OLED polarizer and preparation method thereof
By optimizing the preparation method of OLED polarizers, controlling the drying temperature and lamination tension of the inner protective film, and combining with surface corona treatment, the problems of easy breakage and difficult-to-control warpage of the liquid crystal phase compensation film are solved, and the polarizer is made thin and Excellent performance and controllable warpage improve the production qualification rate and appearance quality.
Patent Information
- Application Number
- CN202410716205.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-04
- Publication Date
- 2024-10-01
AI Technical Summary
In the production of OLED polarizers, there are problems such as long polarizer production lines, easy damage to the liquid crystal phase compensation film, and difficulty in controlling warpage, resulting in liquid crystal defects and poor lamination.
An OLED polarizer preparation method is adopted, including a protective film, a polarizer substrate, first and second optical compensation films, and a release film. By controlling the drying temperature and lamination tension of the inner protective film, combined with surface corona treatment, optimization The laminating process enables controllability of warpage.
It achieves thin polarizer, excellent performance and controllable warpage, reduces the scratch rate of liquid crystal, and improves the mass production pass rate and appearance yield.
Smart Images

Figure CN118732138A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of polarizers, and in particular to an OLED polarizer and a preparation method thereof. Background Art
[0002] With the development of information and technology, the field of display technology has achieved great progress, and display screens are penetrating into all aspects of human life at an unstoppable speed. OLED display technology is a new generation of flat panel display technology after LCD. Compared with LCD display, OLED display technology has many advantages. LCD displays require backlight modules and upper and lower polarizers, while OLED displays do not require backlight modules, only a layer of polarizer, and have a simpler and thinner structure. In addition, it also has the advantages of fast response speed and flexibility. The rapid progress in technology in recent years and its broad application prospects have made it a hot research topic in the fields of smart phones, smart TVs, AR / VR and wearable electronic devices.
[0003] In order to solve the problem of reflection interference of ambient light, a circular polarizer needs to be added to the outside of the OLED display screen. Furthermore, in order to achieve an integrated black state effect, the compensation effect of the half phase compensation film and the quarter phase compensation film stacking method is the best. The liquid crystal coating phase compensation film has the advantages of adjustable optical compensation characteristics, arbitrary adjustment of the optical axis, thin thickness, and basically no effect on the overall transmittance after bonding. It is the main direction of the future development of OLED polarizers. However, there are two major difficulties in the production and preparation of OLED polarizers with liquid crystal coating half phase compensation film and quarter phase compensation film stacking: first, the polarizer production line is long and has more rollers, and the ultra-thin liquid crystal phase compensation film is very easy to be damaged by friction, resulting in liquid crystal bright lines, liquid crystal cracks, liquid crystal bright spots and other liquid crystal defects; second, the polarizer is a composite structure of multi-layer film and glue. It is affected by the tension of each layer of film material and the temperature and humidity sensitivity of each layer of glue. The warping is difficult to control, especially to prevent the polarizer from being poorly bonded to the panel, and the warping after the release film is torn off needs to be controlled. Summary of the invention
[0004] In view of the above technical problems, the present invention discloses an OLED polarizer and a preparation method thereof. The obtained polarizer is thin, has good performance, and has the characteristics of controllable warping.
[0005] To this end, the technical solution adopted by the present invention is:
[0006] A method for preparing an OLED polarizer, wherein the OLED polarizer comprises, from top to bottom, a protective film, a polarizer substrate, a first optical compensation film, a second optical compensation film, and a release film, wherein the first optical compensation film and the second optical compensation film are half phase compensation films, and the steps of preparing the OLED polarizer include:
[0007] Step S1, preparing a polarizing film; washing and drying the first inner protective film and the second inner protective film, and then bonding the two sides of the polarizing film to the first inner protective film and the second inner protective film respectively through an adhesive, laminating, and drying to obtain a polarizer substrate; wherein, the drying temperature of the first inner protective film layer is higher than the drying temperature of the second inner protective film layer; the bonding tension between the first inner protective film layer and the polarizing film is 40 to 60N higher than the bonding tension between the second inner protective film layer and the polarizing film; the moisture content of the polarizer substrate is 2.00% to 3.00%; wherein, during the bonding process, the bonding tension is controlled by controlling the tension control system.
[0008] Step S2, performing corona treatment on the surface of the first optical compensation film, and then laminating the first optical compensation film and the second inner protective film of the polarizer substrate by an adhesive to obtain a first laminate;
[0009] Step S3, performing corona treatment on the surface of the second optical compensation film, and bonding the first laminate and the second optical compensation film by adhesive to obtain a second laminate;
[0010] Step S4, laminating the second laminate with the release film, and laminating a protective film on the surface of the first inner protective film of the second laminate to obtain an OLED polarizer.
[0011] As a further improvement of the present invention, in step S1, the drying temperature of the first inner protective film is 60-80°C, and the drying temperature of the first inner protective film layer is 10-30°C higher than the drying temperature of the second inner protective film layer; the laminating tension of the first inner protective film layer is 140±10N, and the laminating tension of the second inner protective film layer is 100±10N.
[0012] As a further improvement of the present invention, in step S1, the polarizing film is dried before being laminated, and the drying temperature of the polarizing film is 50-70°C; in step S1, the drying temperature of the polarizer substrate is 70-90°C.
[0013] As a further improvement of the present invention, in step S2, the surface treatment is corona treatment, glue coating, and drying treatment in sequence; and both sides of the first optical compensation film are subjected to corona treatment.
[0014] As a further improvement of the present invention, the corona treatment is carried out using a power density automatic mode corona; the power density of the corona equipment is 0 to 500 W*min / ㎡; preferably, the power density of the corona equipment is 30 to 200 W*min / ㎡.
[0015] As a further improvement of the present invention, after corona treatment, the water drop contact angle of the first optical compensation film is 10° to 60°; preferably, the water drop contact angle of the first optical compensation film is 20° to 50°.
[0016] As a further improvement of the present invention, the first optical compensation film is a liquid crystal type half phase compensation film, and the second optical compensation film is a liquid crystal type quarter phase compensation film.
[0017] As a further improvement of the present invention, the thickness of the first optical compensation layer is 1-10 μm; the thickness of the first optical compensation layer is 1-5 μm.
[0018] As a further improvement of the present invention, in step S2, one side of the first optical compensation film is first subjected to corona treatment, and then an adhesive is applied thereto, and after drying, the film is laminated to the second inner protective film of the polarizer substrate. Furthermore, the lamination tension of the polarizer substrate is 200±10N, and the lamination tension of the first optical compensation film is 80±10N.
[0019] As a further improvement of the present invention, in step S3, the other side of the first optical compensation film and one side of the second optical compensation film are corona treated, and an adhesive is coated on one side of the second optical compensation film. After drying, the second side of the second optical compensation film is bonded to the other side of the first optical compensation film of the first laminate. Furthermore, when one side of the second optical compensation film is bonded to the other side of the first optical compensation film of the first laminate, the bonding tension of the first laminate is 200±10N, and the bonding tension of the second optical compensation film is 80±10N.
[0020] As a further improvement of the present invention, in step S4, the other side of the second optical compensation film is corona treated, the release agent surface of the release film is coated with adhesive, dried, and laminated to the other side of the second optical compensation film; further, when the release agent surface of the release film is laminated to the other side of the second optical compensation film, the lamination tension of the second laminate is 200±10N, and the lamination tension of the second optical compensation film is 80±10N.
[0021] The present invention also discloses an OLED polarizer, which is prepared by using any one of the above methods for preparing the OLED polarizer.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] First, by adopting the technical scheme of the present invention, through optimizing the process flow, the temperature difference and tension difference between the upper and lower first inner protective film layers and the second inner protective film layers, the moisture content of the polarizer substrate, and the fitting tension between the first optical compensation film, the second optical compensation film, the release film and the laminate are controlled in a coordinated manner, so as to control the warping of the polarizer with both preservation and release and the warping with preservation but no release, realize the controllable warping, and achieve the batch production qualified rate of up to 100%.
[0024] Second, the first optical compensation film and the second optical compensation film of the technical solution of the present invention respectively use liquid crystal type half and quarter phase compensation films, and the thickness of the prepared OLED polarizer is ultra-thin, only about 90μm, and the liquid crystal compensation film has basically no effect on the overall transmittance after bonding. The liquid crystal molecules themselves have the characteristics of birefringence, and the liquid crystal type half and quarter phase compensation films use an alignment method to adjust the angle to match the polarizer axis, so each layer of material can be roll-to-roll bonded, reducing material loss.
[0025] Third, the technical solution of the present invention adopts an online single-side corona method in the laminating process of the first optical compensation film and the release film, and an online double-side corona method in the laminating process of the second optical compensation film and the release film. After corona treatment, the film is timely laminated with the best adhesion, avoiding the occurrence of corona failure during turnover and storage; and 5 processes are used to achieve an 8-layer OLED polarizer, and the process path is simple. In addition, after the corona treatment, the first optical compensation film and the second optical compensation film are not subjected to roller friction, and are immediately laminated with the adjacent layer, avoiding the generation of liquid crystal defects such as liquid crystal scratches, and the liquid crystal scratch defect rate is reduced from the highest 3.8% to the lowest 0.4%, improving the appearance yield of the polarizer. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 is a schematic structural diagram of an OLED polarizer according to Example 1 of the present invention;
[0027] Figure 2 4 is a sampling diagram of a warpage test according to an embodiment of the present invention.
[0028] Reference numerals include:
[0029] 1-protective film layer, 2-polarizer substrate, 3-first optical compensation layer, 4-second optical compensation layer, 5-release film, 6-first adhesive layer, 7-second adhesive layer, 8-third adhesive layer;
[0030] 20-functional coating, 1-first inner protective film, 22-polarizing film, 23-second inner protective film. DETAILED DESCRIPTION
[0031] The preferred embodiments of the present invention are described in further detail below.
[0032] Example 1
[0033] like Figure 1 As shown, an OLED polarizer includes a protective film layer 1, a polarizer substrate 2, a first adhesive layer 6, a first optical compensation layer 3, a second adhesive layer 7, a second optical compensation layer 4, a second adhesive layer 8, and a release film 5. By providing the first optical compensation layer 4 and the second optical compensation layer 6, the display can have a better display effect. The polarizer substrate 2 includes a first inner protective film 21, a polarizing film 22 and a second inner protective film 23, and the polarizing film 22 is located between the first inner protective film layer 21 and the second inner protective film layer 23; a functional coating 20 is provided on the top of the first inner protective film layer 21. Furthermore, the first optical compensation layer 3 is a liquid crystal type half phase compensation film, and the first optical compensation layer 4 is a liquid crystal type quarter phase compensation film.
[0034] The method for preparing the above-mentioned OLED polarizer comprises the following steps:
[0035] Step S10, preparing a polarizer substrate: swelling, dyeing, water washing I, stretching, water washing II, coloring, and drying a polyvinyl alcohol resin film to obtain a polarizing film; at the same time, the first inner protective film layer and the second inner protective film layer are washed and dried, and then the polarizing film and the first inner protective film layer and the second inner protective film layer are bonded with an adhesive to obtain a laminate of the polarizing film and the two inner protective film layers; and then the laminate is dried to obtain a polarizer substrate.
[0036] The thickness of the polarizing film is generally 20 μm or less, preferably 5 to 15 μm. A functional coating, such as a hardening coating, a low-reflection coating, and an anti-glare coating, is fixedly connected to the top of the first inner protective film layer, preferably a transparent hardening coating. The thickness of the hardening coating is 5 μm. The transparent hardening coating can effectively resist scratches during long-term use, thereby increasing the service life of the display. The thickness of the first inner protective film layer and the second inner protective film layer is generally 50 μm or less, preferably 10 to 30 μm. The material of the first inner protective film layer and the second inner protective film layer is generally triacetyl cellulose film (TAC), cycloolefin polymer film (COP), polymethyl methacrylate film (PMMA), polyester film (PET), etc., preferably a TAC film with good optical properties, mature technology, stable quality, and easy cutting.
[0037] Furthermore, the warping of the polarizer substrate is controlled by controlling the drying temperature of the first inner protective film layer and the second inner protective film layer. The drying temperature of the first inner protective film layer is higher than that of the second inner protective film layer, and the temperature difference is preferably 10 to 30°C. The drying temperature of the first inner protective film layer is preferably 80±10°C, and the drying temperature of the second inner protective film layer is preferably 60±10°C.
[0038] Furthermore, the warping of the polarizer substrate is controlled by controlling the lamination tension between the first inner protective film layer and the second inner protective film layer. The lamination tension of the first inner protective film layer is higher than that of the second inner protective film layer, and the lamination tension difference is preferably 40 to 60 N. Furthermore, the lamination tension of the first inner protective film layer is 140 ± 10 N, and the lamination tension of the second inner protective film layer is 100 ± 10 N.
[0039] Furthermore, the warpage change can be controlled by controlling the moisture content of the polarizer substrate. Specifically, the moisture content can be controlled by controlling the drying temperature of the polarizer film and the polarizer substrate, wherein the drying temperature of the polarizer film is preferably 50 to 70° C., and the drying temperature of the polarizer substrate is preferably 70 to 90° C. The moisture content of the polarizer substrate is preferably 2.00% to 3.00%.
[0040] Step S20, the polarizer substrate and the first optical compensation layer are laminated to obtain a first laminate: because the first optical compensation layer has a large contact angle and low adhesive performance, it is necessary to first perform surface treatment on one side of the first optical compensation layer to enhance its adhesiveness. Then, an adhesive layer is coated on the treated surface, and after drying, it is laminated to the bottom surface of the second inner protective film layer of the polarizer substrate; further, the lamination tension is 200+80N.
[0041] Furthermore, the first optical compensation layer is a half phase compensation film, preferably a liquid crystal half phase compensation film. The thickness of the first optical compensation layer is 1 to 10 μm, preferably 1 to 5 μm. By setting a liquid crystal first optical compensation layer, the thickness of the polarizer can be greatly reduced. Due to the characteristics of liquid crystal materials, the first optical compensation layer is subjected to online corona treatment. That is, after corona, gluing, and drying, it is immediately bonded to the polarizer substrate, the process path is simple, the turnover and storage time are reduced, it has the best bonding effect, and also improves the apparent quality of the polarizer.
[0042] Furthermore, the first optical compensation layer and the second optical compensation layer both need to be corona coated on both sides to reduce their contact angles and increase their hydrophilicity, thereby improving the bonding fastness and ensuring the reliability of the polarizer and other properties.
[0043] Furthermore, the power density automatic mode corona is adopted, that is, the power density is set, and the corona power can be automatically adjusted according to the machine speed when the width is constant, which can avoid the abnormal instability of the corona intensity caused by the unstable machine speed. The power density is 0 to 500W*min / ㎡, preferably 30 to 200W*min / ㎡. Furthermore, the corona of the half phase compensation film, by controlling the power density, the water droplet contact angle after corona is 10° to 60°, preferably 20° to 50°.
[0044] Step S30, laminating the first laminate and the second optical compensation layer to obtain a second laminate, the steps comprising: similarly corona-treating the bottom surface of the first optical compensation layer of the first laminate, and corona-treating one side of the second optical compensation layer, and then coating the corona-treating surface of the second optical compensation layer with an adhesive, and after drying, laminating the second laminate with the bottom surface of the corona-treating first optical compensation layer of the first laminate; the laminating tension is 200+80N.
[0045] Step S40, the second laminate is bonded to the release film, the steps comprising: corona-treating the bottom surface of the second optical compensation layer of the second laminate, coating the release agent surface of the release film with adhesive, and after drying, bonding with the bottom surface of the second optical compensation layer of the second laminate after corona-treating; the bonding tension is 200+80N.
[0046] The liquid crystal type half phase compensation film and liquid crystal type quarter phase compensation film are extremely thin, and the polarizer production line is long and has many rollers, so they are easily damaged by friction, resulting in defects such as liquid crystal scratches, liquid crystal cracks and liquid crystal bright spots. They need to be corona treated without roller friction and immediately bonded to the adjacent layers to avoid the occurrence of liquid crystal defects.
[0047] The data of three batches of Example 1 using the above method are shown in Table 1. At the same time, for comparison, in Example 1, the first optical compensation layer, i.e., the liquid crystal type half phase compensation film, and the second optical compensation layer, i.e., the liquid crystal type quarter phase compensation film, are not subjected to roller friction after corona treatment, and are immediately bonded to the adjacent layer, while the control example 1 is subjected to roller friction after corona treatment. Both the control example 1 and Example 1 are three batches, and the data are shown in Table 1. It can be seen that the polarizer coil produced by the front process is cut, edged, and inspected in the back process, and the defect rate of liquid crystal type is reduced by an average of 2.55% after improvement.
[0048] Table 1
[0049] batch Total number of inspections (pieces) LCD scratch defective number (pcs) LCD scratch defect rate Comparative Example 1 Lot.1 7961 144 1.81% Comparative Example 1 Lot.2 36809 1385 3.76% Comparative Example 1 Lot.3 99910 3233 3.24% Example 1 Lot.1 340 2 0.59% Example 1 Lot.2 79531 328 0.41% Example 1 Lot.3 372794 3006 0.81%
[0050] Warp Control Effect:
[0051] Warpage test sampling Figure 2 As shown, with the protective film facing upward, three samples on the width OS, CS, and DS sides are taken respectively, with the short side of the sample parallel to the compensation axis, and the angle between the compensation axis and the absorption axis is 45°. Then the warpage of the protective film and release film (referred to as "protection and release") is tested first, and the highest warpage value of the warpage of the four corners is tested respectively. The warpage toward the protective film surface is recorded as positive warpage, and the warpage toward the release film surface is recorded as negative warpage, and it is judged according to the specification of -5mm to +5mm. Similarly, the release film is torn off, and the warpage of the protective film and the release film torn off (referred to as "protection without release") is tested, and it is judged according to the specification of -9mm to +5mm.
[0052] Example 1 ensures that the polarizer has warping with or without release, and the qualified rate of mass production is as high as 100% by collaboratively controlling the temperature difference and tension difference between the upper and lower TACs (i.e., the first inner protective film layer and the second inner protective film layer), the moisture content of the polarizer substrate, and the fitting tension between the first optical compensation film, the second optical compensation film, the release film and the laminate.
[0053] On the basis of Example 1, the lamination tension between the polarizer substrate II and the half phase compensation film, the lamination tension between the first laminate and the quarter phase compensation film, and the lamination tension between the second laminate and the release film are changed, as shown in Table 2. Among them, the temperature difference between the upper and lower TACs of Example 1 and the control example are 80°C and 60°C respectively, and the drying temperature of the polarizing layer is 60°C. The warpage qualified rates of the control example and the example under different process conditions are shown in Table 2.
[0054] Table 2
[0055]
[0056] Note: In the table, the data in the column of polarizer substrate and half-phase compensation film bonding tension (N) indicates that the tension of the polarizer substrate is 200N, and the bonding tension of the half-phase compensation film is 80N. The same is true for other data.
[0057] Each control example and Example 1 includes 6 groups of warpage with preservation and warpage without preservation, and the data are shown in Table 3 and Table 4.
[0058] Table 3
[0059]
[0060] Table 4
[0061]
[0062]
[0063] By comparing the embodiment with the comparative example 4, it can be seen that under the same process conditions, the qualified rates of substrate moisture content ≤3.1% with warpage and without warpage are higher than those with substrate moisture content>3.1%, which means that the lower the moisture content of the substrate, the lower the shrinkage rate of the polarizer and the lower the warpage.
[0064] By comparing the embodiment with the control example 2, it can be seen that under the same process conditions, the qualified rates of the upper and lower TAC tension difference of 30N with warping and the qualified rates of the upper and lower TAC tension difference of 50N with warping and the qualified rates of the upper and lower TAC tension difference of 50N with warping and the qualified rates of the upper and lower TAC tension difference of 60N with warping are both higher than those of the upper and lower TAC tension difference of 60N. This shows that the smaller the upper and lower TAC tension difference is, the smaller the substrate warping is, and the smaller the corresponding OLED polarizer warping is. However, due to the lamination of the half and quarter phase compensation films and release films, the polarizer will change in the negative warping direction, so the substrate needs to have a certain positive warping height for balance.
[0065] By comparing the control example 3 with the control example 5, it can be seen that under the same conditions of other processes, the lamination tension between the substrate and the half phase compensation film, the lamination tension between the first laminate and the quarter phase compensation film, and the lamination tension between the second laminate and the release film are 200N+80N, 200N+80N, and 200N+80N, respectively, and the pass rate of the non-release warpage is better than that of 200N+80N, 150N+70N, and 180N+100N. This shows that the same tension difference is adopted in the three processes, and the shrinkage stress of the half phase compensation film, the quarter phase compensation film, and the release film is controlled to a considerable extent, the stress of each layer is uniform, and the warpage is easier to control.
[0066] The polarizer prepared in this embodiment has a pass rate of 83% with or without warping, and a pass rate of 100% without or without warping.
[0067] In summary, the preparation method of the OLED polarizer provided by the present invention has the following advantages by optimizing the process flow:
[0068] First, the first optical compensation film adopts a liquid crystal half-phase compensation film, and the second optical compensation film adopts a quarter-phase compensation film. The prepared OLED polarizer is ultra-thin, only about 90μm, and the liquid crystal compensation film has basically no effect on the overall transmittance after bonding.
[0069] Secondly, the liquid crystal molecules themselves have the characteristic of birefringence. The first optical compensation film and the second optical compensation film are aligned to adjust the angle to match the axial direction of the polarizer, so each layer of material can be roll-to-roll laminated, reducing material loss.
[0070] Thirdly, the first optical compensation film and release film lamination process adopts an online single-sided corona method, and the second optical compensation film and release film lamination process adopts an online double-sided corona method. After corona treatment, they are laminated in time with the best adhesion, avoiding the occurrence of corona failure during turnover and storage. And 5 processes are required to achieve an 8-layer OLED polarizer, and the process path is simple.
[0071] Fourthly, after corona treatment, the first optical compensation film and the second optical compensation film are immediately bonded to the adjacent layers without roller friction, thus avoiding the occurrence of liquid crystal defects such as liquid crystal scratches. The liquid crystal scratch defect rate is reduced from a maximum of 3.8% to a minimum of 0.4%, thereby improving the appearance yield of the polarizer.
[0072] Fifth, by collaboratively controlling the drying temperature difference and tension difference of the first inner protective film and the second inner protective film, the moisture content of the polarizer substrate, and the bonding tension of the first optical compensation film, the second optical compensation film, the release film and the laminate, the warping of the polarizer with or without release is controlled, and the qualified rate of mass production is as high as 100%.
[0073] The above contents are further detailed descriptions of the present invention in combination with specific preferred embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, which should be regarded as falling within the protection scope of the present invention.
Claims
1. A method for preparing an OLED polarizer, characterized in that: The OLED polarizer includes a protective film, a polarizer substrate, a first optical compensation film, a second optical compensation film, and a release film from top to bottom, wherein the first optical compensation film is a liquid crystal type half phase compensation film, and the second optical compensation film is a liquid crystal type quarter phase compensation film. The preparation steps of the OLED polarizer include: Step S1, preparing a polarizing film; washing and drying a first inner protective film and a second inner protective film, and then laminating and drying the two sides of the polarizing film with the first inner protective film and the second inner protective film respectively; wherein the drying temperature of the first inner protective film layer is higher than the drying temperature of the second inner protective film layer; the laminating tension between the first inner protective film layer and the polarizing film is 40 to 60 N higher than the laminating tension between the second inner protective film layer and the polarizing film; the moisture content of the polarizing film substrate is 2.00% to 3.00%; Step S2, performing corona treatment on the surface of the first optical compensation film, and then laminating the first optical compensation film and the second inner protective film of the polarizer substrate by an adhesive to obtain a first laminate; Step S3, performing corona treatment on the surface of the second optical compensation film, and bonding the first laminate and the second optical compensation film by adhesive to obtain a second laminate; Step S4, laminating the second laminate with the release film, and laminating a protective film on the surface of the first inner protective film of the second laminate to obtain an OLED polarizer.
2. The method for preparing an OLED polarizer according to claim 1, characterized in that: In step S1, the drying temperature of the first inner protective film is 60-80°C, and the drying temperature of the first inner protective film layer is 10-30°C higher than the drying temperature of the second inner protective film layer; the laminating tension of the first inner protective film layer is 140±10N, and the laminating tension of the second inner protective film layer is 100±10N.
3. The method for preparing an OLED polarizer according to claim 2, characterized in that: In step S1, the polarizing film is dried and then laminated, and the drying temperature of the polarizing film is 50-70°C; in step S1, the drying temperature of the polarizer substrate is 70-90°C.
4. The method for preparing an OLED polarizer according to claim 2, wherein: In step S2, the surface treatment is sequentially performing corona treatment, glue coating, and drying treatment; both sides of the first optical compensation film are subjected to corona treatment.
5. The method for preparing an OLED polarizer according to claim 4, characterized in that: The corona treatment is performed using a power density automatic mode corona; the power density of the corona equipment is 0 to 500 W*min / ㎡; preferably, the power density of the corona equipment is 30 to 200 W*min / ㎡; After the corona treatment, the water drop contact angle of the first optical compensation film is 10° to 60°; preferably, the water drop contact angle of the first optical compensation film is 20° to 50°.
6. The method for preparing an OLED polarizer according to claim 5, characterized in that: The thickness of the first optical compensation layer is 1-10 μm; the thickness of the first optical compensation layer is 1-5 μm.
7. The method for preparing an OLED polarizer according to claim 6, characterized in that: In step S2, one side of the first optical compensation film is first subjected to corona treatment, and then coated with adhesive, and after drying, is laminated to the second inner protective film of the polarizer substrate.
8. The method for preparing an OLED polarizer according to claim 7, characterized in that: In step S3, the other side of the first optical compensation film and one side of the second optical compensation film are subjected to corona treatment, and an adhesive is coated on one side of the second optical compensation film, and after drying, the adhesive is bonded to the other side of the first optical compensation film of the first laminate.
9. The method for preparing an OLED polarizer according to claim 8, characterized in that: In step S4, the other side of the second optical compensation film is subjected to corona treatment, and the release agent side of the release film is coated with adhesive, dried, and then laminated to the other side of the second optical compensation film.
10. An OLED polarizer, characterized in that: The OLED polarizer is prepared by the preparation method of any one of claims 1 to 9.