Preparation method of electrode circuit
By depositing barrier layers and Cu layers in the production of semiconductor integrated circuits, making electroplated photoresist, and using PECVD and Ar plasma bombardment technology to protect Cu sidewalls, the breakage and line width caused by wet etching of Cu electrode lines are solved. Solve the problem of poor uniformity and achieve high-density and uniform Cu wire preparation.
Patent Information
- Application Number
- CN202410811946.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-21
- Publication Date
- 2024-10-01
AI Technical Summary
In the production process of semiconductor integrated circuits, the wet etching method of Cu electrode lines causes problems such as breakage and poor line width uniformity when the Cu line width and line spacing are below 10 μm/10 μm.
The barrier layer and Cu layer are sequentially deposited on the substrate to make electroplated photoresist, and then the electroplated Cu layer is deposited. After stripping the photoresist, the first etching is performed, and then the etching barrier layer is deposited by PECVD and controlled by Ar plasma bombardment. The incident angle is to remove the etching barrier layer, protect the electroplated Cu sidewall, and perform a second etching to remove the uncovered Ti layer to ensure line width consistency.
It achieves high-density preparation of Cu wires, with line width and line spacing below 5 μm/5 μm, and good line width uniformity, meeting the needs of high-density IC carrier boards.
Smart Images

Figure HDA0004906394610000011 
Figure HDA0004906394610000012 
Figure HDA0004906394610000013
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of integrated circuits, and more specifically, to a method for preparing an electrode circuit. Background Art
[0002] In the production process of semiconductor integrated circuits, Cu is usually used as the electrode material. Generally, a TiCu seed layer with a thickness of 100-500nm is deposited on the substrate by magnetron sputtering deposition. Then, a Cu film material of more than 5μm is deposited by electroplating. The TiCu seed layer is much thinner than the thickness of electroplated Cu.
[0003] After the electroplating of Cu is completed, the electroplating photoresist needs to be stripped, the substrate is placed in a Cu etching solution, the entire surface is etched, and the seed layer on which the electroplated Cu is not deposited is etched away to obtain an electroplated Cu electrode pattern. During the etching process, the entire surface of the electroplated Cu is exposed to the Cu etching solution and is etched together with the seed layer. Since the thickness of the electroplated Cu is much greater than the thickness of the seed layer, after the exposed seed layer is etched, most of the electroplated Cu is retained to form a Cu electrode layer pattern. However, the current etching method is wet etching, which is characterized by isotropy. While etching the seed layer downward, the electroplated Cu film layers on both sides will also be etched sideways, especially when the Cu line width and line spacing are below 10μm / 10μm, problems such as broken lines and poor line width uniformity are prone to occur.
[0004] Therefore, there is an urgent need to develop a method for preparing electrode circuits, especially when the Cu line width and line spacing are below 10μm / 10μm, it is not easy to have problems such as broken wires, and high-density electrode circuits can be obtained to improve line width uniformity. Summary of the invention
[0005] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention provides a method for preparing an electrode circuit. The method provided by the present invention can produce a high-density electrode circuit, and when the Cu line width and line spacing are below 10μm / 10μm, the problem of line breakage is not likely to occur, and the line width uniformity is high.
[0006] A first aspect of the present invention provides a method for preparing an electrode circuit.
[0007] Specifically, a method for preparing an electrode circuit comprises the following steps:
[0008] (1) depositing a barrier layer and a Cu layer on the surface of the substrate in sequence, making an electroplated photoresist, and then depositing an electroplated Cu layer;
[0009] (2) stripping the electroplated photoresist to obtain a substrate after the electroplated photoresist is stripped;
[0010] (3) placing the substrate after the electroplating photoresist is stripped in an etching solution for a first etching, until the Cu layer at the original position of the electroplating photoresist is completely etched, thus completing the first etching to obtain a substrate after the first etching;
[0011] (4) depositing an etching stop layer on the surface of the substrate after the first etching by plasma enhanced chemical vapor deposition to obtain a substrate containing the etching stop layer;
[0012] (5) using Ar plasma bombardment (Plasma Enhanced Chemical Vapor Deposition, referred to as PECVD) to bombard the substrate surface containing the etching barrier layer until the etching barrier layer covering the electroplated Cu layer surface and the Ti layer surface where the electroplated photoresist was originally located is etched away, and the bombardment is terminated, wherein the incident angle of the Ar plasma bombardment is 80-90° with the substrate surface;
[0013] (6) After the bombardment, the substrate is placed in an etching solution for a second etching, and the etching is terminated until the Ti layer at the original location of the electroplated photoresist is completely etched.
[0014] After the etching of the Cu layer at the original location of the electroplated photoresist is completed, the PECVD is performed to deposit an etching barrier layer with excellent step coverage on the substrate; then, Ar plasma is used to bombard the substrate surface, and the included angle between the incident angle of the Ar plasma bombardment and the substrate surface is controlled to be 80-90 degrees, so that the etching barrier layer covering the electroplated Cu surface and the Ti layer surface (i.e., the gap between the electroplated Cu wires) is etched away, and the etching barrier layer of the electroplated Cu side wall is retained; then, the substrate is placed in an etching solution for a second etching, and the Ti layer at the original location of the electroplated photoresist that is not covered by the electroplated Cu and is exposed to the outside is etched away; because the electroplated Cu side wall is protected by the etching barrier layer, the side wall is not affected by the etching solution during etching and side etching occurs, so the line width and line spacing of the Cu wire will not increase, the line width of the electroplated Cu wire is consistent with the preset line width, and the line width and line spacing can reach 5μm / 5μm or less, so that a high-density Cu wire can be obtained, and the Cu wire has good uniformity.
[0015] Preferably, in step (1), the substrate is one of glass, EMC, PI, and ABF.
[0016] Preferably, in step (1), the barrier layer is one of a Ti layer, a Mo layer, a Ta layer and a TiW layer.
[0017] Further preferably, in step (1), the barrier layer is a Ti layer. The Ti layer and the Cu layer are collectively referred to as a TiCu seed layer. Cu serves as a conductive layer and the Ti layer serves as a barrier layer.
[0018] Preferably, in step (1), the thickness of the barrier layer is 20-200 nm.
[0019] Preferably, in step (1), the sum of the thickness of the Cu layer and the electroplated Cu layer is 5-6 μm.
[0020] Preferably, in step (2), the stripping solution is ethylene glycol and / or amide solution.
[0021] Preferably, in step (2), the peeling temperature is 30-60°C.
[0022] Preferably, in step (3) and step (6), the etching solution is fluorine-containing H 2 O 2 Etching fluid.
[0023] Further preferably, in step (3) and step (6), the etching solution is a fluorine-containing H 2 O 2 Etching fluid.
[0024] Preferably, in step (3), the etching rate of the Cu layer is 6-15 nm / s, and / or the etching rate of the barrier layer is 0.1-1 nm / s. The etching rate of the barrier layer is relatively slow. In the etching solution, the entire surface of the substrate will be etched by the etching solution, and side etching will occur on both sides of the electroplated Cu; the etching time required for the barrier layer is long, and the impact of side etching is greater; the Cu layer of the seed layer is etched away first.
[0025] Preferably, in step (4), the reaction gas for plasma enhanced chemical vapor deposition is SiH 4 and N 2 O, or the reaction gas of the plasma enhanced chemical vapor deposition is SiH 4 and NH 3 .SiH 4 +N 2 O→SiO 2 or SiH 4 +NH 3 →SiNx.
[0026] Preferably, in step (4), the etching stop layer is SiO 2 layer and / or SiNx layer.
[0027] Preferably, in step (4), the thickness of the etching stop layer is 1-20 nm.
[0028] Preferably, in step (4), the electroplated Cu surface, the electroplated Cu sidewall, and the surface of the Ti layer where the electroplated photoresist was originally located all contain an etching stop layer.
[0029] The thickness of the etching barrier layer on the electroplated Cu surface, the electroplated Cu sidewall, and the Ti layer surface where the electroplated photoresist was originally located is almost the same. Due to the excellent step coverage of PECVD, the thickness of the etching barrier layer deposited on the electroplated Cu surface, the electroplated Cu sidewall, and the gap between the electroplated Cu wires (above the exposed Ti film, i.e., the Ti film where the electroplated photoresist was originally located) is not much different.
[0030] Preferably, in step (4), the temperature of the plasma enhanced chemical vapor deposition is 100-400°C.
[0031] Preferably, in step (5), the angle between the incident angle of the Ar plasma bombardment and the substrate surface is 90°, that is, the incident angle of the Ar plasma bombardment is perpendicular to the substrate surface.
[0032] Preferably, in step (5), after the bombardment is completed, the etching barrier layer of the electroplated Cu sidewall is retained.
[0033] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0034] The present invention first deposits a barrier layer and a Cu layer on the substrate to make an electroplated photoresist, then electroplates the Cu layer, peels off the electroplated photoresist, and then places it in an etching solution to etch away the Cu layer at the original location of the electroplated photoresist, which requires a shorter etching time, and then deposits an etching barrier layer with excellent step coverage on the substrate by PECVD; then Ar The surface of the substrate is bombarded with Ar plasma, and the angle between the incident angle of the Ar plasma bombardment and the substrate surface is controlled to be 80-90°, so as to etch away the etching barrier layer covering the electroplated Cu surface and the Ti layer surface (i.e., the gap between the electroplated Cu wires), and retain the etching barrier layer of the electroplated Cu side wall; the substrate is then placed in an etching solution for a second etching, so as to etch away the Ti layer which is not covered by the electroplated Cu and is exposed to the outside and is where the electroplated photoresist was originally located; since the electroplated Cu side wall is protected by the etching barrier layer, its side wall is not affected by the etching solution during etching and no side etching occurs, so the line width and line spacing of the Cu wire will not increase, and the line width of the electroplated Cu wire is consistent with the preset line width, and the line width and line spacing can reach below 5μm / 5μm, so that a high-density Cu wire can be obtained, and the Cu wire has good uniformity, which meets the growing needs of advanced packaging and high-density IC substrates. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 Schematic diagram of a substrate after TiCu layer deposition, electroplating photoresist production, and Cu electroplating are completed in step (1) of Example 1 of the present invention;
[0036] Figure 2 This is a schematic diagram of the substrate after stripping the electroplated photoresist in step (2) of Example 1 of the present invention;
[0037] Figure 3 Schematic diagram of a substrate in which the Cu layer at the location where the electroplated photoresist was originally located is etched away in step (3) of Example 1 of the present invention;
[0038] Figure 4 This is a schematic diagram of a substrate for depositing an etch stop layer by PECVD in step (4) of Example 1 of the present invention;
[0039] Figure 5 Schematic diagram of a substrate in which the vertically incident Ar plasma bombards the surface of the substrate to remove the electroplated Cu surface and the etching stop layer where the electroplated photoresist was originally located in step (5) of Example 1 of the present invention;
[0040] Figure 6 Schematic diagram of the substrate in which the Ti layer not covered by the electroplated Cu (the Ti layer where the electroplated photoresist was originally located) is etched away in step (6) of Example 1 of the present invention. DETAILED DESCRIPTION
[0041] In order to make the technical scheme of the present invention more clearly understood by those skilled in the art, the following embodiments are listed for illustration. It should be pointed out that the following embodiments do not limit the protection scope of the present invention.
[0042] Unless otherwise specified, the raw materials, reagents or devices used in the following examples can be obtained from conventional commercial sources or by existing known methods.
[0043] Example 1
[0044] A method for preparing an electrode circuit comprises the following steps:
[0045] (1) a 100 nm Ti layer and a 300 nm Cu layer (seed layer Cu) are sequentially deposited on the surface of the substrate, and then a coating, exposure and development method are used to prepare an electroplating photoresist, and then an electroplating method is used to deposit electroplated Cu; the substrate after step (1) is as follows Figure 1 As shown; wherein the total thickness of the Cu film (i.e., the sum of the thickness of the seed layer Cu and the electroplated Cu) is about 6 μm;
[0046] (2) Using ethylene glycol stripping solution, strip the electroplated photoresist at 30° C. After completing step (2), the substrate is as follows: Figure 2 As shown;
[0047] (3) Place the substrate after stripping the electroplated photoresist in an etching solution for the first etching. The etching solution is H 2 O 2The etching solution has a concentration of 15%, a process temperature of 30°C, an etching rate of 10 nm / s for the Cu layer, and an etching rate of 0.4 nm / s for the Ti layer. The etching rate of the Cu layer is faster, and the Cu layer at the original location of the electroplated photoresist will be etched away first, until the Cu layer is completely etched, and the first etching is completed; the substrate after completing step (3) is as follows Figure 3 As shown;
[0048] (4) SiO with a thickness of 10 nm is deposited on the substrate surface after the first etching by PECVD deposition. 2 The etching barrier layer is etched to obtain a substrate containing an etching barrier layer. At this time, the electroplated Cu surface, the electroplated Cu sidewall, and the Ti layer surface where the electroplated photoresist was originally located all contain an etching barrier layer with a thickness of 10 nm. The substrate after completing step (4) is as follows Figure 4 As shown;
[0049] (5) Ar plasma bombardment is performed on the surface of the substrate containing the etching barrier layer by vertical incidence until the etching barrier layer covering the surface of the electroplated Cu layer and the surface of the Ti layer where the electroplated photoresist was originally located is etched away, and the bombardment is terminated. At this time, the etching barrier layer on the side wall of the electroplated Cu is retained. The substrate after completing step (5) is as follows Figure 5 As shown;
[0050] (6) The substrate is placed in an etching solution for a second etching until the Ti layer at the original location of the electroplated photoresist is completely etched, and the etching is completed. The substrate after step (6) is as follows Figure 6 The designed line width is 5 μm, and the 510mm*515mm large board is tested. The results show that the electrode line width prepared in Example 1 is in the range of 4.8-5.2 μm, indicating that since the electroplated Cu sidewall is protected by the etching barrier layer, the sidewall is not affected by the etching solution during etching, and no side etching occurs. Therefore, it can meet the requirements of high-density electrode lines (line width requirement 5±0.3 μm), and the uniformity of the Cu conductor is good.
[0051] Comparative Example 1
[0052] This comparative example provides a method for preparing an electrode circuit, which differs from Example 1 in that no etching barrier layer is deposited and no Ar plasma bombardment is performed, that is, step (4) and step (5) are not performed. The designed line width is 5 μm, and the line width of the electrode circuit prepared in Comparative Example 1 is 2.7-4.8 μm in a 510 mm*515 mm large board test, indicating that relatively serious side etching occurs and cannot meet the requirements of high-density electrode circuits.
Claims
1. A method for preparing an electrode circuit, characterized in that: The steps include: (1) depositing a barrier layer and a Cu layer on the surface of the substrate in sequence, making an electroplated photoresist, and then depositing an electroplated Cu layer; (2) stripping the electroplated photoresist to obtain a substrate after the electroplated photoresist is stripped; (3) placing the substrate after the electroplating photoresist is stripped in an etching solution for a first etching, until the Cu layer at the original position of the electroplating photoresist is completely etched, thus completing the first etching to obtain a substrate after the first etching; (4) depositing an etching stop layer on the surface of the substrate after the first etching by plasma enhanced chemical vapor deposition to obtain a substrate containing the etching stop layer; (5) bombarding the substrate surface containing the etching barrier layer with Ar plasma until the etching barrier layer covering the electroplated Cu layer surface and the Ti layer surface is etched away, and the bombardment is terminated, wherein the incident angle of the Ar plasma bombardment is 80-90° with respect to the substrate surface; (6) After the bombardment, the substrate is placed in an etching solution for a second etching, and the etching is terminated until the Ti layer at the original location of the electroplated photoresist is completely etched.
2. The preparation method according to claim 1, characterized in that: In step (1), the barrier layer is one of a Ti layer, a Mo layer, a Ta layer, and a TiW layer.
3. The preparation method according to claim 2, characterized in that: In step (1), the thickness of the barrier layer is 20-200 nm.
4. The preparation method according to claim 1, characterized in that: In step (1), the thickness of the Cu layer is 200-600 nm.
5. The preparation method according to claim 1, characterized in that: In step (3), the etching rate of the Cu layer is 6-15 nm / s, and / or the etching rate of the barrier layer is 0.1-1 nm / s.
6. The preparation method according to claim 1, characterized in that: In step (4), the reaction gas of the plasma enhanced chemical vapor deposition is SiH4 and N2O, or the reaction gas of the plasma enhanced chemical vapor deposition is SiH4 and NH3.
7. The preparation method according to claim 6, characterized in that: In step (4), the etching stop layer is a SiO2 layer and / or a SiN x layer.
8. The preparation method according to claim 7, characterized in that: In step (4), the thickness of the etching stop layer is 1-20 nm.
9. The preparation method according to claim 1, characterized in that: In step (4), the temperature of the plasma enhanced chemical vapor deposition is 100-400°C.
10. The preparation method according to claim 1, characterized in that: In step (5), the angle between the incident angle of the Ar plasma bombardment and the substrate surface is 90°.