Nickel-series low-temperature steel as-cast dendritic structure corrosive agent and display method
By using a corrosive agent formulated with carboxyl compounds, surfactants and ferric chloride, the safety hazards of picric acid and strong acid in the existing technology are solved, and the clear display and quality assessment of the as-cast dendrite structure of nickel-based low-temperature steel is achieved. Provides a safe and environmentally friendly corrosion method.
Patent Information
- Application Number
- CN202410909057.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-08
- Publication Date
- 2024-10-01
Smart Images

Figure CN118730679A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metallurgical detection, and relates to a nickel-based low-temperature steel cast dendrite structure corrosive agent and a display method. Background Art
[0002] The clean and efficient development of the energy and chemical industries is inseparable from the construction of ultra-low temperature storage and transportation facilities. Nickel-based low-temperature steel is the most important structural material for building such facilities and ensuring their service safety. In order to ensure safety during transportation and storage, the most stringent requirements are placed on the low-temperature toughness of nickel-based low-temperature steel. In the actual continuous casting and solidification production process, as the thickness of the solidified shell increases, the directional heat transfer direction of the heat flow changes, and there are often cross dendrites between the columnar crystals and the equiaxed crystals. This cast dendrite structure directly affects the low-temperature impact toughness of the material. Therefore, finding a method for the corrosion of cast dendrite structure of nickel-based low-temperature steel and evaluating the quality of the ingot are of great significance to improving the quality of nickel-based low-temperature steel.
[0003] At present, the dendrite corrosion method for ingot casting mainly uses picric acid or strong acids such as nitric acid and sulfuric acid as the main corrosive agent. For example, CN102023112B discloses a method for preparing an etchant that displays ultra-low carbon solidified dendrite structure, and the etchant includes picric acid, cupric chloride, hydrochloric acid, anhydrous ethanol, water, and sodium alkylbenzene sulfonate; CN112903402B discloses a cast dendrite etchant and a method of use for hot working die steel H13, and the etchant includes nitric acid, sulfuric acid, a surfactant, chloride, etc. Picric acid is explosive, flammable, and toxic, and is restricted from large-scale use, while nitric acid and sulfuric acid are highly corrosive and unsafe during use. Therefore, there is an urgent need for a safe and environmentally friendly etchant to replace picric acid or strong acid, which can clearly display the dendrite structure of nickel-based low-temperature steel ingot castings, and is used to evaluate the quality of nickel-based low-temperature steel ingot castings, so as to achieve the purpose of quality control of nickel-based low-temperature steel production processes. Summary of the invention
[0004] To achieve the above-mentioned purpose, the present invention provides a nickel-based low-temperature steel cast dendrite structure corrosive agent and display method, which solves the problems existing in the prior art.
[0005] The present invention aims to provide a nickel-based low-temperature steel cast dendrite structure etchant and display method, which does not contain explosive, flammable and toxic picric acid and can clearly display the dendrite structure of the nickel-based low-temperature steel ingot.
[0006] The technical solution of the present invention:
[0007] A nickel-based low-temperature steel cast dendrite structure corrosive agent and display method, using carboxyl compounds, surfactants, anhydrous ethanol, ferric chloride to prepare the corrosive agent, grinding and polishing the cast detection surface to make a smooth surface, using a hot corrosion method to corrode the detection test, blowing dry after corrosion, and observing the dendrite structure of the ingot using a metallographic microscope.
[0008] The process steps include:
[0009] (1) Preparation of the etchant: The etchant includes a carboxyl compound, which is low-concentration acetic acid, anhydrous ethanol, and a surfactant. The surfactant is a detergent and ferric chloride. The mass ratio of the volume of acetic acid, the volume of anhydrous ethanol, the volume of the detergent, and the mass ratio of ferric chloride is (10-15) mL: (100-110) mL: (3-5) mL: (1.5-2) g. The solution is prepared in a glass container according to the above ratio and fully stirred with a stirring tool.
[0010] (2) Preparation of sample polished surface: The nickel-based low-temperature steel ingot sample is subjected to pre-grinding, coarse grinding, fine grinding, polishing, and drying in sequence to obtain a polished surface;
[0011] (3) Corrosion of the sample: Immerse the smooth surface sample in the prepared corrosive agent and place it in a 60-70℃ water bath for corrosion. Take out the sample and rinse it in running water for 5-10 seconds. Then spray it with alcohol and dry it to obtain a metallographic sample.
[0012] (4) The prepared metallographic sample is placed under a metallographic microscope to observe the dendrites, and the secondary dendrite spacing can be measured;
[0013] The mass concentration of the acetic acid is 10% to 15%;
[0014] Preferably, the detergent is Lanfei brand worker's hand soap or White Cat brand detergent;
[0015] Preferably, the glass container is a glass cup;
[0016] Preferably, the stirring tool is a glass rod;
[0017] Preferably, the stirring time is 2 to 3 minutes, and the stirring rate is 40 to 50 r / min;
[0018] Further preferably, the grinding in step (2) comprises: firstly pre-grinding with a grinding wheel, and then grinding with 300#, 600#, 1000#, and 2000# water-abrasive sandpaper in sequence;
[0019] More preferably, the polishing in step (2) is performed using 3um diamond grinding paste;
[0020] More preferably, the etching time in step (3) is 80 to 90 seconds;
[0021] More preferably, the drying in step (3) is performed by drying with a hair dryer;
[0022] More preferably, the method for measuring the secondary dendrite spacing in step (4) is to adopt the intercept method.
[0023] The outstanding features and remarkable effects of the present invention are mainly reflected in:
[0024] (1) The present invention does not require picric acid, which is flammable, explosive and toxic, nor does it require strong acids such as nitric acid and sulfuric acid, which are highly corrosive. The acetic acid used is a safe and environmentally friendly weak acid, which is conducive to the corrosion of steel segregation at high temperatures. Ferric chloride provides chloride ions, which enhance the corrosiveness of acetic acid, quickly display dendrite structure, and improve the corrosion efficiency of the corrosive agent. The addition of detergent as a surfactant solvent can inhibit the corrosion of non-segregation areas to avoid excessive corrosion of non-segregation areas that affects the effect.
[0025] (2) The dendrites are clearly visible and the secondary dendrite spacing can be measured;
[0026] (3) The raw materials and equipment required for the present invention are simple and easy to obtain, and the operation is easy to master;
[0027] (4) The present invention has a wide application scope and is applicable to nickel-based low-temperature steel in the cast state. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0029] Figure 1 This is a diagram showing the etching effect of the dendrite etchant used in Example 1 of the present invention;
[0030] Figure 2 This is a diagram showing the etching effect of the dendrite etchant used in Example 2 of the present invention;
[0031] Figure 3 This is the etching diagram of the dendrite etchant used in Comparative Example 1 of the present invention. DETAILED DESCRIPTION
[0032] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] Embodiment 1
[0034] The steps include:
[0035] (1) 15 ml of acetic acid with a mass concentration of 10%, 100 ml of anhydrous ethanol, 3 ml of detergent, and 2 g of ferric chloride are placed in a glass cup and stirred with a glass rod for 2 min at a stirring rate of 40 r / min, and allowed to stand for 3 min to prepare an etchant;
[0036] (2) The continuous casting ingot test sample was pre-ground with a grinding wheel, and then ground with 300#, 600#, 1000#, and 2000# water-abrasive sandpaper in sequence; then polished with 3um diamond grinding paste until the test surface reached a mirror effect, and cleaned with ethanol to obtain a smooth surface; the chemical composition of the nickel-based low-temperature steel is shown in Table 1;
[0037] (3) Place the polished surface in the prepared corrosive agent in an etched manner, etch it in a 65°C water bath for 80 seconds, rinse it with running water for 5 seconds, clean it with alcohol, and then blow it dry with a hair dryer to obtain a metallographic sample;
[0038] (4) Place the metallographic sample under a metallographic microscope and magnify it 25 times to obtain Figure 1 ,Depend on Figure 1 Well-developed cross-dendritic crystals can be clearly observed, and the secondary dendrite spacing can be measured.
[0039] Embodiment 2
[0040] The steps include:
[0041] (1) 12 ml of acetic acid with a mass concentration of 13%, 105 ml of anhydrous ethanol, 2 ml of detergent, and 1.5 g of ferric chloride were placed in a glass cup and stirred with a glass rod for 2.5 min at a stirring rate of 45 r / min. The mixture was allowed to stand for 3 min to prepare an etchant;
[0042] (2) The continuous casting ingot test sample was pre-ground with a grinding wheel, and then ground with 300#, 600#, 1000#, and 2000# water-abrasive sandpaper in sequence; then polished with 3um diamond grinding paste until the test surface reached a mirror effect, and cleaned with ethanol to obtain a smooth surface; the chemical composition of the nickel-based low-temperature steel is shown in Table 1;
[0043] (3) Place the polished surface in the prepared corrosive agent in an etched manner, etch it in a 70°C water bath for 90 seconds, rinse it with running water for 8 seconds, then clean it with alcohol, and then blow dry it with a hair dryer to obtain a metallographic sample;
[0044] (4) Place the metallographic sample under a metallographic microscope and magnify it 25 times to obtain Figure 2 ,Depend on Figure 1 Well-developed cross-dendritic crystals can be clearly observed, and the secondary dendrite spacing can be measured.
[0045] Comparative Example 1
[0046] The steps include:
[0047] (1) 15 ml of acetic acid with a mass concentration of 10%, 105 ml of water, 2 ml of detergent, and 1.5 g of ferric chloride are placed in a glass cup and stirred with a glass rod for 2 min at a stirring rate of 42 r / min. The mixture is allowed to stand for 3 min to prepare an etchant;
[0048] (2) The continuous casting ingot test sample was pre-ground with a grinding wheel, and then ground with 300#, 600#, 1000#, and 2000# water-abrasive sandpaper in sequence; then polished with 3um diamond grinding paste until the test surface reached a mirror effect, and cleaned with ethanol to obtain a smooth surface; the chemical composition of the nickel-based low-temperature steel is shown in Table 1;
[0049] (3) Place the polished surface in the prepared corrosive agent in an etched manner, etch it in a 70°C water bath for 90 seconds, rinse it with running water for 8 seconds, then clean it with alcohol, and then blow dry it with a hair dryer to obtain a metallographic sample;
[0050] (4) Place the metallographic sample under a metallographic microscope and magnify it 25 times to obtain Figure 3 , the dendrites are not clear and the secondary dendrite spacing cannot be measured.
[0051] Table 1 Composition (WT%) of nickel-based low-temperature steels tested in the examples and comparative examples
[0052]
[0053] The above description is only a preferred embodiment of the present invention and is not intended to limit the protection scope of the present invention. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention are included in the protection scope of the present invention.
Claims
1. A nickel-based low-temperature steel cast dendrite structure etchant and display method, wherein the detected nickel-based low-temperature steel has a composition (WT) of C = 0.03-0.13%, Mn = 0.30-0.90%, Si = 0.05-0.30%, Ni = 6.50-9.500%, P ≤ 0.010%, S ≤ 0.008%, V ≤ 0.03%, Mo = 0.02-0.30%, and the rest is Fe and unavoidable impurity elements, characterized in that: The process steps include: (1) Preparation of the etchant: The etchant includes a carboxyl compound, which is low-concentration acetic acid, anhydrous ethanol, and a surfactant, wherein the surfactant is a detergent and ferric chloride; the mass ratio of the volume of acetic acid, the volume of anhydrous ethanol, the volume of the detergent, and the mass ratio of ferric chloride is (10-15) mL: (100-110) mL: (3-5) mL: (1.5-2) g. The solution is prepared in a glass container according to the above ratio and is fully stirred with a stirring tool; (2) Preparation of sample polished surface: The nickel-based low-temperature steel ingot sample is subjected to pre-grinding, coarse grinding, fine grinding, polishing, and drying in sequence to obtain a polished surface; (3) Corrosion of the sample: Immerse the smooth surface sample in the prepared corrosive agent and place it in a 60-70℃ water bath for corrosion. Take out the sample and rinse it in running water for 5-10 seconds. Then spray it with alcohol and dry it to obtain a metallographic sample. (4) The prepared metallographic sample is placed under a metallographic microscope to observe the dendrites and measure the secondary dendrite spacing.
2. A nickel-based low-temperature steel cast dendrite structure corrosive agent and display method according to claim 1, characterized in that: The mass concentration of the acetic acid is 10% to 15%.
3. A nickel-based low-temperature steel cast dendrite structure corrosive agent and display method according to claim 1, characterized in that: The surfactant is Lanfei brand worker's hand washing liquid or White Cat brand detergent.
4. A nickel-based low-temperature steel cast dendrite structure corrosive agent and display method according to claim 1, characterized in that: The glass container is a glass cup.
5. A nickel-based low-temperature steel cast dendrite structure corrosive agent and display method according to claim 1, characterized in that: The stirring tool is a glass rod.
6. A nickel-based low-temperature steel cast dendrite structure etchant and display method according to claim 1, characterized in that: The stirring time is 2 to 3 minutes, and the stirring rate is 40 to 50 r / min.
7. A nickel-based low-temperature steel cast dendrite structure corrosive agent and display method according to claim 1, characterized in that: The grinding in step (2) includes pre-grinding with a grinding wheel, and then grinding with 300#, 600#, 1000#, and 2000# water-abrasive sandpaper in sequence. The polishing is polishing with 3um diamond grinding paste.
8. A nickel-based low-temperature steel cast dendrite structure etchant and display method according to claim 1, characterized in that: The etching time in step (3) is 80 to 90 seconds.
9. A nickel-based low-temperature steel cast dendrite structure corrosive agent and display method according to claim 1, characterized in that: The drying in step (3) is performed by using a hair dryer.
10. The nickel-based low-temperature steel cast dendrite structure corrosive agent and display method according to claim 1, characterized in that: The method for measuring the secondary dendrite spacing in step (4) is to adopt the intercept method.