Paper surface sizing agent and preparation method thereof

By using multifunctional polymer copolymers and modified materials in paper surface sizing agents to form a multi-dimensional hydrophobic network structure, the problem of insufficient water resistance and strength of paper in the existing technology is solved, and a low-dosage, efficient paper surface is achieved. Treatment, suitable for paper such as corrugated paper, improves water resistance and smoothness.

CN118727508AActive Publication Date: 2024-10-01JIUZHOU BIO-TECH (SUZHOU) CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410746673.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-11
Publication Date
2024-10-01
Estimated Expiration
2044-06-11

AI Technical Summary

Technical Problem

Existing paper surface sizing agents are not comprehensive enough in improving the water resistance and strength of paper, and the dosage is large and the cost is high. Moreover, the development of corrugated paper and board paper in the market is faced with reduced weight, poor pulp quality, and internal sizing of paper. Problems such as unstable quality.

Method used

Multifunctional polymer copolymer is used, and hydrophobic monomers, cationic monomers and modified monomers are grafted and copolymerized with styrene, butyl acrylate, hydroxyethyl acrylate and other monomers in combination with cationic starch to form a multi-dimensional Hydrophobic network structure, modified wollastonite and bentonite, and polyamide polyurea resin are used to prepare a low-dosage but highly efficient paper surface sizing agent.

Benefits of technology

It achieves the formation of a multi-dimensional hydrophobic network structure on the paper surface, significantly reduces the Cobb value, improves the water resistance and strength of the paper, has low cost, and has a more comprehensive effect. It is suitable for corrugated paper and other papers, and improves the water resistance and smoothness of the finished paper.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004886636430000151
    Figure BDA0004886636430000151
  • Figure BDA0004886636430000161
    Figure BDA0004886636430000161
Patent Text Reader

Abstract

The invention discloses a paper surface sizing agent which comprises a cationic monomer, a hydrophobic monomer, a modified monomer, cationic starch, styrene, butyl acrylate and hydroxyethyl acrylate. According to the paper surface sizing agent disclosed by the invention, various functional monomers including a hydrophobic monomer, a cationic monomer and a modified monomer are introduced and are combined with monomers such as styrene, butyl acrylate and hydroxyethyl acrylate to carry out graft copolymerization modification on cationic starch, so that a multifunctional high-molecular copolymer is obtained, and the relative cost is low; after film forming, the cross-linking agent can be effectively combined on the paper fiber surface in a cross-linking manner, and a multi-dimensional spatial hydrophobic network structure is formed on the paper surface, so that the dual effects of effectively reducing the Cobb value of the paper and improving the paper strength are achieved, and the effects of effectively improving the water resistance of the paper and the paper surface strength are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a paper surface treatment agent, in particular to a paper surface sizing agent and a preparation method thereof. Background Art

[0002] In the modern papermaking industry, with the development of paper coating technology, we have put forward higher requirements for coating pigment additives. The coating not only protects the value of the coated object, but also plays a good decorative role due to its rich colors. Nowadays, with the continuous improvement of people's environmental awareness, the development of water-based coatings has been strongly advocated, and the solid components in the coating, such as pigments and fillers, occupy an important part.

[0003] The main components of conventional paper and paperboard are plant fibers, and such fibers have good hygroscopicity. Since the narrow gaps between the fibers in wet paper act as capillary attraction for water, untreated paper easily absorbs moisture. Therefore, sizing has become an indispensable process in the papermaking process. By adding sizing agents and processing pulp, paper sheets or paperboard under certain process conditions, the purpose is to form a hydrophobic protective film on the surface of the paper, which plays a role in water resistance and reduces the hydrophilicity of plant fibers.

[0004] The current development direction of paper in the market, especially the development of corrugated paper and board paper, has increasingly severe problems, mainly reflected in the reduction of gram weight, deterioration of pulp quality, unstable quality of internal sizing paper, etc., so an excellent paper surface sizing agent is needed to protect and control the water resistance of finished paper, improve paper strength and have rapid maturation performance. At present, there are many types of sizing agents on the market, with large dosage, high cost, and insufficient overall effect. Summary of the invention

[0005] In order to overcome the above-mentioned shortcomings, one of the purposes of the present invention is to provide a paper surface sizing agent to improve the waterproof performance of paper or cardboard, improve the surface strength of paper, and achieve comprehensive performance of rapid maturation. The surface sizing agent is added in a small amount, the effect is obvious and more comprehensive, the cost is reduced, and it is green and environmentally friendly.

[0006] In order to achieve the above purpose, the technical solution adopted by the present invention is: a paper surface sizing agent, including cationic monomers, hydrophobic monomers, modified monomers, cationic starch, styrene, butyl acrylate and hydroxyethyl acrylate.

[0007] Further, by weight, the cationic monomer is 2-4 parts, the hydrophobic monomer is 3-6 parts, the modified monomer is 1-2 parts, the cationic starch is 40-80 parts, the styrene is 60-120 parts, the butyl acrylate is 40-80 parts and the hydroxyethyl acrylate is 6-12 parts.

[0008] Illustratively, the cationic monomer is in a range of 2 parts, 2.5 parts, 3 parts, 3.5 parts, 4 parts, or any two thereof;

[0009] The hydrophobic monomer is in the range of 3 parts, 4 parts, 5 parts, 6 parts or any two parts thereof;

[0010] The modified monomer is 1 part, 1.5 parts, 2 parts or any two of them;

[0011] Cationic starch is 40 parts, 50 parts, 60 parts, 70 parts, 80 parts or any two thereof;

[0012] Styrene 60 parts, 70 parts, 80 parts, 90 parts, 100 parts, 110 parts, 120 parts or any two thereof;

[0013] Butyl acrylate is 40 parts, 50 parts, 60 parts, 70 parts, 80 parts or any two thereof;

[0014] The content of hydroxyethyl acrylate is 6 parts, 7 parts, 8 parts, 9 parts, 10 parts, 11 parts, 12 parts or any two thereof.

[0015] Furthermore, it also includes 0.2-0.5 parts of modified wollastonite, 0.2-0.5 parts of modified bentonite, and 1.0-2.0 parts of polyamide polyurea resin.

[0016] Exemplarily, the modified wollastonite is in the range of 0.2 parts, 0.3 parts, 0.4 parts, 0.5 parts or any two of them; the modified bentonite is in the range of 0.2 parts, 0.3 parts, 0.4 parts, 0.5 parts or any two of them; the polyamide polyurea resin is in the range of 1.0 parts, 1.1 parts, 1.2 parts, 1.3 parts, 1.4 parts, 1.5 parts, 1.7 parts, 1.8 parts, 1.9 parts, 2.0 parts or any two of them.

[0017] Furthermore, the modified wollastonite is a 600-mesh fibrous papermaking grade wollastonite modified by using a silane coupling agent KH-550 and dodecylamine, and the Mohs hardness of the wollastonite is in the range of 5.0-5.5;

[0018] The modified bentonite is bentonite modified by sulfuric acid acidification method;

[0019] The content of the polyamide polyurea resin is 50%.

[0020] Further, the weight ratio of the hydrophobic monomer to the modified monomer is 1.0-3.0: 1. Exemplarily, the weight ratio of the hydrophobic monomer to the modified monomer is 1.0: 1, 1.5: 1, 2.0: 1, 2.5: 1, 3.0: 1.

[0021] Furthermore, the cationic monomer is selected from one or two of dimethyldiallylammonium chloride and dimethylaminopropylmethacrylamide;

[0022] The hydrophobic monomer is selected from one or more of benzyl acrylate, benzyl methacrylate, and 2-benzyl methyl acrylate;

[0023] The modified monomer is selected from one or more of divinyltetramethyldisiloxane, tetramethyltetravinylcyclotetrasiloxane, and hexamethylhexavinylcyclohexasiloxane;

[0024] The cationic starch is cationic cassava modified starch, and its content is 88% by weight.

[0025] Furthermore, it also includes 0.05-0.10 parts of α-amylase, 3-5 parts of cationic emulsifier and 6-10 parts of glacial acetic acid; illustratively, α-amylase is in the range of 0.05 parts, 0.06 parts, 0.07 parts, 0.08 parts, 0.09 parts, 0.10 parts or any two of them; cationic emulsifier is in the range of 3 parts, 3.5 parts, 4 parts, 4.5 parts, 5 parts or any two of them, and glacial acetic acid is in the range of 6 parts, 7 parts, 8 parts, 9 parts, 10 parts or any two of them;.

[0026] The α-amylase is a liquid medium-temperature α-amylase with an enzyme activity of 4000 U / g;

[0027] The cationic emulsifier is one or both of dodecyldimethylbenzyl ammonium chloride and benzyltrimethylammonium chloride.

[0028] Furthermore, it also includes an initiator and a reducing agent, wherein the initiator includes one or more of ammonium persulfate, potassium persulfate, and sodium persulfate; and the reducing agent includes one or more of sodium bisulfite, potassium bisulfite, and ammonium bisulfite.

[0029] Another object of the present invention is to provide a method for preparing a paper surface sizing agent, comprising the following steps:

[0030] S1, preparing pre-emulsion A: adding 50-100 parts of water and 3-5 parts of cationic emulsifier to an emulsifying kettle, stirring evenly, then sequentially adding 60-120 parts of styrene, 40-80 parts of butyl acrylate, 6-12 parts of hydroxyethyl acrylate, 3-6 parts of hydrophobic monomer, 2-4 parts of cationic monomer, 1-2 parts of modified monomer, stirring evenly, stirring at a speed of 300-400 r / min, stirring time of 20-30 min, to prepare pre-emulsion A;

[0031] S2, preparing initiator solution B: dissolving 3-6 parts of initiator in 45-90 parts of water to prepare initiator solution B;

[0032] S3, preparing reducing agent solution C: dissolving 0.5-1 part of reducing agent in 10-20 parts of water to prepare reducing agent solution C;

[0033] S4, add 230-460 parts of water, 40-80 parts of cationic starch, and 0.05-0.10 parts of α-amylase to the reactor, stir evenly and heat, further heat to 70-80°C, and stir and react for 20-40 minutes; after the reaction is completed, add 6-10 parts of glacial acetic acid to the reactor to terminate the enzymatic reaction, and keep the reaction for 5-10 minutes;

[0034] S5, adding part of the pre-emulsion A, the added pre-emulsion A accounts for 10% of the mass of the pre-emulsion A prepared in S1, and then adding part of the initiator solution B for water-soluble polymerization reaction, the added initiator solution B accounts for 20% of the mass of the initiator solution B prepared in S2, and the reaction time is 20-30min;

[0035] The remaining pre-emulsion A and the remaining initiator solution B are added dropwise for emulsion polymerization reaction at a reaction temperature of 75-83°C. The remaining pre-emulsion A is added dropwise for 90-120 minutes, and the remaining initiator solution B is added dropwise for 100-130 minutes. After the reaction is completed, the reaction is kept warm for about 60-90 minutes.

[0036] S6, after the heat preservation is finished, the temperature is lowered to 70-75°C, and the reducing agent solution C is added dropwise, and the dripping is completed within 20-30 minutes, and the heat preservation reaction is carried out for 20-30 minutes;

[0037] S8, cooling to below 40°C, adding 0.2-0.5 parts of modified wollastonite and 0.2-0.5 parts of modified bentonite respectively, stirring for 30-40 minutes, then adding 1.0-2.0 parts of polyamide polyurea resin (PAPU) and further stirring for 30-40 minutes, adding appropriate amount of water to adjust the solid content of the product to 29%-31%, and obtaining the final product.

[0038] The beneficial effects of the present invention are:

[0039] 1) The paper surface sizing agent of the present invention introduces a variety of functional monomers, including hydrophobic monomers, cationic monomers and modified monomers, and combines styrene, butyl acrylate, hydroxyethyl acrylate and other monomers to carry out graft copolymerization modification on cationic starch to obtain a multifunctional high molecular copolymer with relatively low cost; after film formation, it can be effectively cross-linked and bonded to the surface of paper fibers, and form a multi-dimensional spatial hydrophobic network structure on the surface of paper, achieving the dual effects of effectively reducing the Cobb value of paper and improving the strength of paper, thereby effectively improving the water resistance of paper and the surface strength of paper.

[0040] 2) By controlling the mass ratio of the hydrophobic monomer benzyl methacrylate and the modified monomer tetramethyltetravinylcyclotetrasiloxane to 1.0-3.0:1 and combining a certain amount of cationic monomers, the cationic sizing agent polymer main chain structure is provided with a larger number of hydrophobic cationic grouped side chains, so that the sizing agent can achieve good water and moisture resistance and improve paper strength when used in small amounts when combined with paper fibers.

[0041] 3) Introduce modified monomers containing siloxane groups (one or more of divinyltetramethyldisiloxane, tetramethyltetravinylcyclotetrasiloxane, and hexamethylhexavinylcyclohexasiloxane), utilize the cross-linking hydrophobic effect of the silicone monomer, and combine with the hydrophobic ester group and hydroxyl group contained in the original high molecular polymer to form a strong water-resistant effect containing multiple hydrophobic groups superimposed on each other, thereby further improving the overall water resistance of the paper.

[0042] 4) The introduction of 600 mesh fibrous papermaking grade wollastonite modified by silane coupling agent KH-550 and dodecylamine and bentonite modified by sulfuric acid acidification can make the polymer of the surface glue firmly adsorbed on the surface of paper, and form a high-hardness multi-dimensional network protective film structure on the surface of paper, thereby comprehensively improving the water resistance and hardness of the original paper protective film, thereby significantly improving the film-forming water resistance and film strength of the surface glue, and making the surface glue after joint microscopic modification have better water resistance and harder strength.

[0043] 5) When the surface sizing agent of the present invention is added to the application evaluation system containing starch, a more effective cross-linking and bonding effect can be achieved between the surface sizing agent, the starch system and the paper fibers. In addition, the original surface sizing agent can be rapidly film-formed and matured in combination with the polyamide polyurea resin (PAPU) contained in the surface sizing agent, and more firmly adsorbed on the surface of the paper, thereby further improving the water resistance and overall stability of the paper.

[0044] 6) The surface glue performance comparison experiment shows that the paper surface glue of the present invention has a good water-resistant effect; and compared with the application evaluation of the current commercially available surface glue with a uniform addition amount, it is found that the surface glue of the present invention has a smaller amount, better effect, and low cost. After the paper surface glue of the present invention is used for paper such as cardboard and Valencia paper, the resulting finished paper has excellent water resistance and good paper strength, and improves the smoothness and glossiness of the finished paper. DETAILED DESCRIPTION

[0045] In order to make the above-mentioned purpose, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below. In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed below.

[0046] Except as shown in the operating examples or otherwise indicated, all numbers used in the specification and claims to indicate the amount of ingredients, physicochemical properties, etc. are understood to be adjusted by the term "about" in all cases. Therefore, unless otherwise indicated, the numerical parameters listed in the above specification and the attached claims are approximate values, and those skilled in the art can use the teachings disclosed herein to seek to obtain the desired properties and appropriately change these approximate values. The use of numerical ranges expressed as endpoints includes all numbers within the range and any range within the range, for example, 1 to 5 includes 1, 1.1, 1.3, 1.5, 2, 2.75, 3, 3.80, 4 and 5, etc.

[0047] The applicant found that the current development direction of paper in the market, especially the development of corrugated paper and board paper, has increasingly severe problems, mainly reflected in the reduction of gram weight, deterioration of pulp quality, unstable quality of internally sized paper, etc., so an excellent paper surface sizing agent is needed to protect and control the water resistance of finished paper, improve paper strength and have rapid maturation performance. At present, there are many types of sizing agents on the market, with large dosage, high cost, and insufficient overall effect.

[0048] In view of the above technical problems, the present invention provides a paper surface sizing agent. The paper surface sizing agent is obtained by introducing a plurality of functional monomers in a specific ratio for emulsion polymerization reaction to obtain a multifunctional high molecular copolymer. The surface sizing agent polymer contains a large number of hydrophobic ester groups, hydrocarbon groups, siloxane groups and other groups. After film formation, it can be effectively cross-linked and bonded to the surface of paper fibers, and form a multi-dimensional spatial hydrophobic network structure on the surface of paper, so as to achieve the dual effects of effectively reducing the Cobb value of paper and improving the surface strength of paper; a small amount of modified wollastonite and modified bentonite are combined to make the surface sizing agent high molecular polymer more firmly and evenly adsorbed on the surface of paper, thereby comprehensively improving the water resistance and hardness of the original paper protective film; on the other hand, an appropriate amount of polyamide polyurea resin (PAPU) is added to coordinate and optimize the sizing agent polymer, so that the surface sizing agent matures more quickly on the paper surface, further improving the cross-linking and bonding performance with the paper fibers, and improving the overall water resistance and strength of the paper.

[0049] The specific preparation steps of paper surface sizing agent are as follows:

[0050] S1. Preparing pre-emulsion A: adding 50-100 parts of water and 3-5 parts of cationic emulsifier into an emulsifying kettle, stirring evenly, then sequentially adding 60-120 parts of styrene, 40-80 parts of butyl acrylate, 6-12 parts of hydroxyethyl acrylate, 3-6 parts of hydrophobic monomer, 2-4 parts of cationic monomer, 1-2 parts of modified monomer, stirring evenly, stirring at a speed of 300-400 r / min, stirring for 20-30 min, to prepare pre-emulsion A.

[0051] The cationic emulsifier is selected from one or both of dodecyldimethylbenzyl ammonium chloride and benzyltrimethylammonium chloride.

[0052] The hydrophobic monomer is selected from one or more of benzyl acrylate, benzyl methacrylate, and 2-benzyl methyl acrylate;

[0053] The cationic monomer is selected from one or two of dimethyldiallylammonium chloride and dimethylaminopropyl methacrylamide;

[0054] The modified monomer is selected from one or more of divinyltetramethyldisiloxane, tetramethyltetravinylcyclotetrasiloxane, and hexamethylhexavinylcyclohexasiloxane.

[0055] S2. Prepare initiator solution B: dissolve 3-6 parts of initiator in 45-90 parts of water to prepare initiator solution B; the initiator is selected from one or more of ammonium persulfate, potassium persulfate, and sodium persulfate.

[0056] S3. Prepare reducing agent solution C: dissolve 0.5-1 part of reducing agent in 10-20 parts of water to prepare reducing agent solution C; the reducing agent is selected from one or more of sodium bisulfite, potassium bisulfite, and ammonium bisulfite.

[0057] S4, add 230-460 parts of water, 40-80 parts of cationic starch, and 0.05-0.10 parts of α-amylase to the reactor, stir evenly and heat, further heat to 70-80°C, and stir and react for 20-40 minutes; after the reaction is completed, add 6-10 parts of glacial acetic acid to the reactor to terminate the enzymatic reaction, and keep the reaction for 5-10 minutes;

[0058] The cationic starch is cationic cassava modified starch, and its content is 88% by weight. The α-amylase is liquid medium-temperature α-amylase, and its enzyme activity is 4000 U / g.

[0059] S5, adding part of the pre-emulsion A, the added pre-emulsion A accounts for 10% of the total pre-emulsion A prepared in S1, and then adding part of the initiator solution B for water-soluble polymerization reaction 1 minute later, the added initiator solution B accounts for 20% of the initiator solution B prepared in S2, and the reaction time is 20-30 minutes;

[0060] The remaining pre-emulsion A and the remaining initiator solution B are added dropwise for emulsion polymerization reaction at a reaction temperature of 75-83°C. The remaining pre-emulsion A is added dropwise for 90-120 minutes, and the remaining initiator solution B is added dropwise for 100-130 minutes. After the reaction is completed, the reaction is kept warm for about 60-90 minutes.

[0061] S6, after the heat preservation is finished, the temperature is lowered to 70-75°C, and the reducing agent solution C is added dropwise, and the dripping is completed within 20-30 minutes, and the heat preservation reaction is carried out for 20-30 minutes;

[0062] S7, cooling to below 40°C, adding 0.2-0.5 parts of modified wollastonite and 0.2-0.5 parts of modified bentonite respectively, stirring for 30-40 minutes, then adding 1.0-2.0 parts of polyamide polyurea resin (PAPU) and stirring for further 30-40 minutes, adding an appropriate amount of water to adjust the solid content of the product, and obtaining the final product, wherein the solid content of the paper surface sizing agent is 29%-31%. The polyamide polyurea resin (PAPU) was purchased from Wuxi Tianxin Chemical Co., Ltd., model LWR-02 (PAPU)

[0063] Example

[0064] The following examples describe the disclosure of the present invention in more detail, and these examples are intended for illustrative purposes only, as various modifications and variations within the scope of the disclosure of the present invention will be apparent to those skilled in the art. Unless otherwise stated, all parts, percentages, and ratios reported in the following examples are by weight, and all reagents used in the examples are commercially available or synthesized according to conventional methods and can be used directly without further processing, and the instruments used in the examples are commercially available.

[0065] Example 1

[0066] S1. Add 50 g of water and 3 g of cationic emulsifier dodecyl dimethyl benzyl ammonium chloride to a pre-emulsifier, and add 60 g of styrene, 40 g of butyl acrylate, 6 g of hydroxyethyl acrylate, 3 g of benzyl methacrylate, 2 g of dimethyl diallyl ammonium chloride and 1 g of tetramethyl tetravinyl cyclotetrasiloxane in sequence under stirring at a stirring rate of 400 r / min for 30 min to prepare a pre-emulsion A;

[0067] S2. Add 3 g of ammonium persulfate into 45 g of water to dissolve to prepare initiator solution B;

[0068] S3, adding 0.5 g of sodium bisulfite to 10 g of water to dissolve, to prepare reducing agent solution C;

[0069] S4, add 230g water, 40g cationic starch, 0.05g a-amylase to the reaction vessel, stir evenly and heat, further heat to 70°C, keep warm and stir for 20min; after the insulation reaction is completed, add 6g glacial acetic acid to the reactor to terminate the enzymatic hydrolysis reaction, and keep warm for 10min;

[0070] S5, add 16.5g pre-emulsion A, and then add 9.6g initiator solution B to carry out water-soluble polymerization reaction, the reaction time is 20min; the remaining pre-emulsion A and the remaining initiator solution B are added dropwise to the reaction to carry out polymerization reaction, the reaction temperature is 75°C, the remaining pre-emulsion A is added dropwise for 90min, and the remaining initiator solution B is added dropwise for 100min. After the reaction is completed, keep the reaction warm for about 90min;

[0071] S6, after the heat preservation is finished, the temperature is lowered to 70°C, and the reducing agent solution C is added dropwise, and the dripping is completed in about 30 minutes, and the heat preservation reaction is carried out for 20 minutes;

[0072] S7. Cool down to below 40°C, add 0.2g of modified wollastonite and 0.2g of modified bentonite respectively, stir for 30-40min, then add 1.0g of polyamide polyurea resin LWR-02 (PAPU) and stir for further 30min, add appropriate amount of water to adjust the product to a solid content of 30.3%, and obtain a paper surface sizing agent.

[0073] Example 2

[0074] S1. Add 50 g of water and 3 g of cationic emulsifier dodecyldimethylbenzyl ammonium chloride to a pre-emulsifier, and add 60 g of styrene, 40 g of butyl acrylate, 6 g of hydroxyethyl acrylate, 2 g of benzyl methacrylate, 1 g of 2-benzyl methyl acrylate, 2 g of dimethyldiallylammonium chloride and 1 g of tetramethyltetravinylcyclotetrasiloxane in sequence under stirring, and stir at a stirring rate of 400 r / min for 30 min to prepare pre-emulsion A;

[0075] S2. Add 3 g of ammonium persulfate into 45 g of water to dissolve to prepare initiator solution B;

[0076] S3, adding 0.5 g of sodium bisulfite to 10 g of water to dissolve, to prepare reducing agent solution C;

[0077] S4, add 230g water, 40g cationic starch, 0.05g a-amylase to the reaction vessel, stir evenly and heat, further heat to 80°C, keep stirring and react for 40min; after the insulation reaction is completed, add 6g glacial acetic acid to the reactor to terminate the enzymatic hydrolysis reaction, and keep the temperature for 10min;

[0078] S5, add 16.5g pre-emulsion A, and then add 9.6g initiator solution B to carry out water-soluble polymerization reaction, the reaction time is 20min;

[0079] The remaining pre-emulsion A and the remaining initiator solution B are added dropwise to the reaction for polymerization reaction at a temperature of 75-83°C. The remaining pre-emulsion A is added dropwise for 120 minutes, and the remaining initiator solution B is added dropwise for 100 minutes. After the reaction is completed, the reaction is kept warm for about 60 minutes.

[0080] S6, after the heat preservation is finished, the temperature is lowered to 75°C, and the reducing agent solution C is added dropwise, and the dripping is completed in about 20-30 minutes, and the heat preservation reaction is carried out for 20 minutes;

[0081] S7. Cool down to below 40°C, add 0.2g of modified wollastonite and 0.2g of modified bentonite respectively, stir for 30min, then add 1.0g of polyamide polyurea resin LWR-02 (PAPU) and stir for 40min, add appropriate amount of water to adjust the product to a solid content of 30.2%, and obtain a paper surface sizing agent.

[0082] Example 3

[0083] S1. Add 50 g of water and 3 g of cationic emulsifier dodecyl dimethyl benzyl ammonium chloride to a pre-emulsifier, and add 60 g of styrene, 40 g of butyl acrylate, 6 g of hydroxyethyl acrylate, 3 g of benzyl methacrylate, 2 g of dimethyl diallyl ammonium chloride and 1 g of tetramethyl tetravinyl cyclotetrasiloxane in sequence under stirring at a stirring rate of 400 r / min for 30 min to prepare a pre-emulsion A;

[0084] S2. Add 3 g of ammonium persulfate into 45 g of water to dissolve to prepare initiator solution B;

[0085] S3, adding 0.5 g of sodium bisulfite to 10 g of water to dissolve, to prepare reducing agent solution C;

[0086] S4, add 230g water, 40g cationic starch, 0.05g a-amylase to the reaction vessel, stir evenly and heat, further heat to 80°C, keep stirring and react for 30min; after the insulation reaction is completed, add 6g glacial acetic acid to the reactor to terminate the enzymatic reaction, and keep the reaction for 5min;

[0087] S5, add 16.5g pre-emulsion A, then add 9.6g initiator solution B to carry out water-soluble polymerization reaction, the reaction time is 20-30min; add the remaining pre-emulsion A and the remaining initiator solution B to the reaction in a dropwise manner to carry out polymerization reaction, the reaction temperature is 80°C, the remaining pre-emulsion A is added dropwise for 100min, and the remaining initiator solution B is added dropwise for 120min. After the reaction is completed, keep the reaction warm for about 80min;

[0088] S6, after the heat preservation is finished, the temperature is lowered to 70°C, and the reducing agent solution C is added dropwise, and the dripping is completed in about 30 minutes, and the heat preservation reaction is carried out for 20 minutes;

[0089] S7. Cool down to below 40°C, add 0.5g of modified wollastonite and 0.5g of modified bentonite respectively, stir for 30-40min, then add 1.0g of polyamide polyurea resin LWR-02 (PAPU) and stir for further 35min, add appropriate amount of water to adjust the product to a solid content of 30.5%, and obtain a paper surface sizing agent.

[0090] Example 4

[0091] S1, add 50g water, 1.5g cationic emulsifier dodecyldimethylbenzyl ammonium chloride and 1.5g cationic emulsifier benzyltrimethylammonium chloride into a pre-emulsifier, add 60g styrene, 40g butyl acrylate, 6g hydroxyethyl acrylate, 1.5g benzyl methacrylate, 1.5g 2-benzyl methyl acrylate, 2g dimethyldiallylammonium chloride, 0.5g tetramethyltetravinylcyclotetrasiloxane, 0.5g divinyltetramethyldisiloxane in sequence under stirring condition, stir at 400r / min stirring speed for 30min, prepare pre-emulsion A;

[0092] S2. Add 3 g of ammonium persulfate into 45 g of water to dissolve to prepare initiator solution B;

[0093] S3, adding 0.5 g of sodium bisulfite to 10 g of water to dissolve, to prepare reducing agent solution C;

[0094] S4, add 230g water, 40g cationic starch, 0.05g a-amylase to the reaction vessel, stir evenly and heat, further heat to 80°C, keep stirring and react for 20min; after the insulation reaction is completed, add 6g glacial acetic acid to the reactor to terminate the enzymatic reaction, and keep the reaction for 5min;

[0095] S5, add 16.5g pre-emulsion A, and then add 9.6g initiator solution B to carry out water-soluble polymerization reaction, the reaction time is 20min;

[0096] The remaining pre-emulsion A and the remaining initiator solution B are added dropwise to the reaction for polymerization reaction at a reaction temperature of 83°C. The remaining pre-emulsion A is added dropwise for 120 minutes, and the remaining initiator solution B is added dropwise for 100 minutes. After the reaction is completed, the reaction is kept warm for about 90 minutes.

[0097] S6, after the heat preservation is finished, the temperature is lowered to 75°C, and the reducing agent solution C is added dropwise, and the dripping is completed in about 30 minutes, and the heat preservation reaction is carried out for 20 minutes;

[0098] S7. Cool down to below 40°C, add 0.2g of modified wollastonite and 0.2g of modified bentonite respectively, stir for 30-40min, then add 2.0g of polyamide polyurea resin LWR-02 (PAPU) and stir for further 30min, add appropriate amount of water to adjust the product to a solid content of 30.7%, and obtain a paper surface sizing agent.

[0099] Example 5

[0100] S1, add 50g water, 1.5g cationic emulsifier dodecyldimethylbenzyl ammonium chloride and 1.5g cationic emulsifier benzyltrimethylammonium chloride to a pre-emulsifier, add 60g styrene, 40g butyl acrylate, 6g hydroxyethyl acrylate, 1.5g benzyl methacrylate, 1.5g benzyl acrylate, 2g dimethyldiallylammonium chloride, 0.5g tetramethyltetravinylcyclotetrasiloxane, 0.5g divinyltetramethyldisiloxane in sequence under stirring condition, stir at a stirring rate of 400r / min for 30min, and prepare pre-emulsion A;

[0101] S2. Add 3 g of ammonium persulfate into 45 g of water to dissolve to prepare initiator solution B;

[0102] S3, adding 0.5 g of sodium bisulfite to 10 g of water to dissolve, to prepare reducing agent solution C;

[0103] S4, add 230g water, 40g cationic starch, 0.05g a-amylase to the reaction vessel, stir evenly and heat, further raise the temperature to 70-80°C, keep stirring and react for 20min; after the insulation reaction is completed, add 6g glacial acetic acid to the reactor to terminate the enzymatic hydrolysis reaction, and keep the temperature for 5min;

[0104] S5, add 16.5g pre-emulsion A, and then add 9.6g initiator solution B to carry out water-soluble polymerization reaction, the reaction time is 20min; the remaining pre-emulsion A and the remaining initiator solution B are added dropwise to the reaction to carry out polymerization reaction, the reaction temperature is 75°C, the remaining pre-emulsion A is added dropwise for 90min, and the remaining initiator solution B is added dropwise for 130min. After the reaction is completed, keep the reaction warm for about 60min;

[0105] S6, after the heat preservation is finished, the temperature is lowered to 75°C, and the reducing agent solution C is added dropwise, and the dripping is completed in about 20 minutes, and the heat preservation reaction is carried out for 30 minutes;

[0106] S7. Cool down to below 40°C, add 0.5g of modified wollastonite and 0.5g of modified bentonite respectively, stir for 40min, then add 1.0g of polyamide polyurea resin LWR-02 (PAPU) and stir for 30min, add appropriate amount of water to adjust the product to a solid content of 30.6%, and obtain a paper surface sizing agent.

[0107] Example 6

[0108] S1. Add 50 g of water and 3 g of cationic emulsifier dodecyldimethylbenzyl ammonium chloride into a pre-emulsifier, and add 60 g of styrene, 40 g of butyl acrylate, 6 g of hydroxyethyl acrylate, 1 g of benzyl methacrylate, 1 g of benzyl acrylate, 1 g of 2-benzyl methyl acrylate, 2 g of dimethyldiallylammonium chloride, 0.5 g of tetramethyltetravinylcyclotetrasiloxane and 0.5 g of hexamethylhexavinylcyclohexasiloxane in sequence under stirring at a stirring rate of 400 r / min for 30 min to prepare pre-emulsion A;

[0109] S2. Add 3 g of ammonium persulfate into 45 g of water to dissolve to prepare initiator solution B;

[0110] S3, adding 0.5 g of sodium bisulfite to 10 g of water to dissolve, to prepare reducing agent solution C;

[0111] S4, add 230g water, 40g cationic starch, 0.05g a-amylase to the reaction vessel, stir evenly and heat, further heat to 70°C, keep stirring and react for 20min; after the insulation reaction is completed, add 6g glacial acetic acid to the reactor to terminate the enzymatic hydrolysis reaction, and keep the temperature for 5min;

[0112] S5, add 16.5g pre-emulsion A, then add 9.6g initiator solution B to carry out water-soluble polymerization reaction, the reaction time is 30min; add the remaining pre-emulsion A and the remaining initiator solution B to the reaction in a dropwise manner to carry out polymerization reaction, the reaction temperature is 75°C, the remaining pre-emulsion A is added dropwise for 120min, the remaining initiator solution B is added dropwise for 100min, after the reaction is completed, keep the reaction warm for about 90min;

[0113] S6, after the heat preservation is finished, the temperature is lowered to 70°C, and the reducing agent solution C is added dropwise, and the dripping is completed in about 30 minutes, and the heat preservation reaction is carried out for 20 minutes;

[0114] S7. Cool down to below 40°C, add 0.2g of modified wollastonite and 0.2g of modified bentonite respectively, stir for 30min, then add 1.0g of polyamide polyurea resin LWR-02 (PAPU) and stir for 40min, add appropriate amount of water to adjust the product to a solid content of 30.3%, and obtain a paper surface sizing agent.

[0115] Experimental Examples

[0116] Preparation of the evaluation formula for the application of paper surface sizing agent: add 85g of starch to 415g of water, and add 0.1g of amylase, put them into a beaker and stir, heat to 98°C in a water bath, stir and keep warm for 30 minutes, cool down to obtain cooked starch, take 100g of cooked starch, add 0.5g of paper surface sizing agent, stir for 20 minutes, apply with No. 2 coating rod, and evenly apply it on the un-sizing corrugated core paper at a speed of 15m / min, dry in an oven at 90°C for 40 seconds, and start testing.

[0117] By using the above method, the paper surface sizing agents in Examples 1-6 of the present invention and commercially available paper surface sizing agents were compared. Table 1 shows the evaluation application data of the paper surface sizing agents. The Cobb value was detected by the Cobb method according to the GB / T540-1989 method. The surface strength was measured by using the J-IGT350 IGT printing adaptor. The smaller the Cobb value, the better, and the greater the surface strength, the better.

[0118] Table 1: Evaluation and application data of paper surface sizing agents

[0119]

[0120]

[0121] From the data measured in Table 1, it can be concluded that adding 0.50g of the paper surface glue of the present invention to 100g of cooked starch in a uniform absolute dry addition will have a good water-resistant effect and excellent surface strength; and compared with the application evaluation of the uniform addition amount of the current commercially available surface glue, it is found that the surface glue of the present invention has a smaller dosage, good effect, and better water-resistant performance than the blank. And it is significantly better than the general commercially available surface glue on the market. The commercially available surface glue in this embodiment is a cationic surface glue produced by Solenis Chemical Co., Ltd., with a solid content of 31.2%. In summary, the paper surface glue product of the present invention has the following advantages:

[0122] 1) The product production process is relatively simple, green and environmentally friendly, and no waste is discharged;

[0123] 2) Introduce a variety of functional monomers, including hydrophobic monomers, cationic monomers and modified monomers, and combine them with monomers such as styrene, butyl acrylate, hydroxyethyl acrylate, etc. to carry out graft copolymerization modification on cationic starch to obtain a multifunctional polymer copolymer surface sizing agent, which can be effectively cross-linked and bonded to the surface of paper fibers after film formation, and form a multi-dimensional spatial hydrophobic network structure on the surface of paper, thereby effectively improving the water resistance and strength of paper.

[0124] 3) By controlling the mass ratio of the hydrophobic monomer benzyl methacrylate and the modified monomer tetramethyltetravinylcyclotetrasiloxane to 1.0-3.0:1 and combining a certain amount of cationic monomers, the rigid main chain of the polymer is provided with a larger number of hydrophobic cationic grouped side chains, so that the surface adhesive can achieve good water and moisture resistance under low dosage conditions.

[0125] 4) Introduce modified monomers containing siloxane groups: one or more of divinyltetramethyldisiloxane, tetramethyltetravinylcyclotetrasiloxane, and hexamethylhexavinylcyclohexasiloxane. By utilizing the cross-linking hydrophobic effect of the organic silicon monomer and combining the hydrophobic ester group and hydroxyl group contained in the original high molecular polymer, a strong water-resistant performance containing multiple hydrophobic groups stacked layer by layer is formed, further improving the overall water-resistant performance of the paper.

[0126] 4) The introduction of 600 mesh fibrous papermaking grade wollastonite modified by silane coupling agent KH-550 and dodecylamine and bentonite modified by sulfuric acid acidification method can make the surface glue polymer firmly adsorbed on the surface of paper fiber, and form a high-hardness honeycomb-like dense protective film structure on the paper surface, thereby comprehensively improving the water resistance and hardness of the original paper protective film, thereby significantly improving the film-forming water resistance of the surface glue and the surface strength of the paper after film formation.

[0127] 5) When the surface sizing agent of the present invention is added to the application evaluation system containing starch, the cationic surface sizing agent, the starch system and the paper fibers can be more effectively cross-linked and bonded, so that the original surface sizing agent can form a film more uniformly. In combination with the polyamide polyurea resin (PAPU) contained in the surface sizing agent, the original surface sizing agent can be rapidly film-formed and matured, and more firmly adsorbed on the surface of the paper. In combination with the multifunctional active groups such as active hydroxyl groups and polyamino groups contained therein, the surface sizing agent can be more easily cross-linked and cured, thereby further improving the water resistance and overall stability of the paper.

[0128] The above implementation modes are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with this technology to understand the content of the present invention and implement it, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.

Claims

1. A paper surface sizing agent, characterized in that: Including cationic monomers, hydrophobic monomers, modified monomers, cationic starch, styrene, butyl acrylate and hydroxyethyl acrylate.

2. The paper surface sizing agent according to claim 1, characterized in that: By weight, 2-4 parts of cationic monomer, 3-6 parts of hydrophobic monomer, 1-2 parts of modified monomer, 40-80 parts of cationic starch, 60-120 parts of styrene, 40-80 parts of butyl acrylate and 6-12 parts of hydroxyethyl acrylate.

3. The paper surface sizing agent according to claim 1, characterized in that: The invention also comprises 0.2-0.5 parts of modified wollastonite, 0.2-0.5 parts of modified bentonite and 1.0-2.0 parts of polyamide polyurea resin.

4. The paper surface sizing agent according to claim 3, characterized in that: The modified wollastonite is 600-mesh fibrous papermaking grade wollastonite modified by silane coupling agent KH-550 and dodecylamine, and the Mohs hardness of the wollastonite is in the range of 5.0-5.5; the modified bentonite is bentonite modified by sulfuric acid acidification method.

5. The paper surface sizing agent according to claim 1, characterized in that: The weight ratio of the hydrophobic monomer to the modified monomer is 1.0-3.0:

1.

6. The paper surface sizing agent according to claim 1, characterized in that: The cationic monomer is selected from one or two of dimethyldiallylammonium chloride and dimethylaminopropyl methacrylamide; The hydrophobic monomer is selected from one or more of benzyl acrylate, benzyl methacrylate, and 2-benzyl methyl acrylate; The modified monomer is selected from one or more of divinyltetramethyldisiloxane, tetramethyltetravinylcyclotetrasiloxane, and hexamethylhexavinylcyclohexasiloxane; The cationic starch is cationic cassava modified starch.

7. The paper surface sizing agent according to claim 1, characterized in that: It also includes 0.05-0.10 parts of α-amylase, 3-5 parts of cationic emulsifier and 6-10 parts of glacial acetic acid; The α-amylase is a liquid medium-temperature α-amylase with an enzyme activity of 4000 U / g; The cationic emulsifier is selected from one or both of dodecyldimethylbenzyl ammonium chloride and benzyltrimethylammonium chloride.

8. The paper surface sizing agent according to claim 1, characterized in that: The invention also comprises an initiator and a reducing agent, wherein the initiator is selected from one or more of ammonium persulfate, potassium persulfate and sodium persulfate; and the reducing agent is selected from one or more of sodium bisulfite, potassium bisulfite and ammonium bisulfite.

9. A method for preparing a paper surface sizing agent, comprising the following steps: S1, preparing pre-emulsion A: adding water and cationic emulsifier to an emulsifying kettle, stirring evenly, then sequentially adding styrene, butyl acrylate, hydroxyethyl acrylate, hydrophobic monomer, cationic monomer, and modified monomer, stirring evenly to prepare pre-emulsion A; S2, preparing initiator solution B: dissolving the initiator in water to prepare initiator solution B; S3, preparing reducing agent solution C: dissolving the reducing agent in water to prepare reducing agent solution C; S4, add water, cationic starch, and α-amylase to the reactor, stir and heat to 70-80°C, keep warm and stir for 20-40 minutes, and after the reaction is completed, add 6-10 parts of glacial acetic acid to the reactor to terminate the enzymatic reaction, and keep warm for 5-10 minutes; S5, adding part of the pre-emulsion A, and then adding part of the initiator solution B to carry out a water-soluble polymerization reaction; adding the remaining pre-emulsion A and the remaining initiator solution B to carry out an emulsion polymerization reaction, the reaction temperature is 75-83°C, the remaining pre-emulsion A is added dropwise for 90-120min, and the remaining initiator solution B is added dropwise for 100-130min. After the reaction is completed, the reaction is kept warm for about 60-90min; S6, after the heat preservation is finished, the temperature is lowered to 70-75°C, and the reducing agent solution C is added dropwise, and the dripping is completed in about 20-30 minutes, and the heat preservation reaction is carried out for 20-30 minutes; S7. After adding modified wollastonite and modified bentonite and stirring, add polyamide polyurea resin and further stir, add appropriate amount of water to adjust the solid content of the product, and obtain the final product.

10. The method for preparing a paper surface sizing agent according to claim 9, characterized in that: The solid content of the paper surface sizing agent is 29%-31%.

Citation Information

Patent Citations

  • Cation surface sizing agent and preparation method thereof

    CN101649583A

  • Surface sizing agent as well as preparation method and application thereof

    CN102086614A

  • Preparation method of organic silicon surface sizing agent

    CN102635019A

  • Paper moisture-proof agent and preparation method thereof

    CN114395066A

  • Offset printing surface sizing liquid as well as preparation method and application thereof

    CN117758543A