Modified manganese dioxide positive electrode material, preparation method thereof and aqueous zinc ion battery
Hydrated manganese dioxide nanosheets with a flower-shaped structure were synthesized at room temperature through a microwave-assisted precipitation method, and alkali metal and alkaline earth metal ions were introduced to solve the problems of high temperature, high pressure and strong oxidants in the existing technology, and achieve high efficiency and low cost. Manganese oxide synthesis improves the performance and stability of zinc-ion batteries.
Patent Information
- Application Number
- CN202410925474.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-10
AI Technical Summary
Existing synthesis methods of manganese dioxide cathode materials require high temperature and high pressure conditions or the use of strong oxidants, resulting in high energy consumption, serious waste of resources, and are not suitable for industrial production. Moreover, electrodeposition technology consumes a large amount of electricity and raw materials, and the synthesis cost is high.
The microwave-assisted precipitation method is used to synthesize hydrated manganese dioxide nanosheets with a spherical structure at room temperature. Alkali metal and alkaline earth metal ions are introduced through alkali precipitants and solution impregnation methods to form a stable layered structure and improve conductivity and capacity. And maintain structural stability through ion exchange.
It achieves low energy consumption and safe synthesis of manganese dioxide, improves the specific capacity, cycle stability and rate performance of zinc-ion batteries, reduces production costs, and is suitable for large-scale industrial production.
Smart Images

Figure CN118738362A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of new energy, and specifically relates to a modified manganese dioxide positive electrode material and a preparation method thereof, and an aqueous zinc ion battery. Background Art
[0002] With the rapid development of clean energy transformation and the goal of building a carbon-neutral economy, people are in urgent need of high-performance electrochemical devices to achieve large-scale energy storage. These devices need to be safe, environmentally friendly, low-cost and have long cycle life. Aqueous zinc-ion batteries (AZIBs) use aqueous electrolytes and zinc metal negative electrodes. They have the advantages of high safety, environmental friendliness and high ionic conductivity, and are considered to be one of the most promising choices for energy storage power stations. In recent years, a variety of positive electrode materials have been explored for use in AZIBs, such as transition metal-based compounds, Prussian blue analogs and organic materials. Among them, manganese dioxide, as a very promising positive electrode material, has the advantages of environmental friendliness, high theoretical capacity, low cost and high voltage platform, so it has been widely studied.
[0003] At present, most of the synthesis methods of manganese dioxide positive electrode materials used in industrial production require high temperature calcination, high temperature and high pressure conditions, or use electrolysis. The above methods have problems such as high energy consumption, unsuitability for process production, and serious waste of resources. The remaining methods such as sol-gel method and electrodeposition method are not suitable for large-scale synthesis and are not suitable for industrial production. In addition, the raw materials for synthesizing manganese dioxide mostly involve strong oxidants, such as potassium permanganate, hydrogen peroxide, ammonium persulfate, etc. The introduction of strong oxidants poses a challenge to the safety of equipment for large-scale industrial production.
[0004] Prior art CN103086437A uses manganese sulfate and ammonium bicarbonate as raw materials to prepare manganese carbonate, and then continuously roasts manganese carbonate at 350°C to 380°C to prepare manganese dioxide. This method requires high-temperature roasting treatment, which generates large energy consumption, and it is very easy to produce other manganese oxide impurities when pyrolyzing manganese carbonate to produce manganese dioxide, which affects the performance of the positive electrode material. Prior art CN1 17089857A discloses a method for preparing manganese dioxide positive electrode material by electrodeposition, which uses manganese sulfate solution and sulfuric acid solution as electrolytes, and deposits manganese dioxide on carbon paper by constant potential method or cyclic voltammetry through a three-electrode system. This technology has reaction controllability, and a variety of manganese dioxide positive electrodes with different morphologies can be prepared by adjusting different deposition potentials or scan rates. However, the electrodeposition technology consumes a lot of electricity, causes a lot of raw material waste, and requires special equipment, and the synthesis cost is high.
[0005] Therefore, it is crucial to find a high-performance manganese dioxide synthesis method that meets the requirements of low energy consumption in the preparation process, safe raw materials and no strong oxidants, which is of great significance for promoting the further application of aqueous zinc-ion batteries. Summary of the invention
[0006] In order to solve all or part of the above technical problems, the present invention provides the following technical solutions:
[0007] One of the purposes of the present invention is to provide a modified manganese dioxide positive electrode material, the modified manganese dioxide positive electrode material comprising:
[0008] A flower ball-like structure formed by the aggregation of multiple hydrated manganese dioxide nanosheets, wherein the nanosheets have a stable layered structure;
[0009] Ions and water molecules are distributed at least between the layers of the nanosheets, and the ions include alkali metal ions and alkaline earth metal ions.
[0010] The ions and water molecules in the modified manganese dioxide positive electrode material with the above structure can stabilize the layered structure of manganese dioxide; and the alkaline earth metal ion doping therein can promote the increase of oxygen vacancies in manganese dioxide, improve the conductivity of manganese dioxide, and thus improve the capacity and rate performance of the positive electrode material; in addition, the flower ball-like structure formed by the aggregation of nanosheets has a high specific surface area, which is conducive to promoting its full contact with the electrolyte; when the material is used in the positive electrode of a zinc ion battery, it can improve the diffusion kinetics of zinc ions in manganese dioxide, improve the specific capacity and cycle stability of the zinc ion battery, and the higher conductivity based on the alkaline earth metal ion doping can further improve the rate performance of the battery, so that the battery can be stably cycled at a high current density.
[0011] In some embodiments, the thickness of the nanosheet is 5 nm to 17 nm.
[0012] In some embodiments, the diameter of the flower ball-like structure is 3-10 μm, the pore size of the flower ball-like structure is 80-400 nm, and the specific surface area is 10-30 m 2 / g.
[0013] In some embodiments, in the positive electrode material, the molar ratio of the ions to manganese is 0.1-0.7, and the molar ratio of the water molecules to manganese is 0.3-3.
[0014] In some embodiments, the molar ratio of the alkaline earth metal ions to the alkali metal ions is 0.5 to 5. The present invention finds that different ratios of alkaline earth metal and alkali metal ions affect the size of the manganese dioxide interlayer spacing, and the size of the manganese dioxide interlayer spacing can affect the battery capacity. Within the above molar ratio range, the battery capacity can be further optimized.
[0015] In some embodiments, the alkali metal ions include one or a combination of sodium ions, lithium ions or potassium ions.
[0016] In some embodiments, the alkaline earth metal ions include barium ions and / or strontium ions, preferably barium ions. Strontium and barium ions doped into layered manganese dioxide can effectively improve the capacity, cycle stability and rate performance of manganese dioxide. Under the same doping content, the doping effect of barium ions is slightly better than that of strontium ions.
[0017] The second object of the present invention is to provide a method for preparing a modified manganese dioxide positive electrode material, comprising:
[0018] providing a manganese complex precursor solution comprising a divalent manganese salt, a complexing agent and a solvent;
[0019] Under room temperature conditions, a precipitant is mixed with the manganese complex precursor solution for reaction, and microwave-assisted reaction is performed during the mixing of the precipitant and the manganese complex precursor solution to obtain a product having a flower ball-like structure, wherein the precipitant includes a base containing alkali metal ions, and the flower ball-like structure is formed by aggregation of a plurality of hydrated manganese dioxide nanosheets, wherein the nanosheets have a stable layered structure, and water molecules and alkali metal ions are distributed between the layers;
[0020] The product with the flower ball structure is immersed in a solution containing alkaline earth metal ions, so that at least part of the alkali metal ions between the nanosheet layers are exchanged for alkaline earth metal ions, thereby preparing a modified manganese dioxide positive electrode material.
[0021] The method provided by the present invention can synthesize modified manganese dioxide materials under low energy consumption conditions, which exhibit a flower ball-like morphology with a high specific surface area composed of multiple nanosheets, and because the interlayers contain water molecules, alkali metal ions, and alkaline earth metal ions, they exhibit good stability and electrochemical properties. Specifically, the alkali precipitant is combined with microwave assistance to promote the formation of flower ball-shaped manganese dioxide without high temperature treatment. In addition, the present invention uses a solution impregnation method to modify manganese dioxide, so that alkaline earth metal ions are embedded in the manganese dioxide interlayer, and abundant oxygen vacancies are created to improve the conductivity and capacity of manganese dioxide, and promote the improvement of the cycle stability and rate performance of the battery; during the impregnation process, the alkaline earth metal ions can exchange at least part of the alkali metal ions therein, and the doping achieved by mild ion exchange is conducive to maintaining the stability of the manganese dioxide structure, and the manganese dioxide will not collapse due to the sudden loss of ions between the layers, nor will the space be deformed due to excessive ion embedding. The method for synthesizing manganese dioxide and performing doping modification on manganese dioxide is simple and easy, the whole reaction process is mild, low in energy consumption, and suitable for large-scale industrial production. When used as a positive electrode active material for a zinc ion battery, the method can promote the diffusion kinetics of zinc ions in the material and improve the cycle stability of the zinc ion battery.
[0022] In some embodiments, the complexing agent includes one or more of a phosphate complexing agent, an alcoholamine complexing agent, an aminocarboxylic acid complexing agent or a hydroxycarboxylic acid complexing agent, but is not limited thereto.
[0023] In some embodiments, the complexing agent includes one or more of disodium ethylenediaminetetraacetate, sodium citrate, sodium pyrophosphate, sodium diethylenetriaminepentacarboxylate, triethanolamine, and polyacrylic acid, but is not limited thereto.
[0024] In some embodiments, in the manganese complex precursor solution, the concentration of the complexing agent is 0.01-2 mol / L.
[0025] In some embodiments, the divalent manganese salt includes one or more of manganese sulfate, manganese nitrate, manganese acetate or manganese chloride, but is not limited thereto.
[0026] In some embodiments, the concentration of the divalent manganese salt in the manganese complex precursor solution is 0.01-4 mol / L.
[0027] In some embodiments, the solvent of the manganese complex precursor solution includes water.
[0028] In some embodiments, the manganese complex precursor solution does not contain an oxidant. That is, the method provided by the present invention can synthesize manganese dioxide materials without adding other strong oxidants, thereby solving the safety and environmental problems caused by the use of strong oxidants, as well as the problem of equipment loss.
[0029] In some embodiments, the base containing alkali metal ions is prepared into an alkali solution with a concentration of 0.1N3mol / L, and the alkali solution is added in batches and mixed with the manganese complex precursor solution in a volume ratio of 1:5 to 10:1. The addition rate of the alkali solution is 5 to 50mL / min, and microwave-assisted treatment is performed during the batch addition of the alkali solution. The microwave assistance is stopped after all the alkali solution has been added.
[0030] In some embodiments, the precipitant and the manganese complex precursor solution are mixed under stirring at a speed of 500 to 2000 rpm.
[0031] In some embodiments, after the precipitant and the manganese complex precursor solution are mixed, the mixture is maintained for 2 to 10 hours to carry out the reaction.
[0032] In some embodiments, the microwave-assisted conditions include: a temperature of 30° C. to 60° C. and a microwave power of 100 to 1000W.
[0033] In the above-mentioned range of alkali concentration, volume ratio of alkali to manganese complex precursor solution, and alkali addition rate, with microwave assistance, a manganese dioxide positive electrode material with better morphology and structure can be formed without other oxidants. Specifically, the alkali reacts with divalent manganese ions to form manganous hydroxide (Mn(OH)2), and the addition of the complexing agent promotes the formation of precipitation, so that manganous hydroxide can be oxidized to manganese oxyhydroxide (MnO(OH)) in the air, and the excess alkali in the solution causes the product to eventually become hydrated manganese dioxide (MnO2·xH2O).
[0034] In some embodiments, the alkali metal ions include one or more of sodium ions, lithium ions or potassium ions.
[0035] In some embodiments, the alkaline earth metal ions include barium ions and / or strontium ions. In the prior art, most of the studies on improving the performance of manganese dioxide by metal ion doping are focused on the doping of calcium and magnesium ions, and the related research on strontium and barium ions as doping ions is relatively vacant. One of the reasons is that strontium and barium ions are difficult to be beneficially combined with the manganese dioxide matrix. The method provided by the present invention can not only realize the successful doping of strontium and barium ions into layered manganese dioxide, improve the capacity, cycle stability and rate performance of manganese dioxide, but also the doping process is mild and not easy to damage the layered structure of manganese dioxide.
[0036] In some embodiments, the source of the barium ions and strontium ions includes one or more of their acetates, chlorides, or nitrates.
[0037] In some embodiments, the solid-to-liquid ratio of the product having a flower ball structure to the solution containing alkaline earth metal ions is 30:1 or less.
[0038] In some embodiments, the concentration of the solution containing alkaline earth metal ions is 0.3-3 mol / L. This alkaline earth metal ion concentration can promote an appropriate amount of alkaline earth metal ions to be embedded in the manganese dioxide interlayer.
[0039] In some embodiments, the product having a flower ball-like structure is immersed in the solution containing alkaline earth metal ions for 6 to 48 hours.
[0040] In some embodiments, the product having a flower ball structure is mixed with a solution containing alkaline earth metal ions and ultrasonically treated for 30 to 120 minutes, and then immersed for 6 to 48 hours. Under the above-mentioned ultrasonic treatment and immersion time conditions, the alkaline earth metal ions can be uniformly embedded in the manganese dioxide, and the original interlayer alkali metal ions can be exchanged to obtain a suitable alkaline earth metal ion doping concentration, thereby helping to improve the electrochemical properties of the manganese dioxide material.
[0041] The third object of the present invention is to provide a modified manganese dioxide positive electrode material prepared according to any of the above preparation methods.
[0042] A fourth object of the present invention is to provide an application of any of the above-mentioned modified manganese dioxide positive electrode materials in the preparation of a positive electrode for an aqueous zinc ion battery or an aqueous zinc ion battery.
[0043] A fifth object of the present invention is to provide a positive electrode for an aqueous zinc ion battery, comprising a positive electrode collector and a positive electrode active material layer arranged on the positive electrode collector, wherein the positive electrode active material layer comprises any of the modified manganese dioxide positive electrode materials described above.
[0044] In some embodiments, the positive electrode current collector includes carbon paper, carbon felt, stainless steel foil, titanium foil, etc., but is not limited thereto.
[0045] In some embodiments, the preparation method of the positive electrode for the aqueous zinc ion battery includes: mixing the modified manganese dioxide positive electrode material, conductive carbon black (super P) and polyvinylidene fluoride (PVDF) in a mass ratio of (6-8): (1-2): (1-2), adding methyl pyrrolidone, stirring and mixing evenly to obtain a positive electrode slurry; coating the positive electrode slurry on a positive electrode current collector, and drying to obtain a positive electrode sheet.
[0046] The sixth object of the present invention is to provide an aqueous zinc ion battery, comprising a positive electrode, a negative electrode, a separator and an electrolyte, wherein the positive electrode is the positive electrode for aqueous zinc ions.
[0047] The negative electrode, electrolyte and diaphragm can be any negative electrode, electrolyte and diaphragm suitable for aqueous zinc ion batteries in the prior art, and the present invention does not impose any particular restrictions on this. For example, the negative electrode can be metal zinc or modified metal zinc material. For example, the electrolyte can include 0.5 mol / L to 3 mol / L zinc sulfate and 0.05 mol / L to 0.4 mol / L manganese sulfate.
[0048] Compared with the prior art, the present invention has at least the following beneficial effects:
[0049] (1) The present invention provides a manganese dioxide positive electrode material having a flower ball-like structure formed by aggregation of nanosheets, wherein the alkali metal ions and water molecules contained between the layers can stabilize the layered structure, and the alkaline earth metal ions doped between the layers can promote the increase of oxygen vacancies in the manganese dioxide, thereby improving its conductivity and capacity; and the flower ball-like structure has a high specific surface area and porosity, which can promote sufficient contact between the manganese dioxide and the electrolyte, and the zinc ion battery containing the manganese dioxide positive electrode material has a high specific capacity and rate performance.
[0050] (2) The present invention provides a low-energy preparation method for manganese dioxide. By using an alkali precipitant in combination with microwave assistance, manganese dioxide with a specific structure can be obtained at room temperature without the need for high-temperature sintering, high-temperature and high-pressure environment, and application of current. This method can solve the problem that the preparation of manganese dioxide in the prior art requires high energy consumption and is not conducive to large-scale industrial production. In addition, this preparation method does not require the addition of a strong oxidant, can reduce safety hazards in the transportation, storage, and reaction processes of raw materials, has low requirements for equipment, and is conducive to controlling production costs.
[0051] (3) The present invention modifies manganese dioxide by a solution impregnation method, thereby increasing oxygen vacancies in manganese dioxide and improving its conductivity and capacity. The method is simple and easy to implement, and is beneficially combined with the manganese dioxide synthesis method to maintain its mild and low-energy synthesis route to the greatest extent. In addition, the impregnation method can allow alkaline earth metal ions to be gently doped into manganese dioxide by ion exchange, thereby improving its conductivity and capacity without destroying the original morphology and structure of manganese dioxide. BRIEF DESCRIPTION OF THE DRAWINGS
[0052] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0053] Figure 1 is a schematic diagram of the process for preparing a modified manganese dioxide positive electrode material in Example 1 of the present invention;
[0054] Figure 2 is the XRD pattern of manganese dioxide (not doped with barium) prepared in Comparative Example 3 of the present invention;
[0055] Figure 3 is the XRD pattern of the modified manganese dioxide prepared in Example 1 of the present invention;
[0056] Figure 4 is a SEM image of manganese dioxide (not doped with barium) prepared in Comparative Example 3 of the present invention;
[0057] Figure 5 is a SEM image of the modified manganese dioxide prepared in Example 1 of the present invention;
[0058] Figure 6 is a charge and discharge curve diagram of a full battery assembled with modified manganese dioxide prepared in Example 1 of the present invention at a rate of 0.1C;
[0059] Figure 7is a CV graph of a full battery assembled with modified manganese dioxide prepared in Example 1 of the present invention at a scan rate of 0.2 mV / s;
[0060] Figure 8 This is a cycle performance diagram of a full battery assembled with modified manganese dioxide synthesized in Example 1 of the present invention at a 1C rate.
[0061] Fig. 9 It is a comparison chart of the cycle performance of full batteries assembled with manganese dioxide synthesized in Example 2 of the present invention and Comparative Example 3 at 1C rate.
[0062] Fig.10 It is a comparison chart of the rate performance of full batteries assembled with the manganese dioxide synthesized in Example 2 of the present invention and Comparative Example 3. DETAILED DESCRIPTION
[0063] The technical solution of the present invention is described in detail below in conjunction with specific embodiments so that those skilled in the art can better understand and implement the technical solution of the present invention. The specific functional details disclosed herein should not be interpreted as limiting, but only as the basis for the claims and as a representative basis for teaching those skilled in the art to adopt the present invention in different ways in any appropriate detailed embodiment.
[0064] Example 1
[0065] This embodiment provides a modified manganese dioxide positive electrode material and a preparation method thereof. Figure 1 It is a schematic diagram of the preparation process, which is as follows:
[0066] Prepare 60 mL of a manganese complex precursor aqueous solution, wherein the concentration of disodium ethylenediaminetetraacetate is 0.1 mol / L and the concentration of manganese sulfate is 0.3 mol / L; prepare 50 mL of a 2 mol / L sodium hydroxide solution as a precipitant;
[0067] The sodium hydroxide solution is added dropwise into the manganese complex precursor solution at a speed of 10 mL / min. During the addition, the solution is placed in a 400 W microwave reactor, the temperature is set to 40° C., and the solution is stirred at a speed of 800 rpm. After the addition is completed, the microwave is stopped, and the speed is maintained to react for 5 hours. After the reaction is completed, the solution is filtered and then washed with deionized water to obtain a precipitate, which is manganese dioxide.
[0068] The manganese dioxide obtained above was immersed in a 1 mol / L barium acetate solution at a solid-liquid ratio of 40:3 and ultrasonically treated for 30 minutes, and then immersed for 24 hours. After the immersion was completed, it was filtered, and the solid obtained was washed with deionized water and dried to obtain a modified manganese dioxide positive electrode material.
[0069] The obtained modified manganese dioxide positive electrode material is used to prepare a zinc ion battery, as follows:
[0070] Modified manganese dioxide is used as an active material, and modified manganese dioxide, conductive carbon black, and polyvinylidene fluoride are mixed in a mass ratio of 7:2:1, and an appropriate amount of methyl pyrrolidone is added, and the mixture is stirred and mixed evenly to obtain a positive electrode slurry; the positive electrode slurry is coated on carbon paper, and placed in an oven at 80°C for 12 hours to obtain a positive electrode sheet;
[0071] A zinc ion battery was assembled using metallic zinc as the negative electrode and an aqueous solution of 2 mol / L zinc sulfate and 0.1 mol / L manganese sulfate as the electrolyte, and the battery was tested. The test results are shown in Table 1.
[0072] Example 2
[0073] Prepare 100 mL of a manganese complex precursor aqueous solution, wherein the concentration of sodium citrate is 0.3 mol / L and the concentration of manganese sulfate is 0.3 mol / L; prepare 60 mL of a 2 mol / L sodium hydroxide solution as a precipitant;
[0074] The sodium hydroxide solution is added dropwise into the manganese complex precursor solution at a speed of 20 mL / min. During the addition, the solution is placed in a 400 W microwave reactor, the temperature is set to 40° C., and the solution is stirred at a speed of 800 rpm. After the addition is completed, the microwave is stopped, and the speed is maintained to react for 5 h. After the reaction is completed, the solution is filtered and then washed with deionized water to obtain a precipitate, which is manganese dioxide.
[0075] The manganese dioxide obtained above was immersed in a 1 mol / L barium chloride solution with a solid-liquid ratio of 40:3 for 30 minutes under ultrasonication, and then maintained immersed for 24 hours. After the immersion was completed, vacuum filtration was performed, and the solid was washed with deionized water, and then dried to obtain a modified manganese dioxide positive electrode material.
[0076] The modified manganese dioxide positive electrode material obtained in this example was used, and a positive electrode slurry was prepared in the same manner as in Example 1. The positive electrode slurry was coated on a stainless steel foil and dried in an oven at 80°C for 12 hours to form a positive electrode sheet. Metal zinc was used as the negative electrode, and an aqueous solution of 2 mol / L zinc sulfate and 0.2 mol / L manganese sulfate was used as the electrolyte to assemble a full battery, which was tested. The test results are shown in Table 1.
[0077] Example 3
[0078] Prepare 120 mL of a manganese complex precursor aqueous solution, wherein the concentration of sodium pyrophosphate is 0.1 mol / L and the concentration of manganese sulfate is 0.5 mol / L; prepare 100 mL of a potassium hydroxide solution with a concentration of 1.5 mol / L as a precipitant;
[0079] The potassium hydroxide solution is added dropwise into the manganese complex precursor solution at a rate of 20 mL / min. During the addition, the solution is placed in a 300 W microwave reactor, the temperature is set to 30° C., and stirring is maintained at a speed of 1000 rpm. After the addition is completed, the microwave is stopped, and the speed is maintained to react for 3 hours. After the reaction is completed, the solution is filtered and then washed with deionized water to obtain a precipitate, which is manganese dioxide;
[0080] The manganese dioxide obtained above was immersed in a 1.5 mol / L barium acetate solution at a solid-liquid ratio of 25:2 and ultrasonicated for 1 hour, and then maintained immersed for 24 hours. After the immersion was completed, it was filtered, washed with deionized water to obtain a solid state, and dried to obtain a modified manganese dioxide positive electrode material.
[0081] The modified manganese dioxide positive electrode material obtained in this example was used, and a positive electrode slurry was prepared in the same manner as in Example 1. The positive electrode slurry was coated on carbon felt and dried in an oven at 80°C for 12 hours to form a positive electrode sheet. Metal zinc was used as the negative electrode, and an aqueous solution of 2 mol / L zinc sulfate and 0.1 mol / L manganese sulfate was used as the electrolyte to assemble a full battery, which was tested. The test results are shown in Table 1.
[0082] Example 4
[0083] Prepare 100 mL of a manganese complex precursor aqueous solution, wherein the concentration of sodium diethylenetriamine pentacarboxylate is 0.1 mol / L and the concentration of manganese sulfate is 0.2 mol / L; prepare 60 mL of a 1.5 mol / L sodium hydroxide solution as a precipitant;
[0084] The sodium hydroxide solution is added dropwise into the manganese complex precursor solution at a rate of 40 mL / min. During the addition, the solution is placed in a 400 W microwave reactor, the temperature is set to 50° C., and the solution is stirred at a speed of 1000 rpm. After the addition is completed, the microwave is stopped, and the speed is maintained to react for 4 hours. After the reaction is completed, the solution is filtered and then washed with deionized water to obtain a precipitate, which is manganese dioxide.
[0085] The manganese dioxide obtained above was immersed in a 1.5 mol / L strontium acetate solution at a solid-liquid ratio of 25:2 and ultrasonicated for 1 hour, and then maintained immersed for 24 hours. After the immersion was completed, it was filtered, washed with deionized water to obtain a solid, and dried to obtain a modified manganese dioxide positive electrode material.
[0086] The modified manganese dioxide positive electrode material obtained in this example was used, and a positive electrode slurry was prepared in the same manner as in Example 1. The positive electrode slurry was coated on a titanium foil and dried in an oven at 80°C for 12 hours to form a positive electrode sheet. Metal zinc was used as the negative electrode, and an aqueous solution of 2 mol / L zinc sulfate and 0.1 mol / L manganese sulfate was used as the electrolyte to assemble a full battery, which was then tested.
[0087] Example 5
[0088] Prepare 120 mL of a manganese complex precursor aqueous solution, wherein the concentration of triethanolamine is 0.1 mol / L and the concentration of manganese acetate is 0.3 mol / L; prepare 100 mL of a 1.5 mol / L sodium hydroxide solution as a precipitant;
[0089] The sodium hydroxide solution is added dropwise into the manganese complex precursor solution at a rate of 15 mL / min. During the addition, the solution is placed in an 800 W microwave reactor, the temperature is set to 40° C., and stirring is maintained at a speed of 1000 rpm. After the addition is completed, the microwave is stopped, and the speed is maintained to react for 3 hours. After the reaction is completed, the solution is filtered and then washed with deionized water to obtain a precipitate, which is manganese dioxide;
[0090] The manganese dioxide obtained above was immersed in a 1.5 mol / L barium acetate solution at a solid-liquid ratio of 15:1 and then immersed for 12 hours. After the immersion was completed, vacuum filtration was performed, and the solid was obtained by deionization washing, and then dried to obtain a modified manganese dioxide positive electrode material.
[0091] The modified manganese dioxide positive electrode material obtained in this example was used, and a positive electrode slurry was prepared in the same manner as in Example 1. The positive electrode slurry was coated on carbon paper and dried in an oven at 80°C for 12 hours to form a positive electrode sheet. Metal zinc was used as the negative electrode, and an aqueous solution of 2 mol / L zinc sulfate and 0.2 mol / L manganese sulfate was used as the electrolyte to assemble a full battery, which was tested. The test results are shown in Table 1.
[0092] Example 6
[0093] Prepare 100 mL of a manganese complex precursor aqueous solution, wherein the concentration of polyacrylic acid is 0.1 mol / L and the concentration of manganese chloride is 0.2 mol / L; prepare 60 mL of a 1.5 mol / L sodium hydroxide solution as a precipitant;
[0094] The sodium hydroxide solution is added dropwise into the manganese complex precursor solution at a speed of 20 mL / min. During the addition, the solution is placed in a 500 W microwave reactor, the temperature is set to 30° C., and stirring is maintained at a speed of 1000 rpm. After the addition is completed, the microwave is stopped, and the speed is maintained to react for 4 hours. After the reaction is completed, the solution is filtered and then washed with deionized water to obtain a precipitate, which is manganese dioxide;
[0095] The manganese dioxide obtained above was immersed in a 1.5 mol / L barium chloride solution with a solid-liquid ratio of 20:1 and ultrasonically treated for 1.5 h, and then immersed for 24 h. After the immersion was completed, it was filtered, and the solid obtained was washed with deionized water and dried to obtain a modified manganese dioxide positive electrode material.
[0096] The modified manganese dioxide positive electrode material obtained in this example was used, and a positive electrode slurry was prepared in the same manner as in Example 1. The positive electrode slurry was coated on a stainless steel foil and dried in an oven at 80°C for 12 hours to form a positive electrode sheet. Metal zinc was used as the negative electrode, and an aqueous solution of 2 mol / L zinc sulfate and 0.1 mol / L manganese sulfate was used as the electrolyte to assemble a full battery, which was tested. The test results are shown in Table 1.
[0097] Example 7
[0098] Prepare 100 mL of a manganese complex precursor aqueous solution, wherein the concentration of disodium ethylenediaminetetraacetate is 0.1 mol / L and the concentration of manganese nitrate is 0.2 mol / L; prepare 70 mL of a 1.5 mol / L sodium hydroxide solution as a precipitant;
[0099] The sodium hydroxide solution is added dropwise to the manganese complex precursor solution at a speed of 5 mL / min. During the addition process, it is placed in a 1000 W microwave reactor, the temperature is set to 60° C., and stirring is maintained at a speed of 1000 rpm. After the addition is completed, the microwave is stopped, and the speed is maintained to react for 3 hours. After the reaction is completed, it is filtered and then washed with deionized water to obtain a precipitate, which is manganese dioxide;
[0100] The manganese dioxide obtained above was immersed in a 1.5 mol / L barium nitrate solution with a solid-liquid ratio of 27:1 and ultrasonically treated for 2 hours, and then immersed for another 12 hours. After the immersion was completed, it was filtered, washed with deionized water to obtain a solid, and dried to obtain a modified manganese dioxide positive electrode material.
[0101] The modified manganese dioxide positive electrode material obtained in this example was used, and a positive electrode slurry was prepared in the same manner as in Example 1. The positive electrode slurry was coated on carbon paper and dried in an oven at 80°C for 12 hours to form a positive electrode sheet. Metal zinc was used as the negative electrode, and an aqueous solution of 2 mol / L zinc sulfate and 0.2 mol / L manganese sulfate was used as the electrolyte to assemble a full battery, which was tested. The test results are shown in Table 1.
[0102] Example 8
[0103] The only difference between Example 8 and Example 7 is that the manganese dioxide is immersed in a 1.5 mol / L barium nitrate solution and ultrasonicated for 2 hours, and then maintained immersed for another 6 hours.
[0104] Example 9
[0105] The difference between Example 9 and Example 7 is that the manganese dioxide is immersed in a 1.5 mol / L barium nitrate solution and ultrasonicated for 2 hours, and then immersed for another 3 hours.
[0106] Example 10
[0107] The difference between Example 10 and Example 7 is that the manganese dioxide is immersed in a 1.5 mol / L barium nitrate solution and ultrasonicated for 2 hours, and then maintained immersed for another hour.
[0108] Embodiment 11
[0109] The only difference between Example 11 and Example 7 is that the manganese dioxide is immersed in a 1.5 mol / L barium nitrate solution for 12 h without ultrasonic treatment.
[0110] Example 12
[0111] Prepare 60 mmL of manganese complex precursor aqueous solution, wherein the concentration of disodium ethylenediaminetetraacetate is 0.01 mol / L and the concentration of manganese sulfate is 0.01 mol / L; prepare 50 mL of 0.1 mol / L sodium hydroxide solution as a precipitant;
[0112] The sodium hydroxide solution was added dropwise into the manganese complex precursor solution at a speed of 50 mL / min, and the solution was placed in a 100 W microwave reactor, the temperature was set to 60° C., and the solution was stirred at a speed of 500 rpm. After the addition was completed, the microwave was stopped, and the speed was maintained to react for 2 h. After the reaction was completed, the solution was filtered and washed with deionized water to obtain the precipitate, which was manganese dioxide.
[0113] The manganese dioxide obtained above was immersed in a 0.3 mol / L barium acetate solution with a solid-liquid ratio of 10:1 and ultrasonically treated for 30 minutes, and then immersed for 48 hours. After the immersion was completed, it was filtered, and the solid obtained was washed with deionized water and dried to obtain a modified manganese dioxide positive electrode material.
[0114] The modified manganese dioxide positive electrode material obtained in this example was used to make a full battery in the same manner as in Example 1, and the battery was tested. The test results are shown in Table 1.
[0115] Embodiment 13
[0116] Prepare 60 mL of a manganese complex precursor aqueous solution, wherein the concentration of disodium ethylenediaminetetraacetate is 2 mol / L and the concentration of manganese sulfate is 4 mol / L; prepare 50 mL of a 3 mol / L sodium hydroxide solution as a precipitant;
[0117] The sodium hydroxide solution is added dropwise into the manganese complex precursor solution at a speed of 50 mL / min, and the solution is placed in a 300 W microwave reactor, the temperature is set to 40° C., and the solution is stirred at a speed of 2000 rpm. After the addition is completed, the microwave is stopped, and the speed is maintained to react for 10 hours. After the reaction is completed, the solution is filtered and then washed with deionized water to obtain a precipitate, which is manganese dioxide.
[0118] The manganese dioxide obtained above was immersed in a 3 mol / L barium acetate solution at a solid-liquid ratio of 30:1 and ultrasonically treated for 30 minutes, and then immersed for 48 hours. After the immersion was completed, it was filtered, and the solid obtained was washed with deionized water and dried to obtain a modified manganese dioxide positive electrode material.
[0119] The modified manganese dioxide positive electrode material obtained in this example was used to make a full battery in the same manner as in Example 1, and the battery was tested. The test results are shown in Table 1.
[0120] Embodiment 14
[0121] The only difference between Example 14 and Example 1 is that barium acetate is replaced by strontium acetate, and the rest is implemented in the same way as Example 1.
[0122] Comparative Example 1
[0123] Comparative Example 1 provides a barium-doped modified manganese dioxide whose raw material contains a strong oxidant (potassium permanganate), and the preparation method thereof is as follows:
[0124] 12 mmol potassium permanganate and 2 mmol manganese sulfate were dissolved in 60 ml deionized water, and 0.28 mmol barium chloride was added as a dopant, and stirred to completely dissolve the mixture to obtain a precursor solution;
[0125] The precursor solution was transferred to a stainless steel reactor with a volume of 100 mL, and heated at 160° C. for 12 h to react. After the reaction was completed, it was cooled, and the reaction product was taken out, filtered, washed, and dried to obtain manganese dioxide.
[0126] In the same manner as in Example 1, a zinc ion battery was prepared using the manganese dioxide of Comparative Example 1 and tested. The test results are shown in Table 1.
[0127] Comparative Example 2
[0128] Prepare 100 mL of 115 g / L manganese sulfate solution and 100 mL of 223.39 g / L ammonium bicarbonate solution;
[0129] The ammonium bicarbonate solution was added to the manganese sulfate solution, and the mixture was stirred for 2 hours. The suspension after the reaction was filtered, washed and dried to obtain a manganese carbonate precipitate.
[0130] The manganese carbonate precipitate is placed in a muffle furnace and sintered at 350°C for 3 hours in an air atmosphere to obtain manganese dioxide;
[0131] The obtained manganese dioxide was soaked in 40% sulfuric acid for 2 hours to remove manganese carbonate and manganese monoxide impurities, and then filtered, washed and dried with deionized water to obtain a manganese dioxide positive electrode material.
[0132] In the same manner as in Example 1, a zinc ion battery was prepared using the manganese dioxide of Comparative Example 2 and tested. The test results are shown in Table 1.
[0133] Comparative Example 3
[0134] The only difference between Comparative Example 3 and Example 1 is that the step of immersing the manganese dioxide in a 1 mol / L barium acetate solution is not performed, that is, the manganese dioxide positive electrode material obtained in Comparative Example 3 is not doped with barium.
[0135] In the same manner as in Example 1, a zinc ion battery was prepared using the manganese dioxide of Comparative Example 3 and tested. The test results are shown in Table 1.
[0136] Comparative Example 4
[0137] The difference between Comparative Example 4 and Example 1 is that barium acetate is replaced by calcium chloride, and the rest is the same as Example 1.
[0138] Comparative Example 5
[0139] The difference between Comparative Example 5 and Example 1 is that barium acetate is replaced by magnesium chloride, and the rest is the same as Example 1.
[0140] Figure 2 is the XRD pattern of the manganese dioxide not doped with barium prepared in Comparative Example 3; Figure 3 is the XRD pattern of the modified manganese dioxide doped with barium in Example 1, Figure 3 This indicates that the barium-doped manganese dioxide is successfully synthesized by the strong oxidant-free, room temperature synthesis method adopted in the present invention.
[0141] Figure 4 is a SEM image of the manganese dioxide not doped with barium prepared in Comparative Example 3; Figure 5 This is the SEM image of the modified manganese dioxide obtained in Example 1, showing a flower ball structure with a diameter of about 3N10μm. The specific surface area test is about 10-40m 2 / g. Contrast Figure 4 , Figure 5 It can be seen that the modified manganese dioxide obtained by solution impregnation still maintains the flower ball-like morphology composed of nanosheets, indicating that the impregnation modification method can maintain the morphology and structural stability of manganese dioxide to the greatest extent.
[0142] The elemental composition analysis (EDS test) of the modified manganese dioxide prepared in Example 1 shows that the atomic proportions of Mn, O, Ba, and Na are 29.02%, 65.78%, 1.81%, and 3.39%, respectively. In addition, through the XPS peak data of O, it can be obtained that the oxygen in the water molecule accounts for 15.6% of all oxygen.
[0143] Figure 6is a charge and discharge curve diagram of the full battery in Example 1 at a rate of 0.1C; Figure 7 is a CV graph of the full battery of Example 1 at a scan rate of 0.2 mV / s; Figure 8 It is a cycle performance curve diagram of the full battery of Example 1 at 1C rate, which shows that the manganese dioxide synthesized by this method has good cycle stability.
[0144] Fig. 9 is a cycle performance diagram of the full battery of Example 2 and Comparative Example 3 at 1C rate, Fig.10 It is a comparison chart of the rate performance of the full batteries of Example 2 and Comparative Example 3. Fig. 9 , Fig.10 This shows that the impregnation modification method can greatly improve the discharge specific capacity of the material while maintaining the original good cycle stability.
[0145] Table 1 Related performances of zinc ion batteries in the embodiments of the present invention and the comparative examples
[0146]
[0147]
[0148] Among them, IC=308mAh / g during battery testing
[0149] The various aspects, embodiments, features and examples of the present invention should be considered as illustrative in all aspects and are not intended to limit the present invention, the scope of the present invention is defined only by the claims. Other embodiments, modifications and uses will be apparent to those skilled in the art without departing from the spirit and scope of the claimed invention.
[0150] In addition, the inventors of this case also referred to the aforementioned embodiments and conducted experiments with other raw materials, process operations, and process conditions described in this specification, and obtained relatively ideal results.
[0151] Although the present invention has been described with reference to illustrative embodiments, it will be appreciated by those skilled in the art that various other changes, omissions and / or additions may be made without departing from the spirit and scope of the present invention and that the elements of the embodiments may be replaced by substantial equivalents. In addition, many modifications may be made without departing from the scope of the present invention to adapt specific circumstances or materials to the teachings of the present invention. Therefore, it is not intended herein to limit the present invention to the disclosed specific embodiments for performing the present invention, but it is intended that the present invention will include all embodiments within the scope of the appended claims. In addition, unless specifically stated, any use of the terms first, second, etc. does not indicate any order or importance, but rather uses the terms first, second, etc. to distinguish one element from another.
Claims
1. A modified manganese dioxide positive electrode material, It is characterized in that include: A flower ball-like structure formed by the aggregation of multiple hydrated manganese dioxide nanosheets, wherein the nanosheets have a layered structure; Ions and water molecules are distributed at least between the layers of the nanosheets, and the ions include alkali metal ions and alkaline earth metal ions.
2. The modified manganese dioxide positive electrode material according to claim 1, It is characterized in that The thickness of the nanosheet is 5nm to 17nm; And / or, the diameter of the flower ball structure is 3-10 μm, the pore size of the flower ball structure is 80-400 nm, and the specific surface area is 10-30 m 2 / g; And / or, in the positive electrode material, the molar ratio of the ions to manganese is 0.1 to 0.7, and the molar ratio of the water molecules to manganese is 0.3 to 3; and / or, the molar ratio of the alkaline earth metal ions to the alkali metal ions is 0.5 to 5; And / or, the alkali metal ions include one or a combination of more of sodium ions, lithium ions or potassium ions, and the alkaline earth metal ions include barium ions and / or strontium ions.
3. A method for preparing a modified manganese dioxide positive electrode material, It is characterized in that include: providing a manganese complex precursor solution comprising a divalent manganese salt, a complexing agent and a solvent; Under room temperature conditions, a precipitant is mixed with the manganese complex precursor solution, and microwave-assisted reaction is performed during the mixing of the precipitant and the manganese complex precursor solution to obtain a product having a flower ball-like structure, wherein the precipitant includes a base containing alkali metal ions, and the flower ball-like structure is formed by aggregation of a plurality of hydrated manganese dioxide nanosheets, wherein the nanosheets have a layered structure, and water molecules and alkali metal ions are distributed between the layers; The product with the flower ball structure is immersed in a solution containing alkaline earth metal ions, so that at least part of the alkali metal ions between the nanosheet layers are exchanged for alkaline earth metal ions, thereby preparing a modified manganese dioxide positive electrode material.
4. The preparation method according to claim 3, Features: The complexing agent includes one or more of a phosphate complexing agent, an alcoholamine complexing agent, an aminocarboxylic acid complexing agent or a hydroxycarboxylic acid complexing agent; and / or, the concentration of the complexing agent in the manganese complex precursor solution is 0.01 to 2 mol / L; And / or, the divalent manganese salt includes one or more of manganese sulfate, manganese nitrate, manganese acetate or manganese chloride; and / or, the concentration of the divalent manganese salt in the manganese complex precursor solution is 0.01N4mol / L; and / or, the solvent comprises water; And / or, the manganese complex precursor solution does not contain an oxidant.
5. The preparation method according to claim 4, Features: The complexing agent includes one or a combination of multiple of disodium ethylenediaminetetraacetate, sodium citrate, sodium pyrophosphate, sodium diethylenetriaminepentacarboxylate, triethanolamine, and polyacrylic acid.
6. The preparation method according to claim 3, Features: The alkali containing alkali metal ions is prepared into an alkali solution with a concentration of 0.1 to 3 mol / L, and the alkali solution is mixed with the manganese complex precursor solution in a volume ratio of 1:5 to 10:1 in a batch-wise manner, the alkali solution is added at a speed of 5 to 50 mL / min, and microwave-assisted treatment is performed during the batch-wise addition of the alkali solution; and / or, after the precipitant and the manganese complex precursor solution are mixed, maintaining the mixture for 2 to 10 hours to carry out the reaction; And / or, the microwave-assisted conditions include: a temperature of 30° C. to 60° C., a microwave power of 100 to 1000 W; And / or, the alkali metal ions include one or more of sodium ions, lithium ions or potassium ions, and the alkaline earth metal ions include barium ions and / or strontium ions; and / or, the solid-to-liquid ratio of the product having a flower ball structure to the solution containing alkaline earth metal ions is 30:1 or less; and / or, the concentration of the solution containing alkaline earth metal ions is 0.3 to 3 mol / L; And / or, the immersion time is 6 to 48 hours; And / or, the product having a flower ball structure is mixed with a solution containing alkaline earth metal ions and ultrasonically treated for 30 to 120 minutes, and then immersed for 6 to 48 hours.
7. The modified manganese dioxide positive electrode material prepared by the method according to any one of claims 3 to 6.
8. Use of the modified manganese dioxide positive electrode material according to claim 1, 2 or 7 in preparing a positive electrode for an aqueous zinc ion battery or an aqueous zinc ion battery.
9. A positive electrode for an aqueous zinc ion battery, comprising a positive electrode current collector and a positive electrode active material layer disposed on the positive electrode current collector, It is characterized in that The positive electrode active material layer comprises the modified manganese dioxide positive electrode material according to claim 1, 2 or 7.
10. An aqueous zinc ion battery comprising a positive electrode, a negative electrode, a separator and an electrolyte, Features: The positive electrode is the positive electrode for aqueous zinc ions according to claim 9.
Citation Information
Patent Citations
Method for preparing nano manganese dioxide of different crystal forms and appearances by adopting microwave hydrothermal method
CN101698512A
Preparation method and application of high-stability copper intercalation manganese dioxide electrode material
CN113410443A
Birnessite type manganese dioxide nano flower ball with high crystallinity and preparation method and application of birnessite type manganese dioxide nano flower ball
CN113548695A
Preparation method, product and application of doped birnessite nano flower balls
CN116062795A
Cited By
Ruthenium-substituted manganese dioxide-doped positive electrode material for zinc ion battery as well as preparation method and application of ruthenium-substituted manganese dioxide-doped positive electrode material
CN120341274A