Method and system for enhancing bonding strength of thermal ultrasonic lead

By adopting the step preheating method in the gold wire bonding system, the problems of intermetallic compounds and Kirkendall voids caused by heterogeneous metal contact are solved, the bonding strength and lifespan are improved, and the production efficiency is improved.

CN118737862APending Publication Date: 2024-10-01SHENZHEN ZHENHUA MICROELECTRONICS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310374201.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Intermetallic compounds and Kirkendall voids caused by heterogeneous metal contact in gold wire bonding systems affect bonding strength and reliability, resulting in reduced bonding strength and quality degradation.

Method used

The step preheating method is used to preheat and heat the metal to ensure that the metal surface is softened and heated evenly, reducing the occurrence time of purple spots and Kirkendall voids, and improving bonding strength and lifespan.

Benefits of technology

Through the step preheating method, the bonding strength and quality are improved, the bonding process time is shortened, the bonding life is extended, and the production efficiency is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118737862A_ABST
    Figure CN118737862A_ABST
Patent Text Reader

Abstract

The invention provides a method for enhancing thermal ultrasonic lead bonding strength, which comprises the following steps of: preheating a product, uniformly heating the product to a set preheating temperature, softening a metal surface to facilitate intermolecular bonding of a bonding interface, and promoting effective connection of two metals and diffusion and growth of a metal compound during subsequent bonding; the preheated product is subjected to bonding heating, so that the product is heated to the bonding temperature, an oxidation film on the metal surface is promoted to be broken, interpenetration between metal atoms during bonding is accelerated, and the connection strength between the gold ball and the substrate is improved; performing thermal ultrasonic bonding on the product heated to the bonding temperature; and testing the bonding strength of the bonded product. By adopting a step preheating mode for the metal, the bonding metal is uniformly heated in the preheating stage, the time of the bonding process is shortened, and the occurrence time of purple spots and Kickle cavities is reduced, so that the bonding strength is improved, the bonding quality is improved, and the service life is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of bonding control, and in particular to a method and system for enhancing the thermal ultrasonic wire bonding strength. Background Art

[0002] Research shows that heterogeneous metal contact is the root cause of many reliability problems in bonding systems, including the generation of intermetallic compounds, the appearance of Kirkendall voids, and the degradation of bonding quality due to pad contamination. Among them, intermetallic compounds are the product of chemical changes that occur when heterogeneous metals come into contact, and Kirkendall voids are a physical phenomenon in which atoms diffuse into each other and leave vacancies in situ. The two promote each other and become an important hidden danger that affects the reliability of bonding systems.

[0003] The gold wire bonding system will generate a small amount of intermetallic compounds at the beginning of the process. The appearance of a small amount of intermetallic compounds is a manifestation of the effective bonding of metal atoms, which can play a role in strengthening the bonding strength. However, there is a dynamic change process in the gold-aluminum bonding interface. With the effect of time and temperature, the compound first grows in thickness and expands laterally. Its composition has gradually become diversified, and there are many metal compounds such as Au4Al, Au5Al2 (white spots), Au2Al2, AuAl2 (purple spots), AuAl, etc. Among them, the "purple spots" have the characteristics of high conductivity, small thermal expansion coefficient and brittle quality. These compounds have different lattice constants, thermal expansion coefficients, and volume change rates during the formation process, and have low conductivity. Over time, the resistance of the heterogeneous metal junction will increase significantly and the bonding strength will decrease significantly. Summary of the invention

[0004] To solve the above problems, the present invention provides a method for enhancing the strength of thermal ultrasonic wire bonding, which reduces the occurrence time of purple spots and Kirkendall voids by adopting a step-by-step preheating method for the bonding metal, improves the bonding strength, and thus increases the bonding quality and life.

[0005] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0006] A method for enhancing the strength of thermosonic wire bonding, comprising the following steps:

[0007] Transfer the product to the preheating platform;

[0008] Preheat the product, heat the product evenly to the set preheating temperature, soften the metal surface to facilitate the intermolecular bonding at the bonding interface, promote the effective connection of the two metals during subsequent bonding, and promote the diffusion and growth of metal compounds;

[0009] Transfer the product to the bonding heating platform;

[0010] The preheated product is heated to the bonding temperature to break the oxide film on the metal surface, accelerate the thermal vibration of metal atoms, accelerate the mutual penetration between metal atoms during bonding, and improve the connection strength between the gold ball and the substrate;

[0011] Thermosonic bonding is performed on products heated to bonding temperature.

[0012] Furthermore, the preheating temperature ranges from 70°C to 90°C.

[0013] Furthermore, the preheating temperature is 80°C.

[0014] Furthermore, the bonding temperature is 100°C to 160°C.

[0015] Furthermore, the bonding temperature is 150°C.

[0016] Furthermore, the bonding metal includes Au and Ag.

[0017] Furthermore, when the products are transferred to the preheating platform, multiple products are placed on the preheating platform for preheating, and then moved to the bonding heating platform during production to reduce the waiting time for product preheating and effectively improve production efficiency.

[0018] Furthermore, the method also includes the following steps: before the product is preheated, the product is cleaned, inspected and processed to prevent the metal surface from absorbing impurities.

[0019] Furthermore, the method also includes the following steps: testing the bonding strength of the bonded product.

[0020] A thermosonic wire bonding system, which is used to implement the method for enhancing the thermosonic wire bonding strength as described above, comprising:

[0021] Cleaning module, which is used to clean, inspect and process the product to prevent the metal surface from absorbing impurities;

[0022] The first transfer module is used to transfer the product to the preheating platform;

[0023] The preheating platform is used to preheat the product, uniformly heat the product to the set preheating temperature, soften the metal surface to facilitate the intermolecular bonding of the bonding interface, promote the effective connection of the two metals during subsequent bonding, and promote the diffusion and growth of metal compounds;

[0024] The second transfer module is used to transfer the product to the bonding and heating platform;

[0025] The bonding heating platform is used to heat the preheated product to the bonding temperature, so as to promote the rupture of the oxide film on the metal surface, accelerate the thermal vibration of metal atoms, accelerate the mutual penetration between metal atoms during bonding, and improve the connection strength between the gold ball and the substrate;

[0026] A bonding module, which is used to perform thermosonic bonding on products heated to a bonding temperature;

[0027] The inspection module is used to inspect the bonding strength of the bonded product.

[0028] The temperature-induced internal stresses in the bonding interface may need to be taken into account, as these can severely limit the lifetime of the chip and the reliability of the bond.

[0029] The temperature at the bonding position also seriously affects the bonding strength and has a certain impact on the bondability of the system.

[0030] The present invention provides a method for enhancing the bonding strength of thermal ultrasonic wires, comprising the following steps: cleaning, inspecting and treating a product to prevent the metal surface from absorbing impurities; preheating the product to uniformly heat the product to a set preheating temperature to soften the metal surface to facilitate the intermolecular bonding at the bonding interface, promote the effective connection of the two metals during subsequent bonding, and promote the diffusion and growth of metal compounds; bonding heating the preheated product to heat the product to a bonding temperature to promote the rupture of an oxide film on the metal surface, accelerate the thermal vibration of metal atoms, accelerate the mutual penetration between metal atoms during bonding, and improve the connection strength between a gold ball and a substrate; performing thermal ultrasonic bonding on the product heated to the bonding temperature; and inspecting the bonding strength of the bonded product. By adopting a step preheating method for the metal, the bonding metal is heated evenly and the metal surface is softened in the preheating stage. In the bonding heating stage, it can not only be quickly heated to the bonding temperature, but also the temperature difference between the inside and outside of the metal and between each position is small during bonding, so the metal surface temperature decreases slowly during the bonding process, shortening the bonding process time, reducing the time for purple spots and Kirkendall voids to occur, thereby improving the bonding strength, increasing the bonding quality and life. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 The present invention is a schematic flow chart of a method for enhancing the strength of thermal ultrasonic wire bonding. DETAILED DESCRIPTION

[0032] The embodiments of the present disclosure are described in detail below with reference to the accompanying drawings.

[0033] The following describes the embodiments of the present disclosure through specific examples, and those skilled in the art can easily understand other advantages and effects of the present disclosure from the contents disclosed in this specification. Obviously, the described embodiments are only a part of the embodiments of the present disclosure, rather than all of the embodiments. The present disclosure can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present disclosure. It should be noted that the following embodiments and features in the embodiments can be combined with each other without conflict. Based on the embodiments in the present disclosure, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present disclosure.

[0034] Embodiment 1

[0035] The change of bonding temperature mainly comes from two aspects, one is the bonding temperature set before bonding, and the other is the heat released by the friction caused by ultrasonic vibration. The former is set within a certain range according to different bonding materials, and can generally be set as a fixed value based on experience or actual product verification. The temperature of ultrasonic bonding wire is generally set between 100-150℃, while the latter is determined by the ultrasonic energy.

[0036] Metals deform when heated. When the temperature field acts on the deformed body during plastic deformation, the deformed body expands due to heat and undergoes thermal deformation. The thermal strain formula for isotropic materials is as follows:

[0037]

[0038] In the formula, ε πj is the thermal strain component, α is the linear expansion system, and ΔΤ is the temperature change.

[0039] Wire bonding is highly dependent on temperature. Temperature not only affects the viscoplasticity during the wire bonding contact process, but also affects the diffusion of metal atoms and the formation of new metal phases between the bonding interfaces. The increase in temperature intensifies the activity of metal atoms and increases the metal activation energy of the bonding interface, which is conducive to the mutual fusion of the two. The temperature of the bonding position also seriously affects the bonding strength and has a certain impact on the bondability of the system. When the bonding process is unstable or the bonding fails, the ideal result can be achieved by adjusting this parameter. Temperature has a more significant effect than ultrasound. If the bonding temperature is too low or too high, the bonding cannot be completed or the bonding strength is significantly low. The higher the temperature, the lower the ultrasonic energy required to form the bond. Providing additional energy to the bonding position by heating usually leads to more robust processing (the robustness of the system, the system maintains certain performance characteristics under certain parameter fluctuations) and obtains a larger working window for wire bonding parameters. For thermal ultrasonic bonding, the higher the temperature, the faster the reaction rate and the shorter the time required. However, too high a bonding temperature will affect the material properties and soften the metal, resulting in reduced bonding strength and affecting other components and solder paste. The internal stress generated by temperature on the bonding interface may also be considered, as this seriously limits the chip's service life and bonding reliability.

[0040] like Figure 1 The figure shows a schematic flow chart of a method for enhancing the strength of thermosonic wire bonding, comprising the following steps:

[0041] Clean, inspect and treat the product to prevent the metal surface from absorbing impurities;

[0042] Preheat the product, heat the product evenly to the set preheating temperature, soften the metal surface to facilitate the intermolecular bonding at the bonding interface, promote the effective connection of the two metals during subsequent bonding, and promote the diffusion and growth of metal compounds;

[0043] The preheated product is heated to the bonding temperature to break the oxide film on the metal surface, accelerate the thermal vibration of metal atoms, accelerate the mutual penetration between metal atoms during bonding, and improve the connection strength between the gold ball and the substrate;

[0044] Performing thermosonic bonding on the product heated to the bonding temperature;

[0045] Test the bonding strength of the bonded products.

[0046] In a specific implementation, the preheating temperature ranges from 70°C to 90°C.

[0047] In a specific implementation, the bonding temperature is 100°C to 160°C.

[0048] In a specific implementation, the bonding metal includes Au and Ag.

[0049] Traditional gold wire bonding uses a method of direct heating to the bonding temperature. During automatic production, the bonding surface of the product cannot be quickly heated to the bonding temperature. Even if the bonding metal surface reaches the bonding temperature after a long waiting time, the product is always in a state of temperature change due to the fast heat dissipation rate of the metal shell of the product. The bonding process cools down quickly, and the temperature drop will prolong the bonding waiting time and slow down the production speed.

[0050] For gold wire bonding, research has shown that temperature has a more significant effect than ultrasonic energy. The higher the temperature, the lower the ultrasonic energy required to form a bond. Providing additional energy to the bonding position by heating usually leads to more robust processing and a larger working window for wire bonding parameters. During thermosonic bonding, temperature plays a crucial role. The bonding temperature between the gold pad and the aluminum metal layer during bonding affects the formation of the contact surface. In gold-aluminum bonding, thermosonic bonding shows a wider range of variation as it relies on ultrasonic energy, that is, the higher the bonding temperature, the lower the ultrasonic energy required to achieve the same bonding strength.

[0051] The heterogeneous metal contact of gold and aluminum bonding is the root cause of many reliability problems in the bonding system, including the generation of intermetallic compounds, the appearance of Kirkendall voids, and the reduction of bonding quality due to pad contamination. Among them, intermetallic compounds are the products of chemical changes when heterogeneous metals come into contact, and Kirkendall voids are a physical phenomenon in which atoms diffuse into each other and leave vacancies in situ. The two promote each other and become an important hidden danger affecting the reliability of the bonding system. A small amount of intermetallic compounds will be generated in the early stage of the process of gold wire bonding system. The appearance of a small amount of intermetallic compounds is a manifestation of the effective combination of metal atoms, which can play a role in strengthening the bonding strength. However, there is a dynamic change process in the gold-aluminum bonding interface. With the effect of time and temperature, the compound first grows in thickness and expands laterally. Its composition has gradually become diversified, and there are many metal compounds such as Au4Al, Au5Al2 (white spots), Au2Al2, AuAl2 (purple spots), and AuAl. These compounds have different lattice constants, thermal expansion coefficients, and volume change rates during the formation process, and have low electrical conductivity. As time goes by, the resistance of the joint will increase significantly and the bond strength will decrease significantly. According to experimental observations, with the increase of aging time, in addition to the generation of intermetallic compounds at the bonding interface, Kirkendall voids will also appear. Kirkendall voids are the product of the diffusion of two metal atoms into each other when heterogeneous metals are in contact. The original position of the diffused atoms is not filled by subsequent atoms, resulting in vacancies. It is a purely physical phenomenon.

[0052] Diffusion allows different atoms to fully contact and promotes the formation of intermetallic compounds. The formation of intermetallic compounds consumes diffusing atoms, increases the atomic concentration gradient, accelerates diffusion, and promotes the appearance of voids. As the number increases, the voids gather and eventually form cracks, causing the lead and the compound layer to separate, causing the bonding wire to fall off. The above results show that intermetallic compounds are formed during the bonding process, so there was once good contact between the bonding wire and the metallization layer of the chip bonding area, and the failure was not caused by cold soldering. This failure mode is an inevitable result of heterogeneous metal contact, but in the actual bonding process, the gold wire and the chip bonding area itself cannot achieve 100% effective contact, and the bonding temperature can effectively reduce the risk of bonding failure, and reliable temperature can produce stronger thermosonic bonding. The step preheating method preheats the product uniformly first. During production, it can not only quickly heat to the bonding temperature, but also effectively soften the bonding coating, reduce surface coating pollution, improve the viscosity and plasticity during the bonding contact process, reduce the temperature change during the bonding process, and increase the bonding speed. A good bonding temperature affects the diffusion of metal atoms in the initial bonding stage and the formation of new metal phases between the bonding interfaces, ensuring the composition of intermetallic compounds and reducing the excessive appearance of Kirkendall voids. The increase in temperature intensifies the activity of metal atoms and increases the metal activation energy of the bonding interface, which is conducive to the mutual fusion of the two and the improvement of the bonding strength. While improving the bonding speed and strength, it can also avoid using too high a bonding temperature to affect the performance of the material itself, soften the metal, reduce the bonding strength, and affect other components and solder paste.

[0053] Embodiment 2

[0054] In this embodiment, an American KNS bonding machine, equipment model ICoonPLUS, is used, and a 25μm gold wire is used to verify the effect of the invention. The bonding effects at 80°C, 120°C, 140°C, 150°C and 160°C are compared respectively, and then compared with the ladder preheating method. Under the condition of maintaining fixed bonding parameters such as power, time, pressure, and burning ball current time, the preheating temperature and bonding temperature are changed. The tension and shear force between the gold ball bump and the substrate are the main basis for judging the connection strength. The tension test is related to factors such as the position of the tension point, the lead length, and the tension angle. There is a certain degree of test randomness. Therefore, the lead length, tension position, tension angle and other factors need to be fixed during the test. The shear force test can avoid the above shortcomings and is conducive to the centralized analysis of the bonding characteristics of one or two welds. Therefore, in the experiment, the combined shear force of the gold ball and the substrate and the destructive bonding tension test are used as the judgment parameters of the connection strength. The bonding parameter table adopted is as follows Table 1:

[0055] Table 1

[0056]

[0057] In Test 1, direct heating to 80°C, 140°C, 150°C and 160°C was used as the bonding temperature. The strength effect comparison is shown in Table 2 below:

[0058] Table 2

[0059]

[0060] In Test 2, the effects of direct heating to 150°C and step preheating from 80 to 150°C were compared. The strength effect comparison is shown in Table 3:

[0061] Table 3

[0062]

[0063] In Test 3, the effects of 120-150°C preheating and 80-150°C step preheating were compared, as shown in Table 4:

[0064] Table 4

[0065]

[0066] In Test 4, the heating efficiency was compared between step preheating and single-stage heating. The comparison results are shown in Table 5 below:

[0067] Table 5

[0068] Heating platform Setting the temperature Time for the product to reach the required temperature Single stage heating 150℃±5℃ 10min Preheating 80℃±5℃ 4min Preheat first and then heat 150℃±5℃ 6min

[0069] Preheating allows the product to be placed on the preheating table for a longer time, softening the metal surface and facilitating the intermolecular bonding at the bonding interface. Preheating can heat the product more fully, and the substrate and chip can be heated more evenly, which can promote the effective connection of the two metals during bonding and the diffusion and growth of metal compounds (IMC). According to the results of the heating efficiency test, it takes 2 minutes for the product to rise from 80°C to 150°C. It takes 10 minutes to rise from room temperature to 150°C, so multiple products can be placed on the preheating platform for preheating, and then moved to the bonding heating platform during production to reduce the waiting time for product preheating, which can effectively improve production efficiency. Preheating first and then bonding heating, the total time is 6 minutes. Compared with only bonding heating, the time for a single product is saved by 4 minutes, and the production efficiency is increased by 40%.

[0070] The bonding of Au and Au and Ag metals on the substrate chip inevitably involves the problem of bonding strength between atoms. Since Ag is easily oxidized, its surface is usually covered with an oxide film or other impurity layer. If the bonding temperature is too low, impurities such as the oxide film layer on the metal surface cannot be removed. At the beginning of bonding, Au and Ag metals only have a few points of contact, and the number of contacts between metal atoms cannot be increased. Therefore, if the temperature is too low, the gold ball will not be able to bond with the substrate or the connection strength will be at a very low level. Therefore, it is required that the bonding metal surface cannot adsorb any gas and impurities during bonding.

[0071] The appropriate temperature range can promote the mutual diffusion of metal atoms and accelerate the speed of solid phase reaction. The formula for the diffusion coefficient of metal atoms is:

[0072]

[0073] Where D0 is the static diffusion coefficient and Q is the diffusion activation energy.

[0074] From the formula, we can see that increasing the temperature can accelerate the thermal vibration of metal atoms, making it easier for atoms to leave the equilibrium position and diffuse. In addition, increasing the temperature can soften the metal and accelerate the mutual penetration between metal atoms, thereby increasing the connection strength between the gold ball and the substrate. However, as the temperature increases, the elastic modulus and tensile strength of gold gradually decrease.

[0075] The preheating process before gold wire bonding can make the product reach the bonding temperature faster, reduce the operation time, and make the heat transfer of the product substrate more uniform. Sufficient preheating of the product can increase the product production process parameter window, optimize the bonding parameters and improve product stability. Insufficient preheating will cause the product to fail to reach the optimal bonding temperature, uneven heat transfer of the substrate, resulting in non-stick bonding problems, thereby reducing the bonding strength. In addition, the temperature of the bonding position also seriously affects the bonding strength and has a certain impact on the bondability of the system.

[0076] Embodiment 3

[0077] A thermosonic wire bonding system, which is used to implement the method for enhancing the thermosonic wire bonding strength as described above, comprising:

[0078] Cleaning module, which is used to clean, inspect and process the product to prevent the metal surface from absorbing impurities;

[0079] The first transfer module is used to transfer the product to the preheating platform;

[0080] The preheating platform is used to preheat the product, uniformly heat the product to the set preheating temperature, soften the metal surface to facilitate the intermolecular bonding of the bonding interface, promote the effective connection of the two metals during subsequent bonding, and promote the diffusion and growth of metal compounds;

[0081] The second transfer module is used to transfer the product to the bonding and heating platform;

[0082] The bonding heating platform is used to heat the preheated product to the bonding temperature, so as to promote the rupture of the oxide film on the metal surface, accelerate the thermal vibration of metal atoms, accelerate the mutual penetration between metal atoms during bonding, and improve the connection strength between the gold ball and the substrate;

[0083] A bonding module, which is used to perform thermosonic bonding on products heated to a bonding temperature;

[0084] The inspection module is used to inspect the bonding strength of the bonded product.

[0085] The temperature-induced internal stresses in the bonding interface may need to be taken into account, as these can severely limit the lifetime of the chip and the reliability of the bond.

[0086] The present invention provides a method for enhancing the bonding strength of thermal ultrasonic wires, comprising the following steps: cleaning, inspecting and treating a product to prevent the metal surface from absorbing impurities; preheating the product to uniformly heat the product to a set preheating temperature to soften the metal surface to facilitate the intermolecular bonding at the bonding interface, promote the effective connection of the two metals during subsequent bonding, and promote the diffusion and growth of metal compounds; bonding heating the preheated product to heat the product to a bonding temperature to promote the rupture of an oxide film on the metal surface, accelerate the thermal vibration of metal atoms, accelerate the mutual penetration between metal atoms during bonding, and improve the connection strength between a gold ball and a substrate; performing thermal ultrasonic bonding on the product heated to the bonding temperature; and inspecting the bonding strength of the bonded product. By adopting a step preheating method for the metal, the bonding metal is heated evenly and the metal surface is softened in the preheating stage. In the bonding heating stage, it can not only be quickly heated to the bonding temperature, but also the temperature difference between the inside and outside of the metal is small during bonding, and the metal surface temperature decreases slowly during the bonding process, shortening the bonding process time, reducing the time for purple spots and Kirkendall voids to occur, thereby improving the bonding strength, increasing the bonding quality and life.

[0087] In the description of the present invention, it is necessary to understand that the terms "middle", "length", "up", "down", "front", "back", "vertical", "horizontal", "inside", "outside", "radial", "circumferential" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention.

[0088] In the present invention, unless otherwise clearly specified and limited, the first feature "on" the second feature may be that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. "Multiple" means at least two, such as two, three, etc., unless otherwise clearly and specifically limited.

[0089] In the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral one; it can be a mechanical connection, an electrical connection, or communication with each other; it can be a direct connection, or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0090] The above is only for explaining the implementation mode of the present invention and is not intended to limit the present invention. For those skilled in the art, any modification, equivalent substitution, improvement, etc. made within the spirit and principle of the present invention without creative work should be included in the protection scope of the present invention.

Claims

1. A method for enhancing the strength of thermosonic wire bonding, characterized in that: The following steps are involved: Transfer the product to the preheating platform; Preheat the product, heat the product evenly to the set preheating temperature, soften the metal surface to facilitate the intermolecular bonding at the bonding interface, promote the effective connection of the two metals during subsequent bonding, and promote the diffusion and growth of metal compounds; Transfer the product to the bonding heating platform; The preheated product is heated to the bonding temperature to break the oxide film on the metal surface, accelerate the thermal vibration of metal atoms, accelerate the mutual penetration between metal atoms during bonding, and improve the connection strength between the gold ball and the substrate; Thermosonic bonding is performed on products heated to bonding temperature.

2. The method for enhancing the thermal ultrasonic wire bonding strength according to claim 1, characterized in that: The preheating temperature ranges from 70°C to 90°C.

3. The method for enhancing the thermal ultrasonic wire bonding strength according to claim 2, characterized in that: The preheating temperature is 80°C.

4. The method for enhancing the thermal ultrasonic wire bonding strength according to claim 1, characterized in that: The bonding temperature is 100°C to 160°C.

5. The method for enhancing the thermal ultrasonic wire bonding strength according to claim 4, characterized in that: The bonding temperature is 150°C.

6. The method for enhancing the thermal ultrasonic wire bonding strength according to claim 1, characterized in that: The bonding metals include Au and Ag.

7. The method for enhancing the thermosonic wire bonding strength according to claim 1, characterized in that: When the products are transferred to the preheating platform, multiple products are placed on the preheating platform for preheating, and then moved to the bonding heating platform during production to reduce the waiting time for product preheating and effectively improve production efficiency.

8. The method for enhancing the thermosonic wire bonding strength according to claim 1, characterized in that: The following steps are also included: Before preheating the product, clean, inspect and treat the product to prevent impurities from being adsorbed on the metal surface.

9. The method for enhancing the thermosonic wire bonding strength according to claim 1, characterized in that: The following steps are also included: Test the bonding strength of the bonded products.

10. A thermosonic wire bonding system, characterized in that: The method for implementing the method for enhancing the thermal ultrasonic wire bonding strength according to any one of claims 1 to 9 comprises: The first transfer module is used to transfer the product to the preheating platform; The preheating platform is used to preheat the product, uniformly heat the product to the set preheating temperature, soften the metal surface to facilitate the intermolecular bonding of the bonding interface, promote the effective connection of the two metals during subsequent bonding, and promote the diffusion and growth of metal compounds; The second transfer module is used to transfer the product to the bonding and heating platform; The bonding heating platform is used to heat the preheated product to the bonding temperature, so as to promote the rupture of the oxide film on the metal surface, accelerate the thermal vibration of metal atoms, accelerate the mutual penetration between metal atoms during bonding, and improve the connection strength between the gold ball and the substrate; The bonding module is used to perform thermosonic bonding on products heated to a bonding temperature.