Lithium iron phosphate positive pole piece, preparation method of lithium iron phosphate positive pole piece, lithium ion battery and electric equipment

By optimizing the material formula and preparation process of the lithium iron phosphate cathode plate, increasing the area density and compaction density, forming a good conductive network, solving the battery cycle performance and internal resistance problems, and improving the electrochemical performance and rate performance of the battery.

CN118738283APending Publication Date: 2024-10-01GREE ALTAIRNANO NEW ENERGY INC
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410849154.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

When increasing the areal density and compacted density of existing lithium iron phosphate cathode sheets, it is difficult to balance the cycle performance and internal resistance of the battery, and the compacted density cannot be further improved due to material properties and technical reasons, affecting the electrochemistry of the battery. performance.

Method used

Using cathode materials including lithium iron phosphate, binder, conductive agent, single-walled carbon nanotubes and multi-walled carbon nanotubes, the cathode slurry is prepared by wet stirring and rolled into pole sheets, increasing the area density to 420-430g /cm2 and compacted density to 2.55g/cm3 to form a good three-dimensional conductive network and optimize the material formula to improve battery performance.

Benefits of technology

It achieves excellent electrochemical performance under high surface density and compacted density, reduces resistivity and internal stress, improves the rate charge and discharge capacity retention rate and first-efficiency performance of the battery, and avoids the problem of pole piece brittleness and fragmentation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004916395340000011
    Figure HDA0004916395340000011
  • Figure HDA0004916395340000012
    Figure HDA0004916395340000012
  • Figure HDA0004916395340000021
    Figure HDA0004916395340000021
Patent Text Reader

Abstract

The invention relates to the field of lithium ion batteries, and discloses a lithium iron phosphate positive pole piece, a preparation method of the lithium iron phosphate positive pole piece, a lithium ion battery and electric equipment. The positive pole piece comprises a current collector and a positive pole material coated on the current collector, the positive electrode material comprises lithium iron phosphate, a binder, a conductive agent, a single-walled carbon nanotube, a multi-walled carbon nanotube and graphene; the surface density of the positive pole piece is 420-430 g / cm < 2 >, and the compaction density is 2.55 g / cm < 3 >. The positive pole piece disclosed by the invention has relatively high surface density, and the compaction density of the lithium iron phosphate positive pole piece is improved to a limit value range by optimizing the formula composition of the positive pole material, so that lithium iron phosphate particles can be effectively connected to form a good three-dimensional conductive network, and the battery not only keeps excellent electrochemical performance, but also has good electrochemical performance. And the flexibility of the pole piece can be improved, the internal stress of the pole piece is reduced, and the problems of brittleness, breakage and the like of the pole piece are prevented.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of lithium-ion batteries, and in particular to a lithium iron phosphate positive electrode sheet and a preparation method thereof, as well as a lithium-ion battery and electrical equipment. Background Art

[0002] Lithium-ion batteries have the advantages of high operating voltage, high specific energy, and long cycle life, and are widely used in mobile communications, laptops, electric vehicles, etc. Lithium-ion batteries are mainly composed of electrode plates, diaphragms, electrolytes, and battery shells. The performance of the battery is not only related to the performance of the electrode materials used, but also to the design parameters of the entire electrode, such as surface density and compaction density.

[0003] The internal resistance of the battery usually decreases with the increase of the surface density. Increasing the electrode surface density within a certain range will reduce the internal resistance of the battery; however, as the surface density increases, the cycle performance of the battery will decrease. Therefore, while increasing the electrode surface density, increasing the content of the binder in the positive electrode or increasing the compaction density of the positive electrode can improve the cycle performance of the battery. The compaction density depends on many factors such as the active material and the slurry formula. Due to the limitation of the lithium iron phosphate active material, the compaction density of the lithium iron phosphate positive electrode sheet has an upper limit, which is generally 2.55-2.65g / cm 3 Currently, lithium iron phosphate batteries on the market have low surface density (<320g / cm 2 ) can reach 2.65g / cm 3 The ultimate compaction is 360g / cm 2 The left and right surface density can generally reach 2.5g / cm 3 Compacted, but >400g / cm 2 The compacted density of the surface density is generally 2.45g / cm 3 The following is limited by the current objective technical reasons and cannot be further improved; under the premise of a certain surface density, the smaller the compaction density, the thicker the electrode will be, the higher the resistivity will be, which is not conducive to ion migration, and the porosity is also high, which may produce large closed pores, which is even more detrimental to the performance of the battery.

[0004] Increasing the compaction density of lithium iron phosphate positive electrode sheets can not only increase the energy density (under the premise that the cell volume remains unchanged), but also improve the negative impact caused by the high surface density. However, at the same time, the greater the compaction density, the greater the degree of squeezing between the active material particles, the smaller the porosity of the electrode sheet, and the more difficult it will be for the electrolyte to penetrate, which is not conducive to the utilization of gram capacity. The polarization during the battery cycle will also become larger, which is not conducive to high-rate charging and discharging. Therefore, how to comprehensively improve the electrochemical performance of lithium iron phosphate is an issue that needs attention. Summary of the invention

[0005] In view of this, the purpose of the present application is to provide a lithium iron phosphate positive electrode sheet and a preparation method thereof, so that the lithium iron phosphate positive electrode sheet can improve the electrochemical performance of lithium ion batteries under the premise of higher surface density and compaction density;

[0006] Another object of the present application is to provide a lithium-ion battery and electrical equipment prepared based on the above-mentioned positive electrode sheet.

[0007] In order to solve the above technical problems / achieve the above purposes or at least partially solve the above technical problems / achieve the above purposes, as a first aspect of the present application, a lithium iron phosphate positive electrode sheet is provided, comprising a current collector and a positive electrode material coated on the current collector; the positive electrode material comprises lithium iron phosphate, a binder, a conductive agent, single-walled carbon nanotubes, multi-walled carbon nanotubes and graphene; the surface density of the positive electrode sheet is 420-430 g / cm 2 , compacted density is 2.55g / cm 3 .

[0008] Optionally, the D50 of the lithium iron phosphate is 0.6-1.5 μm, D90≤5 μm, the length of the single-walled carbon nanotube is 5-30 μm, and the length of the multi-walled carbon nanotube is 10-30 μm.

[0009] Optionally, the positive electrode material includes 93-97% lithium iron phosphate, 1-5% binder, 0.1-1% conductive agent, 0.4-0.9% single-walled carbon nanotubes, 0.1-0.3% multi-walled carbon nanotubes and 0.1-0.3% graphene.

[0010] As a second aspect of the present application, a method for preparing the lithium iron phosphate positive electrode sheet is provided, comprising:

[0011] Lithium iron phosphate, a binder, a conductive agent, single-walled carbon nanotubes, multi-walled carbon nanotubes and graphene are mixed in proportion by wet stirring to prepare a lithium iron phosphate positive electrode slurry. The positive electrode slurry is coated on a current collector, dried, and then rolled to obtain the lithium iron phosphate positive electrode sheet.

[0012] As a third aspect of the present application, a lithium-ion battery is provided, comprising the lithium iron phosphate positive electrode plate described in the present application, as well as a separator, an electrolyte and a negative electrode plate.

[0013] Optionally, the N / P ratio of the negative electrode plate is 1.2. Further optionally, the active material of the negative electrode plate is a graphite material.

[0014] As a fourth aspect of the present application, there is provided an electrical device, comprising the lithium-ion battery described in the present application, wherein the lithium-ion battery provides electrical energy for the electrical device.

[0015] The positive electrode plate described in the present application has a high surface density, and by optimizing the formula composition of the positive electrode material, the compaction density of the lithium iron phosphate positive electrode plate is increased to its limit value range, which can effectively connect the lithium iron phosphate particles to form a good three-dimensional conductive network, so that the battery not only maintains excellent electrochemical properties, but also can improve the softness of the plate, reduce the internal stress of the plate, and prevent the plate from brittleness, breakage and other problems. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] The drawings constituting a part of the present application are used to provide a further understanding of the present application. The illustrative embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application.

[0017] Figure 1 The figure shows the comparative results of the resistivity of the LFP positive electrode sheets after rolling of Example 1 and the comparative examples;

[0018] Figure 2 Shown are the first effect comparison results of the soft-pack batteries of Example 1 and various comparative examples;

[0019] Figure 3 The figure shows the comparison results of the DC internal resistance of the soft-pack batteries of Example 1 and each comparative example during charging and discharging;

[0020] Figure 4 The figure shows the comparison results of the rate charging capacity retention rate of the soft-pack battery of Example 1 and each comparative example;

[0021] Figure 5 Shown are the comparison results of the rate discharge capacity retention rate of the soft-pack batteries of Example 1 and various comparative examples. DETAILED DESCRIPTION

[0022] The present application discloses a lithium iron phosphate positive electrode plate and a preparation method thereof, as well as a lithium-ion battery and an electrical device. Those skilled in the art can refer to the content of this article and appropriately improve the process parameters to achieve it. It is particularly important to point out that all similar replacements and modifications are obvious to those skilled in the art, and they are all deemed to be included in this application. The products, processes and applications described in this application have been described through preferred embodiments. Relevant personnel can obviously modify or appropriately change and combine the preparation methods described herein without departing from the content, spirit and scope of this application to realize and apply the technology of this application. Obviously, the described embodiments are part of the embodiments of this application, not all of them. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.

[0023] It should be noted that, in this article, if relational terms such as "first" and "second", "step 1" and "step 2", and "(1)" and "(2)" appear, they are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "comprise", "include" or any other variants thereof are intended to cover non-exclusive inclusion, so that the process, method, article or equipment including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or equipment. In the absence of further restrictions, the elements defined by the sentence "comprise one..." do not exclude the presence of other identical elements in the process, method, article or equipment including the elements. At the same time, the embodiments in this application and the features in the embodiments may be combined with each other without conflict.

[0024] If the compaction density is too small, the distance between particles is large, there are many ion channels, and the electrolyte absorption is large, which is conducive to ion movement. However, due to the small contact area between particles, it is not conducive to electronic conduction, and the discharge polarization increases; within a certain extent, as the compaction density increases, the distance between raw material particles decreases, the contact area increases, the conductive channels and bridges increase, and the active area that can participate in the reaction increases, thereby increasing the specific capacity of the battery. Therefore, the present invention improves the capacity retention rate and first efficiency of the battery under high-rate charge and discharge, and reduces the resistivity and DC internal resistance by increasing the compaction density of the pole piece.

[0025] In addition, the positive electrode surface density of the present application is 420-430g / cm 2 For a pole piece with a larger surface density, if the compaction is low, the pole piece will be thicker, which will make the migration path of lithium ions longer and the internal resistance of the battery larger. Congestion is likely to occur on the migration path of lithium ions, which will cause the lithium ions to be unable to be completely deintercalated in a short time, and finally lead to a loss of specific capacity. For high-rate charging and discharging, the pole piece is required to be able to achieve rapid ion extraction and embedding. Therefore, under high surface density, the improvement of compaction density is very important for improving battery electrical performance. However, due to the properties of lithium iron phosphate materials and current technical means, the compaction density of lithium iron phosphate positive pole pieces under high surface density is generally 2.4g / cm 3 About, >2.5g / cm 3 It is a relatively high compaction density, which is particularly difficult to improve for high surface density lithium iron phosphate (LFP) electrodes.

[0026] Therefore, in the first aspect of the present application, by optimizing the composition of the positive electrode sheet material, a lithium iron phosphate positive electrode sheet is provided, comprising a current collector and a positive electrode material coated on the current collector; the positive electrode material comprises lithium iron phosphate, a binder, a conductive agent, single-walled carbon nanotubes (SWCNT), multi-walled carbon nanotubes (MWCNT) and graphene; the surface density of the positive electrode sheet is 420-430 g / cm 2 , compacted density is 2.55g / cm 3 .

[0027] In certain embodiments of the present application, the D50 of the lithium iron phosphate is 0.6-1.5 μm, D90 ≤ 5 μm, the length of the single-walled carbon nanotube is 5-30 μm, and the length of the multi-walled carbon nanotube is 10-30 μm. The particle size distribution requirements of the present application for lithium iron phosphate can make it have a good particle grading, so that the particles will not break under high compaction, overpressure will not occur, and the positive electrode sheet has a suitable porosity. In addition, electrodes with high compaction density have higher fracture strength, thereby avoiding the fall of electrode particles during the cycle and forming insulating particles. Suitable LFP particle size and positive electrode material can ensure that the distribution of the pore size and pores of the electrode under high compaction density is more uniform, and the distribution of the conductive agent and binder is more uniform, thereby reducing the contact resistance and charge transfer impedance of the electrode.

[0028] The requirement for SWCNT length is based on the consideration that the thickness of the positive electrode sheet is certain under a certain surface density and compaction density, and SWCNT forms a continuous conductive network on the particle surface, which requires SWCNT to have a suitable length. It should be noted that the longer the SWCNT is (>50μm) and the higher the aspect ratio (>3000), the better the electrochemical performance of the battery may be. However, considering the cost reasons, the present application can achieve good electrochemical performance when the SWCNT is 5-30μm, and the cost-effectiveness of improving the electrochemical performance by using better SWCNT is not high.

[0029] In certain embodiments of the present application, the positive electrode material includes 93-97% lithium iron phosphate, 1-5% binder, 0.1-1% conductive agent, 0.4-0.9% single-walled carbon nanotubes, 0.1-0.3% multi-walled carbon nanotubes and 0.1-0.3% graphene. In other embodiments of the present application, the positive electrode material includes 96.5% lithium iron phosphate, 2% binder, 0.5% conductive agent, 0.8% single-walled carbon nanotubes, 0.1% multi-walled carbon nanotubes and 0.1% graphene.

[0030] In certain embodiments of the present application, the binder includes but is not limited to polyvinylidene fluoride (PVDF), polyvinyl alcohol (PVA), styrene-butadiene rubber (SBR), polyolefins (PP, PE, etc.), sodium carboxymethyl cellulose (CMC), polytetrafluoroethylene (PTFE), fluorinated rubber, polyurethane, etc.; the conductive agent is selected from conductive carbon black SP, Ketjen black, graphite, etc.; the current collector includes metal foil, such as aluminum foil, copper foil, etc.

[0031] In a second aspect of the present application, a method for preparing the lithium iron phosphate positive electrode sheet is provided, comprising:

[0032] Lithium iron phosphate, a binder, a conductive agent, single-walled carbon nanotubes, multi-walled carbon nanotubes and graphene are mixed in proportion by wet stirring to prepare a lithium iron phosphate positive electrode slurry. The positive electrode slurry is coated on a current collector, dried, and then rolled to obtain the lithium iron phosphate positive electrode sheet.

[0033] In certain embodiments of the present application, the rolling conditions include a pressure of 80 MPa, a rolling speed of 20 m / min, and room temperature.

[0034] In a third aspect of the present application, a lithium-ion battery is provided, comprising the lithium iron phosphate positive electrode plate described in the present application, as well as a separator, an electrolyte and a negative electrode plate.

[0035] In certain embodiments of the present application, the N / P ratio of the negative electrode plate is 1.2. Since the negative electrode needs to continuously consume lithium ions from the initial formation of the SEI film to the repair of the SEI during the cycle, in order to meet the requirements of long-term cycling of the battery at a high rate, the N / P ratio of the negative electrode design is 1.2.

[0036] In certain embodiments of the present application, the active material of the negative electrode plate is a graphite material, such as natural graphite, artificial graphite, etc. The negative electrode plate can be prepared by referring to the preparation method of the lithium iron phosphate positive electrode plate, and the graphite material, the conductive agent and the binder are mixed in a certain proportion, such as 92% to 98%, 1% to 5%, 1% to 5%, by wet stirring to form a negative electrode slurry, and then coated on the current collector, dried, and rolled to form a negative electrode plate. The electrolyte can be a lithium hexafluorophosphate electrolyte.

[0037] In a fourth aspect of the present application, an electric device is provided, comprising the lithium-ion battery described in the present application, wherein the lithium-ion battery provides electric energy for the electric device. The electric device may be various devices or equipment driven by the lithium-ion battery, including but not limited to electric vehicles, electric vehicles, self-balancing vehicles, flatbed vehicles, aircraft, lighting equipment, household appliances, etc.

[0038] In this application, graphene, single-walled carbon nanotubes and multi-walled carbon nanotubes are introduced to improve the conductivity of lithium iron phosphate pole pieces; SWCNT is used as one of the components of the positive electrode material, on the one hand to build a better conductive network, on the other hand to improve the compaction density of the LFP pole piece (from the conventional 2.4g / cm 3 Increase to 2.55g / cm 3 , the surface density is 420-430g / cm 2 ), further reducing the resistivity of the LFP pole piece. The compaction density affects the internal resistance of the battery and is closely related to the battery cycle and rate performance. The appropriate compaction density can reduce the internal resistance and polarization loss without affecting the insertion and extraction of lithium ions. In addition, in order to reduce the impact of high compaction density, the present invention adds graphene and MWCNT at the same time, thereby balancing the battery performance in all aspects to achieve the best state.

[0039] In each group of comparative experiments provided in this application, unless otherwise specified, other experimental conditions, materials, etc. are kept consistent except for the differences indicated in each group, so as to provide comparability. The experimental materials and reagents used in the examples can be obtained from commercial channels unless otherwise specified.

[0040] The following is a further description of a lithium iron phosphate positive electrode plate and a preparation method thereof, as well as a lithium-ion battery and electrical equipment provided in the present application.

[0041] Embodiment 1:

[0042] Positive electrode slurry: Lithium iron phosphate positive electrode slurry was prepared by wet stirring according to 96.5% lithium iron phosphate, 2% PVDF, 0.5% SP, 0.8% single-walled carbon nanotubes, 0.1% multi-walled carbon nanotubes and 0.1% graphene.

[0043] Negative electrode slurry: Graphite negative electrode slurry was prepared by wet stirring according to 96.3% graphite, 1% SP, 1.2% CMC and 1.5% SBR.

[0044] First, deionized water and a binder are stirred at high speed to prepare a glue solution; then other components except the main material are added to the glue solution and stirred at high speed; then lithium iron phosphate or graphite main material is added and stirred at high speed, and finally positive and negative electrode slurries with qualified viscosity and solid content are prepared, which are coated and dried on the current collector, and rolled at room temperature with a pressure of 80MPa and a rolling speed of 20m / min to achieve the target surface density (420g / cm 2 ) and compacted density (2.55g / cm 3 ) to obtain the positive electrode sheet and the negative electrode sheet (the N / P ratio of the electrode sheet is 1.2), and then assemble them into a lithium-ion battery with the separator and electrolyte according to the assembly process of the soft-pack battery.

[0045] Comparative Example 1:

[0046] The electrode sheet and battery were prepared according to the method of Example 1, except that the positive electrode slurry was 96.5% lithium iron phosphate, 2% PVDF, and 1.5% SP. After preparation, the positive electrode sheet could only reach 2.4g / cm 3 compacted density.

[0047] Comparative Example 2:

[0048] The electrode sheet and battery were prepared according to the method of Example 1, except that the positive electrode slurry was 96.5% lithium iron phosphate, 2% PVDF, 0.5% SP, and 1.0% single-walled carbon nanotubes. After preparation, the positive electrode sheet can reach 2.55g / cm 3 compacted density.

[0049] Comparative Example 3:

[0050] The electrode sheet and battery were prepared according to the method of Example 1, except that the positive electrode slurry was 96.5% lithium iron phosphate, 2% PVDF, 0.5% SP, and 1.0% single-walled carbon nanotubes, and the target compaction density was adjusted to 2.50 g / cm 3 After preparation, the positive electrode sheet can reach 2.50g / cm 3 compacted density.

[0051] Comparative Example 4:

[0052] The electrode sheet and battery were prepared according to the method of Example 1, except that the positive electrode slurry was 96.5% lithium iron phosphate, 2% PVDF, 0.5% SP, and 1.0% single-walled carbon nanotubes, and the target compaction density was adjusted to 2.45 g / cm 3 After preparation, the positive electrode sheet can reach 2.45g / cm 3 compacted density.

[0053] Experimental example:

[0054] The resistivity, initial efficiency, charge and discharge DC internal resistance, and rate charge and discharge capacity retention rate of Example 1 and each comparative example were tested;

[0055] (1) Figure 1 The figure shows the resistivity of the LFP pole piece after rolling. The average resistivity of Comparative Example 1, Comparative Example 2, Example 1, Comparative Example 3, and Comparative Example 4 are 9.721Ω·cm, 7.378Ω·cm, 6.527Ω·cm, 6.910Ω·cm, and 7.900Ω·cm, respectively. It can be clearly seen that although Comparative Example 2 can reach 2.55g / cm under the premise of the same high surface density, 3The compaction density of the comparative example 3 was adjusted to 2.50 g / cm 3 , compared with Comparative Examples 2 and 4, its resistivity is lower, but still inferior to Example 1;

[0056] (2) Figure 2 The comparison results of the first efficiency of each group of batteries are shown; although the surface density of Example 1 and Comparative Example 2 both reached 2.55g / cm 3 However, since Comparative Example 2 does not have additional multi-walled carbon nanotubes and graphene, some negative effects occur at high compaction density, and the first efficiency is low, while Example 1 is not affected by the high compaction density and still maintains the highest first efficiency among all treatment groups;

[0057] (3) Figure 3 The figure shows the comparison results of the DC internal resistance during charge and discharge. It can be seen intuitively from the results in the figure that the charge and discharge internal resistance of Example 1 is still low, and the internal resistance of the other groups is high. The comparison with Comparative Example 2 shows that the higher compaction density will objectively be unfavorable to the battery performance without the addition of multi-walled carbon nanotubes and graphene.

[0058] (4) Figure 4 and Figure 5 The figure shows the comparison results of the capacity retention rate of charge and discharge at multiple rates; Figure 4 and Figure 5 It can be seen that, whether it is the charge capacity retention rate or the discharge capacity retention rate, Example 1 is at a higher level than the comparative examples, which indicates that the positive electrode plate of the present application can ensure that under the premise of higher surface density and compaction density (which is beneficial to the battery capacity density), it can still maintain better rate performance.

[0059] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.

Claims

1. A lithium iron phosphate positive electrode plate, characterized in that: The invention comprises a current collector and a positive electrode material coated on the current collector; the positive electrode material comprises lithium iron phosphate, a binder, a conductive agent, single-walled carbon nanotubes, multi-walled carbon nanotubes and graphene; the surface density of the positive electrode sheet is 420-430 g / cm 2 , compacted density is 2.55g / cm 3 .

2. The lithium iron phosphate positive electrode sheet according to claim 1, characterized in that: The D50 of the lithium iron phosphate is 0.6-1.5 μm, and the D90 is ≤5 μm. The length of the single-walled carbon nanotube is 5-30 μm, and the length of the multi-walled carbon nanotube is 10-30 μm.

3. The lithium iron phosphate positive electrode sheet according to claim 1, characterized in that: The positive electrode material comprises 93-97% lithium iron phosphate, 1-5% binder, 0.1-1% conductive agent, 0.4-0.9% single-walled carbon nanotube, 0.1-0.3% multi-walled carbon nanotube and 0.1-0.3% graphene.

4. The method for preparing a lithium iron phosphate positive electrode sheet according to claim 1, characterized in that: include: Lithium iron phosphate, a binder, a conductive agent, single-walled carbon nanotubes, multi-walled carbon nanotubes and graphene are mixed in proportion by wet stirring to prepare a lithium iron phosphate positive electrode slurry. The positive electrode slurry is coated on a current collector, dried, and then rolled to obtain the lithium iron phosphate positive electrode sheet.

5. A lithium ion battery, characterized in that: It comprises the lithium iron phosphate positive electrode sheet as described in any one of claims 1 to 3, as well as a diaphragm, an electrolyte and a negative electrode sheet.

6. The lithium-ion battery according to claim 5, characterized in that: The N / P ratio of the negative electrode plate is 1.

2.

7. The lithium ion battery according to claim 5 or 6, characterized in that: The active material of the negative electrode plate is a graphite material.

8. An electrical device, characterized in that: The lithium-ion battery comprises the lithium-ion battery according to any one of claims 5 to 7, wherein the lithium-ion battery provides electrical energy for the electrical equipment.

Citation Information

Cited By

  • Composite positive electrode conductive paste and preparation method thereof

    CN120914257A

  • Composite positive electrode conductive paste and preparation method thereof

    CN120914257B