbodiimide is 58.2g:28.5g:150mL:20.6g;
[0027] Under the action of dicyclohexylcarbodiimide, intermediate 3 and intermediate 2 undergo acylation reaction to obtain an auxiliary agent; the specific reaction process is as follows:
[0028]
[0029] The auxiliary agent molecule prepared by the present invention contains a CF bond, a hindered amine and a long carbon chain structure, wherein the CF bond has a high chemical bond strength and good stability, and can give the substrate significant water resistance; and can coat the CC main chain, reduce the surface energy of the substrate, and improve the corrosion resistance of the substrate; in addition, the hindered amine plays the role of a light stabilizer, decomposes hydrogen dioxide to produce stable nitroxide free radicals in light protection, and this compound can very effectively capture the free radicals produced in photo-oxidative degradation, can effectively inhibit the photo-oxidative degradation of the substrate, and can be regenerated under stable conditions, significantly improving the anti-ultraviolet aging performance of the substrate; finally, the long carbon chain belongs to a methylene chain segment, which not only has a strong hydrophobicity, improves the water resistance of the substrate, but also improves the toughness of the substrate, and can be interspersed in the molecular chain of the substrate to improve stability;
[0030] It should be noted that one end of the additive also contains a carbon-carbon double bond, which can cross-link with the matrix, enhance the interaction with the matrix, make the additive difficult to migrate and fall off, and improve the durability of performance.
[0031] Beneficial effects of the present invention:
[0032] 1. The marine cable prepared by the present invention uses polypropylene resin as a matrix, which gives the cable excellent mechanical properties and wear resistance; the addition of EPDM rubber improves the cable's aging resistance;
[0033] 2. Adding modified nano-silica has better compatibility with the matrix than ordinary nano-silica, significantly reduces the agglomeration phenomenon, and further improves the wear resistance and mechanical properties of the cable;
[0034] 3. The prepared additives significantly enhance the cable's light aging resistance, water resistance, corrosion resistance and a certain degree of mechanical properties, and the performance is long-lasting and stable;
[0035] Therefore, the cable produced by the present invention has stable and efficient aging resistance, waterproofness, corrosion resistance and wear resistance, and excellent mechanical properties, and has important application value in the field of ship cable technology. DETAILED DESCRIPTION
[0036] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0037] Example 1
[0038] Preparation of modified nano-silica:
[0039] Disperse 10 g of nano-silica in a three-necked flask filled with 100 mL of toluene. After ultrasonication for 10 min, add 15 g of 3-aminopropyltrimethoxysilane and slowly heat to 75 °C under strong mechanical stirring. React for 8 h. After the reaction is completed, cool to room temperature, filter and collect the residue, wash it with anhydrous ethanol for 4 times, and dry it in a vacuum oven at 60 °C to obtain modified nano-silica.
[0040] Example 2
[0041] Preparation aids:
[0042] S1. In a three-necked flask equipped with a stirring device, 8.6 g of vinyl acetic acid, 12.7 g of 4-amino-3-fluorophenol, 20.6 g of dicyclohexylcarbodiimide and 75 mL of toluene were mixed and stirred evenly, and reacted for 3 h in a water bath at 50° C. After the reaction was completed, the mixture was filtered and the solvent was removed by distillation under reduced pressure to obtain intermediate 1;
[0043] S2. In a three-necked flask equipped with a stirring device, 15.7 g of 2,2,6,6-tetramethylpiperidinol, 50 mL of n-octane, and 0.4 g of molybdenum trioxide were mixed and stirred evenly, heated to 80°C, and 15 mL of tert-butyl hydroperoxide aqueous solution (mass fraction 18%) was added dropwise. After the addition was completed, the reaction was refluxed for 9 h. After the reaction was completed, the filtrate was filtered, activated carbon was added to the filtrate, and stirred for 1 h. The mixture was allowed to stand, filtered, and the filtrate was taken. The n-octane was removed by distillation under reduced pressure to obtain intermediate 2.
[0044] S3, in a three-necked flask equipped with a stirring device, 38.9 g of intermediate 1, 28.8 g of trimesoyl chloride and 150 mL of toluene were mixed and stirred evenly, and then 41.2 g of dicyclohexylcarbodiimide was added, and the temperature was raised to 65 ° C. and reacted for 5 h. Stirring was continued during the reaction. After the reaction was completed, the reaction was filtered, and part of the solvent was removed by rotary evaporation. Then, it was purified by column chromatography (the eluent was a mixed solvent of benzene / ethyl acetate, and the volume ratio of the two was 3:2), and the eluent was removed by rotary evaporation to obtain intermediate 3;
[0045] S4. In a three-necked flask equipped with a stirring device, 58.2 g of intermediate 3, 28.5 g of intermediate 2 and 150 mL of toluene were mixed and stirred evenly, and then 20.6 g of dicyclohexylcarbodiimide was added, and the reaction temperature was controlled to 70°C. The reaction was carried out for 6 hours with continuous stirring during the reaction. After the reaction was completed, the mixture was filtered, evaporated under reduced pressure, and purified by column chromatography (the eluent was a mixed solvent of benzene / ethyl acetate in a volume ratio of 3:4), and the eluent was removed by rotary evaporation to obtain an auxiliary agent.
[0046] Example 3
[0047] Preparation aids:
[0048] S1. In a three-necked flask equipped with a stirring device, 17.2 g of vinyl acetic acid, 25.4 g of 4-amino-3-fluorophenol, 41.2 g of dicyclohexylcarbodiimide and 150 mL of toluene were mixed and stirred evenly, and reacted in a water bath at 50° C. for 3 h. After the reaction was completed, the mixture was filtered and the solvent was removed by distillation under reduced pressure to obtain intermediate 1;
[0049] S2. In a three-necked flask equipped with a stirring device, 31.4 g of 2,2,6,6-tetramethylpiperidinol, 100 mL of n-octane, and 0.8 g of molybdenum trioxide were mixed and stirred evenly, heated to 80°C, and 30 mL of tert-butyl hydroperoxide aqueous solution (mass fraction 18%) was added dropwise. After the addition was completed, the reaction was refluxed for 9 h. After the reaction was completed, the mixture was filtered, activated carbon was added to the filtrate, and stirred for 1 h. The mixture was allowed to stand, filtered, and the filtrate was taken. The n-octane was removed by distillation under reduced pressure to obtain intermediate 2.
[0050] S3, in a three-necked flask equipped with a stirring device, 77.8g of intermediate 1, 57.6g of trimesoyl chloride and 300mL of toluene were mixed and stirred evenly, and then 82.4g of dicyclohexylcarbodiimide was added, and the temperature was raised to 65°C for reaction for 5h. Stirring was continued during the reaction. After the reaction was completed, the mixture was filtered, and part of the solvent was removed by rotary evaporation. The mixture was purified by column chromatography (the eluent was a mixed solvent of benzene / ethyl acetate, and the volume ratio of the two was 3:2), and the eluent was removed by rotary evaporation to obtain intermediate 3;
[0051] S4. In a three-necked flask equipped with a stirring device, 116.4 g of intermediate 3, 57.0 g of intermediate 2 and 300 mL of toluene were mixed and stirred evenly, and then 41.2 g of dicyclohexylcarbodiimide was added, and the reaction temperature was controlled to 70°C. The reaction was carried out for 6 hours. Stirring was continued during the reaction. After the reaction was completed, the mixture was filtered, evaporated under reduced pressure, and purified by column chromatography (the eluent was a mixed solvent of benzene / ethyl acetate in a volume ratio of 3:4), and the eluent was removed by rotary evaporation to obtain an auxiliary agent.
[0052] Example 4
[0053] 80g of polypropylene resin, 10g of EPDM rubber, 4g of antioxidant 264, 12g of modified nano-silicon dioxide prepared in Example 1, 5g of the auxiliary agent prepared in Example 2 and 0.1g of benzoyl peroxide were mixed and added into a twin-screw extruder for melt blending and spinning. The filaments were formed into cable filaments by cooling and blowing, cooling, curing, and winding.
[0054] Example 5
[0055] 90g of polypropylene resin, 12g of EPDM rubber, 5g of antioxidant 1010, 14g of modified nano-silica prepared in Example 1, 7.5g of the auxiliary agent prepared in Example 3 and 0.2g of lauroyl peroxide were mixed and added into a twin-screw extruder for melt blending and spinning. The filaments were formed into cable filaments by cooling and blowing, cooling, curing, and winding.
[0056] Example 6
[0057] 100g of polypropylene resin, 14g of EPDM rubber, 6g of antioxidant 1010, 16g of modified nano-silicon dioxide prepared in Example 1, 10g of the auxiliary agent prepared in Example 3 and 0.3g of lauroyl peroxide were mixed and added into a twin-screw extruder for melt blending and spinning. The filaments were formed into cable filaments by cooling and blowing, cooling, curing, and winding.
[0058] Comparative Example 1
[0059] No auxiliary agent was added, and the remaining steps were the same as in Example 6.
[0060] Comparative Example 2
[0061] Commercially available LyondellBasell aging-resistant high-strength polypropylene (PP-851) was used for melt blending and spinning, and the filaments were formed into filaments through cooling and blowing, cooling, solidification, and winding.
[0062] Examples 4-6 and comparative examples 1-2 were made into corresponding shapes according to different test standards and subjected to the following performance tests:
[0063] The wear resistance is measured using the national standard GB / T 3960 "Test methods for sliding friction and wear of plastics";
[0064] The national standard GB / T 16422.2 "Plastics Laboratory Light Source Exposure Test Method Part 2: Xenon Arc Lamp" was used to test the tensile strength of the samples before and after aging (GB / T 1040-2006);
[0065] The sample was completely immersed in water, taken out after 2 days, and the tensile strength before and after immersion was measured using the national standard GB / T 1040-2006 "Determination of tensile properties of plastics";
[0066] The measured results are shown in the following table:
[0067]
[0068] It can be seen from the above table that the test samples prepared in the embodiments of the present invention have better aging resistance, water resistance and tensile strength than the control examples, and have good wear resistance; therefore, the prepared cables have important application value in the field of ship cable technology.
[0069] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0070] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A process for manufacturing a marine cable, characterized in that: The following steps are involved: The polypropylene resin, EPDM rubber, antioxidant, modified nano-silica, additives and initiator are mixed and added into a twin-screw extruder for melt blending and spinning. The filaments are cooled and blown, cooled, solidified, and rolled to form cable filaments. The marine cables are woven according to the requirements. The auxiliary agent is prepared by the following steps: S1, vinyl acetic acid, 4-amino-3-fluorophenol, dicyclohexylcarbodiimide and toluene were mixed and stirred evenly, and reacted at 50° C. for 3 h. After the reaction was completed, the mixture was filtered and distilled under reduced pressure to obtain intermediate 1; S2, 2,2,6,6-tetramethylpiperidinol, n-octane and molybdenum trioxide were mixed and stirred evenly, heated to 80°C, and tert-butyl hydroperoxide aqueous solution was added dropwise. After the addition was completed, the mixture was refluxed for 9 hours. After the reaction was completed, the mixture was filtered, and activated carbon was added to the filtrate, stirred for 1 hour, allowed to stand, filtered, and the filtrate was taken and distilled under reduced pressure to obtain intermediate 2; S3, mixing intermediate 1, trimesoyl chloride and toluene, adding dicyclohexylcarbodiimide, reacting at 65°C for 5 hours, stirring continuously during the reaction, filtering, rotary evaporating, column chromatography purification, and rotary evaporating to obtain intermediate 3; S4. Mix and stir the intermediate 3, intermediate 2 and toluene evenly, then add dicyclohexylcarbodiimide, react at 70°C for 6 hours, stir continuously during the reaction, filter, distill under reduced pressure, purify by column chromatography, and rotary evaporate to obtain an auxiliary agent.
2. A process for manufacturing a ship cable according to claim 1, characterized in that: In step S1, the ratio of vinylacetic acid, 4-amino-3-fluorophenol, dicyclohexylcarbodiimide and toluene is 8.6 g:12.7 g:20.6 g:75 mL.
3. A process for manufacturing a ship cable according to claim 1, characterized in that: In step S2, the ratio of the amount of 2,2,6,6-tetramethylpiperidinol, n-octane, molybdenum trioxide, and tert-butyl hydroperoxide aqueous solution is 15.7 g:50 mL:0.4 g:15 mL.
4. A process for manufacturing a ship cable according to claim 1, characterized in that: In step S3, the ratio of the amount of intermediate 1, trimesoyl chloride, toluene, and dicyclohexylcarbodiimide is 38.9 g: 28.8 g: 150 mL: 41.2 g.
5. A process for manufacturing a ship cable according to claim 1, characterized in that: In step S4, the ratio of the amount of intermediate 1, intermediate 2, toluene and dicyclohexylcarbodiimide used is 58.2 g: 28.5 g: 150 mL: 20.6 g.
6. A process for manufacturing a ship cable according to claim 1, characterized in that: The raw materials are calculated in parts by weight as follows: 80-100 parts of polypropylene resin, 10-14 parts of ethylene propylene rubber, 4-6 parts of antioxidant, 12-16 parts of modified nano silicon dioxide, 5-10 parts of auxiliary agent, and 0.1-0.3 parts of initiator.
7. A process for manufacturing a ship cable according to claim 1, characterized in that: The initiator is one of benzoyl peroxide and lauroyl peroxide.
8. The manufacturing process of a ship cable according to claim 1, characterized in that: The antioxidant is one of antioxidant 1010 and antioxidant 264.
Citation Information
Cited By
Anti-aging piezoelectric cable
CN119207878A
Polyester FDY (fully drawn yarn) oiling agent with high-concentration emulsion