Method for manufacturing all-solid-state secondary battery
Through the multi-layer compression process and rolling method, the homogeneity problem of all-solid-state secondary batteries is solved, the strength and flatness of the battery are improved, an all-solid-state secondary battery with excellent homogeneity is realized, and the service life of the battery is extended. .
Patent Information
- Application Number
- CN202410202128.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-02-23
- Publication Date
- 2024-10-01
AI Technical Summary
Existing all-solid-state secondary batteries have problems with homogeneity, which affects their performance and lifespan.
A multi-layer compression process is adopted, including the stacking compression method of the positive electrode layer, electrolyte layer, intermediate layer and negative electrode layer. Through different pressures and rolling methods, the electrolyte layer is flattened, the positive electrode layer is dense, the interface is smooth, and the negative electrode layer and the intermediate layer are ensured. The high bonding properties improve the strength and flatness of the battery.
An all-solid-state secondary battery with excellent homogeneity is realized, the strength and flatness of the battery are improved, the extension or cracking of the electrolyte layer is suppressed, the bonding between the negative electrode layer and the intermediate layer is enhanced, and the service life of the battery is extended.
Smart Images

Figure CN118738499A_ABST
Abstract
Description
[0001] This application claims priority based on Japanese Patent Application No. 2023-052753 filed on March 29, 2023, the contents of which are incorporated herein by reference. Technical Field
[0002] The invention relates to a method for manufacturing an all-solid-state secondary battery. Background Art
[0003] In recent years, research and development related to secondary batteries that contribute to energy efficiency are being carried out to ensure that more people can obtain affordable, reliable, sustainable and advanced energy. Even in secondary batteries, all-solid-state secondary batteries with excellent characteristics in terms of safety, life, output, etc. are also attracting attention. As a method for manufacturing an all-solid-state secondary battery, a method for stamping a laminate consisting of a positive electrode layer, a solid electrolyte and a negative electrode layer is known (for example, referring to Japanese Patent No. 6251974). Summary of the invention
[0004] However, in the technology related to secondary batteries, obtaining homogeneity of all-solid-state batteries is a problem.
[0005] The purpose of the present invention is to realize a method for manufacturing an all-solid-state secondary battery having excellent homogeneity and to contribute to improving energy efficiency.
[0006] The aspects of the present invention provide the following means.
[0007] A method for manufacturing an all-solid-state secondary battery according to one embodiment of the present invention comprises: a positive electrode layer forming step, in which a positive electrode layer containing a positive electrode active material is formed; an electrolyte layer stacking step, in which an electrolyte layer containing a solid electrolyte is stacked on one surface of the positive electrode layer; a first compression step, in which a first compressed body is obtained by compressing the positive electrode layer and the electrolyte layer at a first pressure; an intermediate layer stacking step, in which an intermediate layer is stacked on the exposed surface of the electrolyte layer in the first compressed body; a second compression step, in which a second compressed body is obtained by compressing the positive electrode layer, the electrolyte layer and the intermediate layer at a second pressure; a negative electrode layer stacking step, in which a negative electrode layer is stacked on the exposed surface of the intermediate layer in the second compressed body; and a third compression step, in which a third compressed body is obtained by compressing the positive electrode layer, the electrolyte layer, the intermediate layer and the negative electrode layer at a third pressure. The positive electrode layer forming step, the electrolyte layer stacking step, the first compression step, the intermediate layer stacking step, the second compression step, the negative electrode layer stacking step, and the third compression step are performed in sequence. The second pressure is higher than the first pressure and the third pressure.
[0008] According to this method, the electrolyte layer is flattened by performing the first compression step. Since the electrolyte layer is flattened, even if the intermediate layer is stacked on the electrolyte layer and the second compression step is performed, the electrolyte layer can be prevented from sinking into the intermediate layer.
[0009] By performing the second compression step, the positive electrode layer and the intermediate layer become dense, thereby preventing the electrolyte layer from sinking into the intermediate layer.
[0010] By implementing the third compression step, the strength of the all-solid-state secondary battery is improved. For example, in the use environment of the all-solid-state secondary battery, even if repeated loads such as compression and non-compression in the surface direction of the electrolyte layer are generated in the all-solid-state secondary battery, the occurrence of damage caused by the extension or rupture of the electrolyte layer can be suppressed.
[0011] In addition, the smoothness of the interface between the electrolyte layer and the intermediate layer is improved, so an all-solid-state secondary battery with excellent homogeneity can be realized.
[0012] In the method for manufacturing an all-solid-state secondary battery according to one aspect of the present invention, in the positive electrode layer forming step, the positive electrode layer may be formed so as to be stacked on a positive electrode current collector.
[0013] According to this method, the first compressed body includes the positive electrode collector, the positive electrode layer, and the electrolyte layer. Even after the first compression step, damage to the positive electrode collector can be suppressed in the first compressed body.
[0014] In a method for manufacturing an all-solid-state secondary battery according to one embodiment of the present invention, the positive electrode collector may have a first surface and a second surface opposite to the first surface, and in the positive electrode layer forming step, the positive electrode layer is formed respectively on the first surface and the second surface of the positive electrode collector.
[0015] According to this method, a positive electrode layer is formed on the first surface of the positive electrode collector. Similarly, a positive electrode layer is formed on the second surface of the positive electrode collector. That is, a structure in which a positive electrode layer is formed on both surfaces of the positive electrode collector is obtained. In such a structure, even after the first compression process, the second compression process and the third compression process are performed, the restoring force of the positive electrode layer generated on the first surface and the restoring force of the positive electrode layer generated on the second surface cancel each other out. Therefore, in the whole of the all-solid-state secondary battery, the occurrence of warping is suppressed. Therefore, the flatness of the all-solid-state secondary battery can be improved. In particular, when a roller pressing method is used in the first compression process, the second compression process and the third compression process, the difference in friction coefficient between the surface of the roller and the surface of the laminate stacked on both surfaces of the positive electrode collector can be reduced. Thus, the flatness of the all-solid-state secondary battery can be improved.
[0016] In the method for manufacturing an all-solid-state secondary battery according to one aspect of the present invention, the intermediate layer may include a solid electrolyte, a carbide, and a binder.
[0017] Typically, the electrolyte layer is composed of a powder. Therefore, in a structure in which the negative electrode layer is directly bonded to the electrolyte layer, the bonding between the negative electrode layer and the electrolyte layer is low. In contrast, in a method for manufacturing an all-solid-state secondary battery of one embodiment of the present invention, an intermediate layer is sandwiched between the negative electrode layer and the electrolyte layer, and the intermediate layer has a solid electrolyte, a carbide and an adhesive. Therefore, compared with a structure in which the negative electrode layer is directly bonded to the electrolyte layer, in a structure having an intermediate layer, the bonding between the negative electrode layer and the electrolyte layer can be improved.
[0018] In the manufacturing method of an all-solid-state secondary battery of one embodiment of the present invention, the negative electrode layer may have a negative electrode opposing surface opposite to the intermediate layer, and before the negative electrode layer stacking process is performed, the negative electrode opposing surface is roughened, and after the roughened surface treatment is performed, the negative electrode layer stacking process is performed.
[0019] According to this method, by roughening the negative electrode facing surface of the negative electrode layer, a fine concavo-convex shape can be formed on the negative electrode facing surface. In this case, at the interface where the negative electrode facing surface contacts the intermediate layer, the intermediate layer easily enters the concavo-convex shape of the negative electrode facing surface. Therefore, the bonding property between the negative electrode layer and the intermediate layer can be improved.
[0020] In the method for manufacturing an all-solid-state secondary battery according to one aspect of the present invention, in the surface roughening treatment, the surface roughness of the negative electrode facing surface may be set to 20 μm or more.
[0021] According to this method, the surface roughness of the negative electrode facing surface of the negative electrode layer can be fully ensured. In addition, the negative electrode facing surface becomes a surface that is easily deformed. Therefore, when the negative electrode layer is deformed in the third compression step, the stress generated between the negative electrode layer and the intermediate layer is absorbed, and the cushioning property can be improved. Therefore, it is possible to suppress undesired deformation and to apply uniform pressure between the negative electrode layer and the intermediate layer. The bonding property between the negative electrode layer and the intermediate layer can be improved.
[0022] In the manufacturing method of an all-solid-state secondary battery of one embodiment of the present invention, it may be that a compression component for compressing a compression object is used in each of the first compression process, the second compression process, and the third compression process, and in at least one of the first compression process, the second compression process, and the third compression process, the compression component compresses the compression object with a protective sheet sandwiched between the compression object and the compression component.
[0023] According to the method, at least one of the first compression process, the second compression process, and the third compression process is performed using a protective sheet. Therefore, even if pressure is applied to the layer constituting the all-solid-state secondary battery, the damage of the layer can be suppressed. Here, the layer constituting the all-solid-state secondary battery is, for example, a positive electrode collector and a negative electrode layer. In particular, when the layer constituting the all-solid-state secondary battery is a thinner foil-like material, the effect of suppressing the damage of the layer is obtained.
[0024] A method for manufacturing an all-solid-state secondary battery according to one embodiment of the present invention may also include: a negative electrode collector stacking step, in which, after the third compression step, the negative electrode collector is stacked on the exposed surface of the negative electrode layer in the third compressed body; and a fourth compression step, in which the positive electrode layer, the electrolyte layer, the intermediate layer, the negative electrode layer and the negative electrode collector are compressed to obtain an all-solid-state secondary battery.
[0025] According to this method, a structure in which the negative electrode current collector is stacked on the negative electrode layer can be obtained.
[0026] In a method for manufacturing an all-solid-state secondary battery according to one embodiment of the present invention, a compression member for compressing an object to be compressed may be used in the fourth compression step, and in the fourth compression step, the compression member compresses the object to be compressed while a protective sheet is sandwiched between the object to be compressed and the compression member.
[0027] According to this method, the fourth compression step is performed using a protective sheet. Therefore, even if pressure is applied to the negative electrode collector constituting the all-solid-state secondary battery, the damage of the negative electrode collector can be suppressed. In particular, when the negative electrode collector is a thinner foil-like material, the effect of suppressing the damage of the negative electrode collector is obtained.
[0028] According to a method for producing an all-solid-state secondary battery according to one aspect of the present invention, it is possible to provide a method for producing an all-solid-state secondary battery having excellent homogeneity. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 It is a cross-sectional view partially showing the structure of the all-solid-state secondary battery according to the first embodiment of the present invention.
[0030] Figure 2 This is a diagram for explaining a roll pressing method used for manufacturing the all-solid-state secondary battery according to the first embodiment of the present invention, and is a cross-sectional view showing a part of a roll pressing device.
[0031] Figure 3 It is a diagram for explaining the method for manufacturing the all-solid-state secondary battery according to the first embodiment of the present invention, and is a cross-sectional view partially showing the structure of a first compressed body obtained in the middle of the manufacturing.
[0032] Figure 4 It is a diagram for explaining the method for manufacturing the all-solid-state secondary battery according to the first embodiment of the present invention, and is a cross-sectional view partially showing the structure of a second compressed body obtained in the middle of the manufacturing.
[0033] Figure 5 It is a diagram for explaining the method for manufacturing the all-solid-state secondary battery according to the first embodiment of the present invention, and is a cross-sectional view partially showing the structure of a third compressed body obtained in the middle of the manufacturing.
[0034] Figure 6 This is a diagram for explaining a roll pressing method used for manufacturing an all-solid-state secondary battery according to a fourth embodiment of the present invention, and is a cross-sectional view showing a part of a roll pressing device. DETAILED DESCRIPTION
[0035] A method for manufacturing an all-solid-state secondary battery according to an embodiment of the present invention will be described with reference to the drawings.
[0036] In the drawings used in the following description, the scale of each member is appropriately changed so that the size of each member can be recognized.
[0037] The meaning of the term "laminating" is not limited to forming a layer on an object member, but also includes forming a layer in advance and transferring the layer to an object member.
[0038] <First embodiment>
[0039] <Structure of all-solid-state secondary battery>
[0040] like Figure 1 As shown, the all-solid secondary battery 1 includes a positive electrode collector 2, positive electrode layers 3U, 3L, electrolyte layers 4U, 4L, intermediate layers 5U, 5L, negative electrode layers 6U, 6L, and negative electrode collectors 7U, 7L.
[0041] The positive electrode current collector 2 has a first surface 2U and a second surface 2L opposite to the first surface 2U.
[0042] In the direction from the positive electrode collector 2 toward the negative electrode collector 7U, the positive electrode layer 3U, the electrolyte layer 4U, the intermediate layer 5U, the negative electrode layer 6U and the negative electrode collector 7U are sequentially stacked on the first surface 2U. The positive electrode layer 3U, the electrolyte layer 4U, the intermediate layer 5U, the negative electrode layer 6U and the negative electrode collector 7U are compressed relative to the positive electrode collector 2 to form a stacked compressed structure 1U.
[0043] In the direction from the positive electrode collector 2 toward the negative electrode collector 7L, the positive electrode layer 3L, the electrolyte layer 4L, the intermediate layer 5L, the negative electrode layer 6L and the negative electrode collector 7L are sequentially stacked on the second surface 2L. The positive electrode layer 3L, the electrolyte layer 4L, the intermediate layer 5L, the negative electrode layer 6L and the negative electrode collector 7L are compressed relative to the positive electrode collector 2 to form a stacked compressed structure 1L.
[0044] <Positive electrode collector>
[0045] The positive electrode collector 2 is a layer in contact with the positive electrode layers 3U and 3L. The material constituting the positive electrode collector 2 is not particularly limited, and any known material available as a positive electrode collector of a solid secondary battery can be used for the positive electrode collector 2. Examples of the positive electrode collector 2 include metal foils such as stainless steel (SUS) foil and aluminum (Al) foil.
[0046] <Positive electrode layer>
[0047] The positive electrode layers 3U and 3L are layers in contact with the electrolyte layers 4U and 4L, respectively. The positive electrode layers 3U and 3L are layers containing positive electrode active materials, respectively. The positive electrode active materials are not particularly limited, and known materials can be used as positive electrode active materials for solid-state secondary batteries. For example, LiCoO2, LiNiO2, NCM (Li (Ni x Co y Mn z )O2, (0<x<1, 0<y<1, 0<z<1, x+y+z=1)) and other ternary positive electrode materials, LiVO2, LiCrO2 and other layered positive electrode active material particles, LiMn2O4, Li(Ni 0.25 Mn 0.75 )2O4, LiCoMnO4, Li2NiMn3O8 and other spinel positive electrode active materials, LiCoPO4, LiMnPO4, LiFePO4 and other olivine positive electrode active materials, etc.
[0048] The positive electrode layers 3U and 3L may also contain solid electrolytes, conductive additives, adhesives, etc. in addition to the positive electrode active material. The solid electrolytes, conductive additives, adhesives, etc. are not particularly limited, and known materials can be applied as electrode materials for solid-state secondary batteries. An adhesive layer may also be laminated on the outer surface of the positive electrode layers 3U and 3L.
[0049] <Electrolyte layer>
[0050] The electrolyte layers 4U and 4L are layers in contact with the intermediate layers 5U and 5L, respectively. The electrolyte layers 4U and 4L are layers containing a solid electrolyte, respectively. The electrolyte layers 4U and 4L may contain a binder and the like in addition to the above.
[0051] The type of the solid electrolyte is not particularly limited, and examples of the solid electrolyte include sulfide-based solid electrolytes, oxide-based solid electrolytes, nitride-based solid electrolytes, and halide-based solid electrolytes.
[0052] The material of the adhesive is not particularly limited, and as the material of the adhesive, for example, polyvinylidene fluoride (PVdF), polymethyl methacrylate (PMMA), polyisobutylene (PIB), styrene-butadiene rubber (SBR), polyethylene-vinyl acetate copolymer (PEVA), nitrile rubber (NBR), hydrogenated nitrile rubber (HNBR) etc. can be cited. One of them can be used alone, or two or more can be used simultaneously.
[0053] <Middle layer>
[0054] The intermediate layers 5U and 5L are layers in contact with the negative electrode layers 6U and 6L, respectively. Examples of the material of the intermediate layers 5U and 5L include solid electrolytes, carbides, and binders. For example, SnC can be used as the carbide.
[0055] The intermediate layer 5U has at least one of a function of improving ion conductivity between the corresponding electrolyte layer 4U and the negative electrode layer 6U and a function of protecting the surface of the negative electrode layer 6U.
[0056] Likewise, the intermediate layer 5L has at least one of a function of improving ion conductivity between the corresponding electrolyte layer 4L and the negative electrode layer 6L and a function of protecting the surface of the negative electrode layer 6L.
[0057] <Negative electrode layer>
[0058] The negative electrode layers 6U and 6L are layers in contact with the negative electrode current collectors 7U and 7L, respectively. The negative electrode layers 6U and 6L are layers containing negative electrode active materials, respectively. The negative electrode active materials are not particularly limited, and known materials can be used as negative electrode active materials for solid-state secondary batteries. Examples of negative electrode active materials include lithium titanate (Li4Ti5O 12 ) and other lithium transition metal oxides, transition metal oxides such as TiO2, Nb2O3 and WO3, metal sulfides, metal nitrides, graphite, carbon materials such as soft carbon and hard carbon, silicon materials such as silicon monomers, silicon alloys, silicon compounds, as well as lithium metal, lithium alloys and metal indium.
[0059] The negative electrode layers 6U and 6L may contain, in addition to the negative electrode active material, a solid electrolyte, a conductive aid, a binder, etc. The solid electrolyte, conductive aid, binder, etc. are not particularly limited, and known substances can be used as electrode materials for solid secondary batteries.
[0060] <Negative electrode collector>
[0061] The negative electrode current collectors 7U and 7L each correspond to the outermost layer of the all-solid secondary battery 1. In other words, the negative electrode current collector 7U corresponds to the outermost layer of the stacked compressed structure 1U. The negative electrode current collector 7L corresponds to the outermost layer of the stacked compressed structure 1L.
[0062] The material of the negative electrode collectors 7U and 7L is not particularly limited, and known materials can be used as negative electrode collectors of solid secondary batteries. Examples of the negative electrode collectors include metal foils such as copper (Cu) foil, stainless steel (SUS) foil, and aluminum (Al) foil.
[0063] <Method for Manufacturing All-Solid State Secondary Battery According to First Embodiment>
[0064] Next, refer to Figure 1 to Figure 5A method for manufacturing the all-solid-state secondary battery 1 according to the first embodiment will be described.
[0065] The method for manufacturing the all-solid-state secondary battery 1 includes the following steps.
[0066] Step 1: Positive electrode layer forming process
[0067] Step 2: Electrolyte layer lamination process
[0068] Step 3: First compression process
[0069] Step 4: Intermediate layer lamination process
[0070] Step 5: Second compression process
[0071] Step 6: Negative electrode layer stacking process
[0072] Step 7: Third compression process
[0073] Step 8: Negative electrode current collector stacking process
[0074] Step 9: Fourth compression process
[0075] In the method for manufacturing the all-solid secondary battery 1, steps 1 to 9 are performed in sequence. In the first compression step, the second compression step, the third compression step, and the fourth compression step, a known compression step is performed. As an example of the compression step, in this embodiment, a roll pressing method is used.
[0076] <Roller pressing device>
[0077] Figure 2 It is a cross-sectional view showing a part of a roll pressing device for performing the roll pressing method.
[0078] The roller pressing device has a first roller R1 and a second roller R2 that are opposed to each other, and a delivery mechanism that is not shown. The first roller R1 can rotate counterclockwise. The second roller R2 can rotate clockwise. The delivery mechanism can deliver the compressed object 20 to the gap between the first roller R1 and the second roller R2 in the direction from the insertion portion 11 toward the discharge portion 12. The distance between the first roller R1 and the second roller R2 can be adjusted appropriately. In addition, the roller pressing device can appropriately adjust the compressive force applied to the compressed object 20. In the following description, the first roller R1 and the second roller R2 are sometimes simply referred to as "rollers R" without distinguishing between the first roller R1 and the second roller R2.
[0079] The first roller R1 and the second roller R2 are each an example of a compression member that compresses the compression target object.
[0080] <Roller pressing method>
[0081] The compressed object 20 is a laminate having a first layer 10A and a second layer 10B. Before being compressed, the compressed object 20 has a thickness h0. First, the delivery mechanism delivers the compressed object 20 to the gap between the first roller R1 and the second roller R2 through the insertion portion 11. As the first roller R1 and the second roller R2 rotate, the compressed object 20 moves from the insertion portion 11 toward the discharge portion 12. The compressed object 20 is compressed by the first roller R1 and the second roller R2, and the thickness of the compressed object 20 gradually decreases. The thickness of each of the first layer 10A and the second layer 10B constituting the compressed object 20 also gradually decreases. After being compressed, the compressed object 20 has a thickness h that is thinner than the thickness h0.
[0082] Next, steps 1 to 9 are described respectively.
[0083] <Step 1: Positive electrode layer forming process>
[0084] First, the positive electrode current collector 2 and the positive electrode layers 3U and 3L are prepared.
[0085] Next, the positive electrode layer 3U is stacked on the first surface 2U of the positive electrode current collector 2. The positive electrode layer 3L is stacked on the second surface 2L of the positive electrode current collector 2. Thus, a stacked body in which the positive electrode current collector 2 and the positive electrode layers 3U and 3L are stacked is obtained.
[0086] <Step 2: Electrolyte layer lamination process>
[0087] Next, the electrolyte layers 4U and 4L are prepared.
[0088] Next, the electrolyte layer 4U is stacked on the positive electrode layer 3U. The electrolyte layer 4L is stacked on the positive electrode layer 3L. Thus, a stacked body including the positive electrode current collector 2, the positive electrode layers 3U and 3L, and the electrolyte layers 4U and 4L is obtained.
[0089] It should be noted that in the electrolyte layer lamination step, the electrolyte layers 4U, 4L may be formed not only directly on the positive electrode layers 3U, 3L but also by transferring the electrolyte layers 4U, 4L formed separately in advance to the positive electrode layers 3U, 3L.
[0090] <Step 3: First compression step>
[0091] Next, use Figure 2 The roller pressing device shown in the figure compresses the laminated body obtained in the electrolyte layer lamination process. Specifically, as the compression object 20, the laminated body obtained in the electrolyte layer lamination process is inserted between the first roller R1 and the second roller R2. As the first roller R1 and the second roller R2 rotate, the laminated body is gradually compressed. As a result, Figure 3The first compressed body 1MA shown in FIG. In the first compression step, the pressure (first pressure) applied to the laminate by the first roller R1 and the second roller R2 is, for example, 300 MPa to 500 MPa.
[0092] <Step 4: Intermediate layer lamination process>
[0093] Next, the intermediate layers 5U and 5L are prepared.
[0094] Next, the intermediate layer 5U is stacked on the exposed surface of the electrolyte layer 4U in the first compressed body 1MA. The intermediate layer 5L is stacked on the exposed surface of the electrolyte layer 4L in the first compressed body 1MA. Thus, a stacked body is obtained in which the positive electrode collector 2, the positive electrode layers 3U, 3L, the electrolyte layers 4U, 4L, and the intermediate layers 5U, 5L are stacked.
[0095] <Step 5: Second compression step>
[0096] Next, use Figure 2 The roller pressing device shown in the figure compresses the laminated body obtained in the intermediate layer lamination process. Specifically, as the compression object 20, the laminated body obtained in the intermediate layer lamination process is inserted between the first roller R1 and the second roller R2. As the first roller R1 and the second roller R2 rotate, the laminated body is gradually compressed. As a result, Figure 4 The second compression body 1MB shown. In the second compression step, the pressure (second pressure) applied to the laminate by the first roller R1 and the second roller R2 is, for example, 700 MPa or more. Therefore, in the comparison between the first pressure and the second pressure, the second pressure is set higher than the first pressure.
[0097] <Step 6: Negative electrode layer stacking step>
[0098] Next, the negative electrode layers 6U and 6L are prepared.
[0099] Next, the negative electrode layer 6U is stacked on the exposed surface of the intermediate layer 5U in the second compressed body 1MB. The negative electrode layer 6L is stacked on the exposed surface of the intermediate layer 5L in the second compressed body 1MB. Thus, a stacked body is obtained in which the positive electrode collector 2, the positive electrode layers 3U, 3L, the electrolyte layers 4U, 4L, the intermediate layers 5U, 5L and the negative electrode layers 6U, 6L are stacked.
[0100] <Step 7: Third compression step>
[0101] Next, use Figure 2 The roller pressing device shown in the figure compresses the laminated body obtained in the negative electrode layer lamination process. Specifically, as the compression object 20, the laminated body obtained in the negative electrode layer lamination process is inserted between the first roller R1 and the second roller R2. As the first roller R1 and the second roller R2 rotate, the laminated body is gradually compressed. Thus, Figure 5The third compression body 1MC shown. In the third compression process, the pressure (third pressure) applied to the laminate by the first roller R1 and the second roller R2 is, for example, 400 MPa or less. Therefore, in the comparison between the second pressure and the third pressure, the second pressure is set higher than the third pressure. More preferably, in the comparison between the first pressure, the second pressure and the third pressure, the second pressure is set higher than the third pressure, and the first pressure is set higher than the third pressure.
[0102] <Step 8: Negative electrode current collector stacking step>
[0103] Next, negative electrode current collectors 7U and 7L are prepared.
[0104] Next, the negative electrode collector 7U is stacked on the exposed surface of the negative electrode layer 6U in the third compressed body 1MC. The negative electrode collector 7L is stacked on the exposed surface of the negative electrode layer 6L in the third compressed body 1MC. Thus, a stacked body is obtained in which the positive electrode collector 2, the positive electrode layers 3U, 3L, the electrolyte layers 4U, 4L, the intermediate layers 5U, 5L, the negative electrode collectors 7U, 7L, and the negative electrode collectors 7U, 7L are stacked.
[0105] <Step 9: Fourth compression step>
[0106] Next, use Figure 2 The roller pressing device shown compresses the laminated body obtained in the negative electrode current collector lamination process. Specifically, as the compression object 20, the laminated body obtained in the negative electrode current collector lamination process is inserted between the first roller R1 and the second roller R2. As the first roller R1 and the second roller R2 rotate, the laminated body is gradually compressed. Thus, Figure 1 The all-solid-state secondary battery 1 is shown.
[0107] <Effects>
[0108] According to the above method, the electrolyte layers 4U and 4L are flattened by performing the first compression step. Since the electrolyte layers 4U and 4L are flattened, even if the intermediate layers 5U and 5L are stacked on the electrolyte layers 4U and 4L and the second compression step is performed, the electrolyte layer 4U can be prevented from sinking into the intermediate layer 5U, and the electrolyte layer 4L can be prevented from sinking into the intermediate layer 5L.
[0109] By performing the second compression step, the positive electrode layers 3U and 3L and the intermediate layers 5U and 5L become dense, thereby preventing the electrolyte layer 4U from sinking into the intermediate layer 5U and preventing the electrolyte layer 4L from sinking into the intermediate layer 5L.
[0110] By performing the third compression step, the strength of the all-solid-state secondary battery 1 is improved. For example, in the use environment of the all-solid-state secondary battery 1, even if repeated loads such as compression and non-compression in the surface direction of the electrolyte layers 4U and 4L are generated in the all-solid-state secondary battery 1, the occurrence of damage caused by extension or rupture in the electrolyte layers 4U and 4L can be suppressed.
[0111] Furthermore, the smoothness of the interface between the electrolyte layer 4U and the intermediate layer 5U is improved, and the smoothness of the interface between the electrolyte layer 4L and the intermediate layer 5L is improved, so that the all-solid secondary battery 1 having excellent homogeneity can be realized.
[0112] The first compressed body 1MA includes the positive electrode current collector 2, the positive electrode layers 3U and 3L, and the electrolyte layers 4U and 4L. Even after the first compression step, the positive electrode current collector 2 can be prevented from being damaged in the first compressed body 1MA.
[0113] In addition, a positive electrode layer 3U is formed on the first surface 2U of the positive electrode collector 2. Similarly, a positive electrode layer 3L is formed on the second surface 2L of the positive electrode collector 2. That is, a structure in which positive electrode layers 3U and 3L are formed on both sides of the positive electrode collector 2 is obtained. In such a structure, even after the first compression process, the second compression process and the third compression process are performed, the restoring force of the positive electrode layer 3U generated on the first surface 2U and the restoring force of the positive electrode layer 3L generated on the second surface 2L offset each other. Therefore, in the whole of the all-solid-state secondary battery 1, the occurrence of warping is suppressed. Therefore, the flatness of the all-solid-state secondary battery 1 can be improved. In particular, when the roller pressing method is used in the first compression process, the second compression process and the third compression process, the difference in friction coefficient between the surface of the roller R and the surface of the laminate stacked on both sides of the positive electrode collector 2 can be reduced. Thus, the flatness of the all-solid-state secondary battery 1 can be improved.
[0114] Usually, the electrolyte layer is made of powder. Therefore, in the structure where the negative electrode layer directly joins the electrolyte layer, the bonding property between the negative electrode layer and the electrolyte layer is low. In contrast, according to this embodiment, the intermediate layer 5U is sandwiched between the negative electrode layer 6U and the electrolyte layer 4U. In addition, the intermediate layer 5L is sandwiched between the negative electrode layer 6L and the electrolyte layer 4L. In addition, the intermediate layers 5U and 5L respectively have a solid electrolyte, a carbide, and a binder.
[0115] Therefore, compared with a structure in which the electrolyte layer is directly bonded to the negative electrode layer, in a structure including the intermediate layers 5U and 5L, the bondability between the negative electrode layer 6U and the electrolyte layer 4U can be improved, and the bondability between the negative electrode layer 6L and the electrolyte layer 4L can be improved.
[0116] Furthermore, since the negative electrode current collector stacking step and the fourth compression step are performed, a structure in which the negative electrode current collectors 7U and 7L are stacked on the negative electrode layers 6U and 6L, respectively, can be obtained.
[0117] <Second embodiment>
[0118] Next, the all-solid-state secondary battery 1 according to the second embodiment will be described.
[0119] The second embodiment is different from the first embodiment in the structure of negative electrode layers 6U and 6L.
[0120] In the second embodiment, the same components as those in the first embodiment are denoted by the same reference numerals, and description thereof will be omitted or simplified.
[0121] <Negative electrode layer>
[0122] In the second embodiment, the negative electrode layer 6U has a negative electrode facing surface facing the intermediate layer 5U. The negative electrode layer 6L has a negative electrode facing surface facing the intermediate layer 5L.
[0123] <Method for manufacturing all-solid-state secondary battery according to second embodiment>
[0124] First, the above-mentioned steps 1 to 5 are performed in the same manner as in the first embodiment.
[0125] Next, before the negative electrode layer lamination step of step 6, the negative electrode facing surfaces of the negative electrode layers 6U and 6L are roughened. In the roughening, the surface roughness of the negative electrode facing surfaces is set to 20 μm or more.
[0126] After the roughening treatment is performed, the above-mentioned steps 6 to 9 are performed in the same manner as in the first embodiment.
[0127] <Effects>
[0128] According to this method, by roughening the negative electrode facing surface of the negative electrode layers 6U and 6L, a fine concavo-convex shape can be formed on the negative electrode facing surface. In this case, at the interface where the negative electrode facing surface contacts the intermediate layers 5U and 5L, the intermediate layers 5U and 5L easily enter the concavo-convex shape of the negative electrode facing surface. Therefore, the bonding property between the negative electrode layer 6U and the intermediate layer 5U can be improved, and the bonding property between the negative electrode layer 6L and the intermediate layer 5L can be improved.
[0129] In addition, by setting the surface roughness of the negative electrode opposing surface to be greater than 20 μm, the surface roughness of the negative electrode opposing surface of the negative electrode layers 6U and 6L can be fully ensured. In addition, the negative electrode opposing surface becomes a surface that is easily deformed. Therefore, when the negative electrode layers 6U and 6L are deformed in the third compression process, the stress generated between the negative electrode layer 6U and the intermediate layer 5U is absorbed, and the stress generated between the negative electrode layer 6L and the intermediate layer 5L is absorbed. Therefore, the cushioning property can be improved. Therefore, it is possible to suppress unexpected deformation, and it is possible to apply uniform pressure between the negative electrode layer 6U and the intermediate layer 5U, and it is possible to apply uniform pressure between the negative electrode layer 6L and the intermediate layer 5L. It is possible to improve the bonding property between the negative electrode layer 6U and the intermediate layer 5U, and it is possible to improve the bonding property between the negative electrode layer 6L and the intermediate layer 5L.
[0130] <Third embodiment>
[0131] Next, an all-solid-state secondary battery 1 according to a third embodiment will be described.
[0132] The third embodiment is different from the first embodiment in the structures of negative electrode layers 6U, 6L and negative electrode current collectors 7U, 7L.
[0133] In the third embodiment, the same components as those in the first embodiment are denoted by the same reference numerals, and description thereof will be omitted or simplified.
[0134] <Negative electrode layer>
[0135] In the third embodiment, the negative electrode layers 6U and 6L have both the function of the negative electrode layer and the function of the negative electrode collector. The negative electrode layers 6U and 6L are respectively equivalent to the outermost layer of the all-solid-state secondary battery 1. In other words, the negative electrode layer 6U is equivalent to the outermost layer of the stacked compressed structure 1U. The negative electrode layer 6L is equivalent to the outermost layer of the stacked compressed structure 1L.
[0136] The negative electrode layers 6U and 6L each have a structure in which a negative electrode active material layer and a negative electrode current collecting layer are stacked. The negative electrode active material layer contains the negative electrode active material described in the first embodiment. The negative electrode current collecting layer is a metal foil such as copper (Cu) foil, stainless steel (SUS) foil, and aluminum (Al) foil.
[0137] <Method for manufacturing all-solid-state secondary battery according to third embodiment>
[0138] First, the above-mentioned steps 1 to 6 are performed in the same manner as in the first embodiment.
[0139] In the negative electrode layer stacking process of step 6, the negative electrode layer 6U as a stack of negative electrode active material layer and negative electrode current collecting layer is stacked on the exposed surface of the intermediate layer 5U in the second compressed body 1MB. Similarly, the negative electrode layer 6L as a stack of negative electrode active material layer and negative electrode current collecting layer is stacked on the exposed surface of the intermediate layer 5L in the second compressed body 1MB.
[0140] Next, the above step 7 is performed. The third compressed body obtained by step 7 is Figure 1 The all-solid-state secondary battery 1 is shown.
[0141] <Effects>
[0142] According to this method, the negative electrode layers 6U and 6L are stacked bodies of negative electrode active material layers and negative electrode current collector layers, respectively. Therefore, it is not necessary to prepare the negative electrode current collectors 7U and 7L described in step 8, nor is it necessary to compress the stacked body including the negative electrode current collectors 7U and 7L described in step 9. Therefore, the number of steps for manufacturing the all-solid-state secondary battery 1 can be reduced.
[0143] <Fourth embodiment>
[0144] Next, a method for manufacturing the all-solid-state secondary battery according to the fourth embodiment will be described.
[0145] The fourth embodiment is different from the first to third embodiments described above in that a protective sheet is interposed between the compressed object 20 and the roller R.
[0146] In the fourth embodiment, the same components as those of the first to third embodiments are denoted by the same reference numerals, and description thereof will be omitted or simplified.
[0147] <Protective sheet>
[0148] In at least one of the first compression step, the second compression step, the third compression step and the fourth compression step, Figure 6 As shown, the protective sheet 30 is sandwiched between the compressed object 20 and the first roller R1. In other words, the protective sheet 30 is sandwiched between the first compression surface RF1 of the first roller R1 and the first compression target surface 20F of the compressed object 20. Similarly, the protective sheet 30 is sandwiched between the compressed object 20 and the second roller R2. In other words, the protective sheet 30 is sandwiched between the second compression surface RF2 of the second roller R2 and the second compression target surface 20S of the compressed object 20.
[0149] In this state, the first roller R1 and the second roller R2 compress the compression target 20 while rotating.
[0150] In the method for manufacturing the all-solid-state secondary battery of the above-described embodiment, the protective sheet 30 may be interposed between the positive electrode collector 2 and the roller R. The protective sheet 30 may be interposed between each of the negative electrode layers 6U, 6L and the roller R. In addition, the protective sheet 30 may be interposed between each of the negative electrode collectors 7U, 7L and the roller R.
[0151] The protective sheet 30 is separately provided from the positive electrode collector 2, the negative electrode layers 6U, 6L, and the negative electrode collectors 7U, 7L. In other words, the protective sheet 30 is not a component that constitutes the all-solid-state secondary battery. Therefore, after the above-mentioned multiple compression steps are completed, the protective sheet 30 is removed from the compressed object 20. It should be noted that the protective sheet 30 may also remain in a state of covering the compressed object 20 after one compression step is completed until the next compression step is performed.
[0152] It should be noted that in Figure 6 In the illustrated example, the protective sheets 30 are disposed on both surfaces of the object to be compressed 20 , but the protective sheet 30 may be disposed on at least one surface of the object to be compressed 20 .
[0153] As a material of the protective sheet 30, for example, metal foil and resin film are used. Examples of the metal foil include copper (Cu) foil, stainless steel (SUS) foil, and aluminum (Al) foil. Examples of the resin film include polyimide, polyetherimide, and fluororesin. The thickness of the protective sheet 30 is, for example, in the range of 5 to 150 μm.
[0154] <Effects>
[0155] According to this method, the same or similar effect as that obtained by the above-mentioned embodiment is obtained. In at least one of the first compression step, the second compression step, the third compression step, and the fourth compression step, even if pressure is applied to the positive electrode collector 2, the negative electrode layer 6U, 6L, and the negative electrode collector 7U, 7L, the use of the protective sheet 30 can suppress the damage of the positive electrode collector 2, the negative electrode layer 6U, 6L, and the negative electrode collector 7U, 7L.
[0156] In particular, when the positive electrode collector 2, negative electrode layers 6U, 6L, and negative electrode collectors 7U, 7L are made of thin foil-like materials, the positive electrode collector 2, negative electrode layers 6U, 6L, and negative electrode collectors 7U, 7L are effectively prevented from being damaged.
[0157] <Modification>
[0158] In the above embodiment, the stacked compressed structures 1U and 1L are formed on the first surface 2U and the second surface 2L of the positive electrode current collector 2, respectively. The stacked compressed structure may be formed on only one surface of the positive electrode current collector 2.
[0159] In the above-mentioned embodiment, the case where the roll pressing method is used as an example of the compression process is described. However, as long as the compression target 20 can be compressed using a compression member, a compression method other than the roll pressing method may be used.
[0160] Above, the embodiments of the present invention have been described, but it should be understood that these are illustrative embodiments of the present invention and should not be considered to limit the present invention. Additions, omissions, substitutions and other changes can be made without departing from the scope of the present invention. Therefore, the present invention should not be considered to be limited by the above description, but by the claims.
Claims
1. A method for manufacturing an all-solid-state secondary battery, in, The manufacturing method of the all-solid-state secondary battery comprises: a positive electrode layer forming step in which a positive electrode layer including a positive electrode active material is formed; an electrolyte layer laminating step, in which an electrolyte layer including a solid electrolyte is laminated on one surface of the positive electrode layer; a first compression step in which the positive electrode layer and the electrolyte layer are compressed at a first pressure to obtain a first compressed body; an intermediate layer laminating step of laminating an intermediate layer on the surface of the first compressed body where the electrolyte layer is exposed; a second compression step, in which the positive electrode layer, the electrolyte layer, and the intermediate layer are compressed at a second pressure to obtain a second compressed body; a negative electrode layer laminating step of laminating a negative electrode layer on a surface of the second compressed body where the intermediate layer is exposed; and a third compression step, in which the positive electrode layer, the electrolyte layer, the intermediate layer and the negative electrode layer are compressed at a third pressure to obtain a third compressed body; The positive electrode layer forming step, the electrolyte layer laminating step, the first compression step, the intermediate layer laminating step, the second compression step, the negative electrode layer laminating step and the third compression step are sequentially performed. The second pressure is higher than the first pressure and the third pressure, respectively.
2. The method for manufacturing an all-solid-state secondary battery according to claim 1, in, In the positive electrode layer forming step, the positive electrode layer is formed so as to be stacked on a positive electrode current collector.
3. The method for manufacturing an all-solid-state secondary battery according to claim 2, in, The positive electrode current collector has a first surface and a second surface opposite to the first surface, In the positive electrode layer forming step, the positive electrode layer is formed on each of the first surface and the second surface of the positive electrode current collector.
4. The method for manufacturing an all-solid-state secondary battery according to any one of claims 1 to 3, in, The intermediate layer comprises a solid electrolyte, a carbide and a binder.
5. The method for manufacturing an all-solid-state secondary battery according to any one of claims 1 to 3, in, The negative electrode layer has a negative electrode facing surface facing the intermediate layer, Before the negative electrode layer lamination step, the negative electrode facing surface is roughened. After the roughening treatment is performed, the negative electrode layer lamination step is performed.
6. The method for manufacturing an all-solid-state secondary battery according to claim 5, in, In the roughening treatment, the surface roughness of the negative electrode facing surface is set to 20 μm or more.
7. The method for manufacturing an all-solid-state secondary battery according to any one of claims 1 to 3, in, In the first compression step, the second compression step, and the third compression step, a compression member for compressing the compression object is used respectively. In at least one of the first compressing step, the second compressing step, and the third compressing step, the compressing member compresses the object to be compressed in a state where a protective sheet is interposed between the object to be compressed and the compressing member.
8. The method for manufacturing an all-solid-state secondary battery according to claim 1, in, The manufacturing method of the all-solid-state secondary battery comprises: a negative electrode current collector laminating step of laminating a negative electrode current collector on a surface of the third compressed body on which the negative electrode layer is exposed after the third compression step; and A fourth compression step, in which the positive electrode layer, the electrolyte layer, the intermediate layer, the negative electrode layer, and the negative electrode collector are compressed to obtain an all-solid secondary battery.
9. The method for manufacturing an all-solid-state secondary battery according to claim 8, in, In the fourth compression step, a compression member is used to compress the compression object. In the fourth compressing step, the compressing member compresses the object to be compressed in a state where a protective sheet is interposed between the object to be compressed and the compressing member.