Composite material and application thereof

The polyacrylonitrile-Prussian blue composite protective layer prepared by electrospinning solves the problems of zinc dendrites and hydrogen evolution reaction in aqueous zinc-ion batteries, achieves more uniform zinc ion deposition and higher corrosion resistance, and extends Improves battery life and Coulombic efficiency.

CN118738595APending Publication Date: 2024-10-01YANTAI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410923918.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

During the operation of aqueous zinc-ion batteries, problems such as the formation of zinc dendrites, electrolyte corrosion, and hydrogen evolution side reactions seriously affect the performance of the battery. Existing coating materials cannot completely inhibit side reactions and dendrite growth, resulting in battery life and shortening. Coulomb efficiency is low.

Method used

Composite materials are prepared by electrospinning using polyacrylonitrile and Prussian blue analogues to form a protective layer with a hydrophobic-zincphilic structure, which provides uniform nucleation sites through the channel structure of Prussian blue analogues and the chemical stability of polyacrylonitrile. Dots and water-resistant buffer layer inhibit zinc dendrite growth and hydrogen evolution reaction.

Benefits of technology

Significantly reduces the growth of zinc dendrites, increases hydrogen evolution overpotential, reduces corrosion of zinc electrodes, extends battery life and improves Coulombic efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118738595A_ABST
    Figure CN118738595A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of zinc ion batteries, and particularly relates to a composite material and application thereof. The preparation method of the composite material provided by the invention comprises the following steps: dissolving polyacrylonitrile and a Prussian blue analogue in an organic solvent, then carrying out electrostatic spinning on the surface of a matrix, and uncovering a film to obtain the composite material. According to the invention, polyacrylonitrile (PAN) and a Prussian blue analogue (PBAs) are uniformly sprayed and coated on the surface of a substrate through an electrostatic spinning method, and are combined to serve as a water-resistant buffer layer, so that Zn is isolated from an electrolyte, the hydrogen evolution overpotential is improved, the hydrogen evolution reaction is inhibited, and the corrosion and passivation of a zinc electrode are relieved. When the composite material provided by the invention is used as a protective layer of a zinc negative electrode, the service life and coulombic efficiency of a zinc ion battery can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of zinc ion batteries, and in particular relates to a composite material and application thereof. Background Art

[0002] Aqueous zinc-ion batteries have attracted widespread attention due to their low cost, high safety and environmental friendliness. However, problems such as zinc dendrite formation, electrolyte corrosion and hydrogen evolution side reactions during the operation of aqueous zinc-ion batteries have seriously affected the performance of the battery and limited its further development in applications.

[0003] At present, the main method to reduce the occurrence of side reactions and inhibit dendrite growth is to construct an interfacial protective layer on the surface of the zinc negative electrode; among them, surface coating is a simple and effective method. Commonly used coating materials include carbon materials (such as carbon nanotubes, carbon fibers), metal organic framework compounds (MOFs), metal compounds (such as calcium carbonate, titanium dioxide or zinc fluoride) and organic polymers (such as polyvinylidene fluoride (PVDF)). Carbon material coatings usually inhibit the growth of zinc dendrites by regulating the flux and electric field distribution of zinc ions, but cannot completely solve the problem of hydrogen evolution reaction (HER). The metal-ligand bonds in MOFs are prone to interact with water molecules, resulting in the decomposition and instability of the framework. Metal compound coatings can provide abundant zinc-philic sites and promote uniform zinc deposition, but their strength is insufficient and cannot completely isolate the zinc anode from the aqueous solution, and cannot completely inhibit side reactions. Although organic polymer coatings have potential in reducing side reactions and controlling zinc dendrites, their low conductivity often leads to large interfacial resistance and high polarization, thereby reducing the performance of zinc-based batteries at high current density. In addition, the coating prepared by traditional physical coating methods is often difficult to completely / uniformly cover the surface of the zinc negative electrode, and the active material and the protective layer cannot form good internal contact, resulting in high contact resistance and uneven electric field, further increasing the risk of zinc dendrites and corrosion. Summary of the invention

[0004] In view of this, the present invention provides a composite material and application thereof. The composite material provided by the present invention can inhibit the growth of zinc dendrites, inhibit the hydrogen evolution reaction, alleviate the corrosion and passivation of the zinc electrode, and improve the life and coulombic efficiency of the zinc ion battery.

[0005] In order to solve the above technical problems, the present invention provides a composite material, and a method for preparing the composite material comprises the following steps:

[0006] Polyacrylonitrile and Prussian blue analogs are dissolved in an organic solvent and then electrostatic spinning is performed on the surface of a substrate, and the film is peeled off to obtain the composite material.

[0007] Preferably, the dissolving comprises the following steps:

[0008] first dissolving polyacrylonitrile in an organic solvent to obtain a polyacrylonitrile solution;

[0009] The Prussian blue analog is secondly dissolved in the polyacrylonitrile solution to obtain a spinning solution.

[0010] Preferably, the relative molecular weight of the polyacrylonitrile is 50,000 to 150,000; the organic solvent includes N,N-dimethylformamide, dimethyl sulfoxide or N-methylpyrrolidone;

[0011] The mass ratio of polyacrylonitrile to the organic solvent is 8 to 10:100;

[0012] The mass ratio of the polyacrylonitrile to the Prussian blue analogue is 1:0.3-1.

[0013] Preferably, the first dissolution is performed under the condition of a first stirring, the temperature of the first stirring is 55 to 65° C., and the time is 1.5 to 2.5 hours.

[0014] Preferably, the second dissolving comprises a second stirring and a third stirring performed sequentially;

[0015] The second stirring temperature is 55-65°C and the time is 1.5-2.5h;

[0016] The temperature of the third stirring is 20-30° C., and the time is 6-12 hours.

[0017] Preferably, the electrospinning conditions include: voltage of 12 to 20 kV, distance of 8 to 20 cm, flow rate of 0.2 to 1.5 mL / h, and time of 20 min to 8 h.

[0018] Preferably, the substrate comprises zinc foil, copper foil or aluminum foil;

[0019] The composite material has a thickness of 5 to 700 μm.

[0020] The present invention also provides application of the composite material described in the above technical solution in an aqueous zinc ion battery.

[0021] Preferably, the composite material is used as a diaphragm of an aqueous zinc ion battery or a protective layer of a zinc negative electrode.

[0022] Preferably, when the composite material is used as a protective layer of a zinc negative electrode, the method for preparing a zinc negative electrode using the composite material as a protective layer comprises the following steps:

[0023] Polyacrylonitrile and Prussian blue analogs are dissolved in an organic solvent and then electrospun on the surface of zinc foil to obtain a zinc negative electrode with the composite material as a protective layer.

[0024] The present invention provides a composite material, and the preparation method of the composite material comprises the following steps: dissolving polyacrylonitrile and Prussian blue analogs in an organic solvent, and then electrospinning on the surface of a substrate, and removing the film to obtain the composite material. In the present invention, the composite material has a "hydrophobic-zincophilic" structure. The present invention uses an electrospinning method to evenly spray polyacrylonitrile (PAN) and Prussian blue analogs (PBAs) on the surface of a substrate. First, the larger channel size of the Prussian blue analog ensures the reversible insertion / removal of cations in three-dimensional space, and Zn 2+ There is a strong electrostatic interaction between them, which provides uniform nucleation sites for zinc ion deposition, significantly reduces the local current density, constructs a more uniform local electric field, reduces the size of zinc nucleation, and inhibits the growth of zinc dendrites; secondly, the good chemical stability of PAN can resist the influence of acid, alkali and oxidation conditions, and the cyanide in PAN provides electron pairs, interacts strongly with Zn ions, guides the coordination adsorption of zinc ions, and transfers Zn along long organic chains, providing stable nucleation sites for zinc ion transmission and deposition; finally, compared with Zn and PAN, the PBAs-PAN protective layer exhibits hydrophobic properties, reduces the number of water molecules hydrated with zinc ions, and the combination of the two acts as a water-resistant buffer layer to isolate Zn from the electrolyte, increase the hydrogen evolution overpotential, inhibit hydrogen evolution reaction, and alleviate the corrosion and passivation of the zinc electrode. Using the composite material provided by the present invention as a protective layer for the zinc negative electrode can improve the life and coulomb efficiency of the zinc ion battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is the XRD spectrum of zinc ferrocyanide prepared in Example 1;

[0026] Figure 2 This is the XRD spectrum of nickel ferrocyanide prepared in Example 2;

[0027] Figure 3 The XRD spectrum of the FeHCF-PAN / Zn electrode prepared in Example 1, wherein a is the overall XRD spectrum, and b is a local enlarged view with a peak position of 16.5 to 25°;

[0028] Figure 4 is the infrared spectrum of FeZnHCF-PAN in Example 3;

[0029] Figure 5 is the SEM image of FeZnHCF-PAN in Example 3;

[0030] Figure 6 The water contact angle test results of the electrodes prepared in Example 1 and Comparative Examples 1-2 are shown in Figure 1, wherein a is the result of the water contact angle of Comparative Example 2, b is the result of the water contact angle of Comparative Example 1, and c is the result of the water contact angle of Example 1;

[0031] Figure 7 The Tafel plots of the symmetrical batteries prepared in Example 1 and Comparative Examples 1-2;

[0032] Figure 8 The CA diagram of a symmetrical battery assembled from electrodes prepared in Example 1 and Comparative Examples 1-2;

[0033] Fig. 9 XRD spectra of the electrodes of the batteries prepared in Example 1 and Comparative Examples 1-2 after 100 cycles;

[0034] Fig.10 The SEM images of the zinc negative electrodes of the symmetrical batteries prepared in Example 1 and Comparative Examples 1-2 after 100 cycles, wherein a is the SEM image of Comparative Example 2, b is the SEM image of Comparative Example 1, and c is the SEM image of Example 1;

[0035] Fig.11 Graph showing the cycle stability of a symmetrical battery prepared from the FeZnHCF-PAN / Zn electrode prepared in Example 1;

[0036] Fig.12 This is a cycle stability diagram of a zinc symmetric battery prepared using the FeZnHCF-PAN separator prepared in Example 3;

[0037] Fig.13 Graph showing the cycle stability of a symmetrical battery prepared from the PAN / Zn electrode prepared in Comparative Example 1;

[0038] Fig.14 This is the cycling stability diagram of the symmetrical battery prepared using the Zn electrode of Comparative Example 2. DETAILED DESCRIPTION

[0039] The present invention provides a composite material, and a method for preparing the composite material comprises the following steps:

[0040] Polyacrylonitrile and Prussian blue analogs are dissolved in an organic solvent and then electrostatic spinning is performed on the surface of a substrate, and the film is peeled off to obtain the composite material.

[0041] In the present invention, the dissolving preferably comprises the following steps:

[0042] first dissolving polyacrylonitrile in an organic solvent to obtain a polyacrylonitrile solution;

[0043] The Prussian blue analog is secondly dissolved in the polyacrylonitrile solution to obtain a spinning solution.

[0044] The present invention first dissolves polyacrylonitrile in an organic solvent to obtain a polyacrylonitrile solution. In the present invention, the relative molecular weight of the polyacrylonitrile (PAN) is preferably 50,000 to 150,000; the organic solvent preferably includes N,N-dimethylformamide (DMF), dimethyl sulfoxide (DMSO) or N-methylpyrrolidone (NMP), and more preferably N,N-dimethylformamide. In the present invention, the mass ratio of the polyacrylonitrile and the organic solvent is preferably 8 to 10:100, and more preferably 9 to 10:100. In the present invention, the first dissolution is preferably carried out under the condition of the first stirring, and the temperature of the first stirring is preferably 55 to 65°C, and more preferably 60°C; the time of the first stirring is preferably 1.5 to 2.5h, and more preferably 2h. The present invention has no special limitation on the rotation speed of the first stirring, as long as it can be completely dissolved.

[0045] After obtaining the polyacrylonitrile solution, the present invention dissolves the Prussian blue analogue in the polyacrylonitrile solution for the second time to obtain a spinning solution. In the present invention, the Prussian blue analogue preferably includes zinc ferrocyanide, nickel ferrocyanide, cobalt ferrocyanide or zinc ferrocyanide, more preferably zinc ferrocyanide or nickel ferrocyanide. In the present invention, the Prussian blue analogue (PBAs) is preferably synthesized by a traditional coprecipitation method. In the present invention, the preparation method of the Prussian blue analogue preferably includes the following steps: adding potassium ferrocyanide solution and metal hydrochloride solution dropwise to a sodium chloride solution, mixing, and then separating the solid and liquid to obtain the Prussian blue analogue. In the present invention, the molar concentration of the potassium ferrocyanide solution is preferably 0.08-0.12 mol / L, more preferably 0.1 mol / L. In the present invention, the metal hydrochloride solution preferably includes one or two of ferric chloride solution, zinc chloride solution, cobalt chloride solution, nickel chloride solution and zinc chloride solution, more preferably a mixed solution of ferric chloride and zinc chloride or nickel chloride solution; the total molar concentration of metal ions in the metal hydrochloride solution is preferably 0.08-0.12 mol / L, more preferably 0.1 mol / L. In the present invention, the molar concentration of the sodium chloride solution is preferably 0.8-1.2 mol / L, more preferably 1 mol / L. In the present invention, the volume ratio of the potassium ferricyanide solution, the metal hydrochloride solution and the sodium chloride solution is preferably 0.8-1.2:0.8-1.2:1, more preferably 1:1:1. The present invention has no special requirements for the rate of the dripping, as long as it is added dropwise. In the present invention, the mixing is preferably carried out under stirring, and the stirring temperature is preferably 25-35°C, more preferably 30°C; the stirring speed is preferably 200-800r / min, more preferably 400r / min; the stirring time is preferably 16-20h, more preferably 18h. In the present invention, the solid-liquid separation is preferably filtration, and the filtration is preferably vacuum filtration. In the present invention, the solid obtained by solid-liquid separation is preferably washed with water and ethanol in sequence and then dried. In the present invention, the water for washing is preferably deionized water, and the number of times of washing is preferably 2-3 times; the solvent for ethanol washing is preferably anhydrous ethanol, and the number of times of ethanol washing is preferably 2-4 times, more preferably 3 times. The present invention has no special requirements for the drying, as long as the moisture on the surface of the solid can be removed.

[0046] In the present invention, the mass ratio of the polyacrylonitrile and the Prussian blue analogs (PBAs) is preferably 1:0.3-1, more preferably 1:0.6-0.7. In the present invention, the second dissolution preferably includes a second stirring and a third stirring performed sequentially. In the present invention, the temperature of the second stirring is preferably 55-65°C, more preferably 60°C; the time of the second stirring is preferably 1.5-2.5h, more preferably 2h. In the present invention, the temperature of the third stirring is preferably 20-30°C, more preferably 23-25°C; the time of the third stirring is preferably 6-12h, more preferably 8-12h.

[0047] In the present invention, the substrate preferably includes zinc foil, copper foil or aluminum foil, more preferably zinc foil.

[0048] The present invention preferably further comprises: cleaning the substrate before electrospinning. The present invention has no special requirements for the cleaning, and a conventional cleaning method in the art can be used.

[0049] In the present invention, the conditions for electrospinning preferably include: voltage of 12-20 kV, distance of 8-20 cm, flow rate of 0.2-1.5 mL / h, time of 20 min-8 h, more preferably: voltage of 16 kV, distance of 10 cm, flow rate of 0.2-0.5 mL / h, time of 1-6 h. The present invention preferably limits the electrospinning time according to the required thickness of the composite material.

[0050] In the present invention, after the electrospinning, the process preferably further comprises: drying the electrospinning product. The present invention has no special limitation on the drying process, and conventional methods in the art can be used.

[0051] In the present invention, the thickness of the composite material is preferably 5 to 700 μm, more preferably 5 to 15 μm or 200 to 700 μm. In the present invention, when the thickness of the composite material is 5 to 15 μm, it is preferably used as a protective layer of the negative electrode; when the thickness of the composite material is 200 to 700 μm, it is preferably used as a separator of a zinc ion battery.

[0052] The present invention also provides application of the composite material described in the above technical solution in an aqueous zinc ion battery.

[0053] In the present invention, the composite material is preferably used in an aqueous zinc ion battery as a diaphragm or a protective layer of a zinc negative electrode of the aqueous zinc ion battery. In the present invention, when the composite material is used as a protective layer of a zinc negative electrode, the preparation method of a zinc negative electrode using the composite material as a protective layer comprises the following steps:

[0054] Polyacrylonitrile and Prussian blue analogs are dissolved in an organic solvent and then electrospun on the surface of zinc foil to obtain a zinc negative electrode with the composite material as a protective layer.

[0055] In the present invention, the preparation method of the zinc negative electrode with the composite material as the protective layer is consistent with the preparation method of the above-mentioned composite material, the difference is that zinc foil is used as the substrate, and the film is not peeled off after electrospinning, and the thickness of the protective layer formed by the composite material is 5 to 15 μm.

[0056] In the present invention, when the composite material is used as a separator, it is preferred to use a ZnSO4 solution as an electrolyte and a polished Zn sheet as two electrodes of a symmetrical battery to prepare a battery.

[0057] In order to further illustrate the present invention, the technical solutions provided by the present invention are described in detail below in conjunction with embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0058] Example 1

[0059] Preparation of zinc electrode with composite material as protective layer

[0060] 100 mL of a 0.1 mol / L K3Fe(CN)6 solution and 100 mL of a mixed solution of 0.08 mol / L FeCl3 and 0.02 mol / L ZnCl2 were added dropwise to 100 mL of a 1 mol / L NaCl aqueous solution, stirred at 400 r / min for 18 h at 30°C, and then vacuum filtered; the solid obtained by vacuum filtration was washed with deionized water and anhydrous ethanol for 3 times, and then dried to obtain ferrozinc ferrocyanide (FeZnHCF);

[0061] 0.75 g of polyacrylonitrile with a relative molecular mass of 50,000 and 7.5 g of DMF were heated and stirred at 60° C. for 2 h to obtain a polyacrylonitrile solution;

[0062] After adding 0.5 g of zinc ferrocyanide to the polyacrylonitrile solution, stirring was continued at 60° C. for 2 h, and then at 25° C. for 12 h to obtain a spinning solution;

[0063] The spinning solution was placed in a plastic syringe and electrospun for 40 min on the cleaned zinc foil surface at a voltage of 16 kV, a distance of 10 cm and a flow rate of 0.2 mL / h. After drying, a zinc electrode with a composite material as a protective layer was obtained, which was recorded as FeZnHCF-PAN / Zn electrode.

[0064] Example 2

[0065] Preparation of zinc electrode with composite material as protective layer

[0066] 100 mL of a 0.1 mol / L K3Fe(CN)6 solution and 100 mL of a 0.1 mol / L NiCl2 solution were added dropwise to 100 mL of a 1 mol / L NaCl aqueous solution, stirred at 400 r / min for 18 h at 30° C., and then vacuum filtered; the solid obtained by vacuum filtration was washed three times with deionized water and anhydrous ethanol, and then dried to obtain nickel ferrocyanide (NiHCF);

[0067] 0.75 g of polyacrylonitrile with a relative molecular mass of 150,000 and 9.38 g of DMF were heated at 55° C. and stirred for 2.5 h to obtain a polyacrylonitrile solution;

[0068] After adding 0.45 g of nickel ferrocyanide to the polyacrylonitrile solution, the mixture was stirred at 60° C. for 2 h, and then stirred at 25° C. for 12 h to obtain a spinning solution;

[0069] The spinning solution was placed in a plastic syringe and electrospun for 40 min on the cleaned zinc foil surface at a voltage of 16 kV, a distance of 10 cm and a flow rate of 1.5 mL / h. After drying, a zinc electrode with the composite material as a protective layer was obtained, which was recorded as NiHCF-PAN / Zn electrode.

[0070] Example 3

[0071] Preparation of composite materials as separators for zinc-ion batteries

[0072] Prepare a spinning solution according to the method of Example 1;

[0073] The spinning solution was placed in a plastic syringe and electrospun for 6 h on the cleaned aluminum foil surface at a voltage of 16 kV, a distance of 10 cm and a flow rate of 0.5 mL / h. After drying, the film was peeled off to obtain a composite material, which was recorded as FeZnHCF-PAN.

[0074] Comparative Example 1

[0075] 0.75 g of polyacrylonitrile with a relative molecular mass of 50,000 and 7.5 g of DMF were heated and stirred at 60° C. for 2 h, and then stirred at 25° C. for 12 h to obtain a polyacrylonitrile solution;

[0076] The polyacrylonitrile solution was placed in a plastic syringe and electrospun for 40 min on the cleaned zinc foil surface at a voltage of 16 kV, a distance of 10 cm and a flow rate of 2 mL / h. After drying, a zinc electrode with polyacrylonitrile as a protective layer was obtained, which was recorded as PAN / Zn electrode.

[0077] Comparative Example 2

[0078] A pure zinc electrode was used as a comparative example.

[0079] The ferrocyanide zinc ferrocyanide prepared in Example 1 was subjected to X-ray diffraction detection to obtain an XRD spectrum, as shown in FIG. Figure 1 As shown. Figure 1 It can be seen that the iron-zinc Prussian blue material was successfully synthesized.

[0080] The nickel ferrocyanide prepared in Example 2 was subjected to X-ray diffraction detection to obtain an XRD spectrum, as shown in FIG. Figure 2 As shown. Figure 2 It can be seen that nickel ferrocyanide was successfully synthesized.

[0081] The FeZnHCF-PAN / Zn electrode prepared in Example 1 was subjected to X-ray diffraction detection to obtain an XRD spectrum. Figure 3 As shown; a is the overall XRD spectrum, b is a local enlarged view with a peak position of 16.5-25°. Figure 3 It can be seen from a that 36°, 39°, 43°, 54°, 70° and 71° are characteristic peaks of zinc. Figure 3 The characteristic peak of Prussian blue can be seen in b).

[0082] The FeZnHCF-PAN in Example 3 was subjected to infrared spectroscopy analysis to obtain an infrared spectrum, as shown in FIG. Figure 4 As shown. Figure 4 It can be seen that at 2942cm -1 The absorption peak at 2098 cm is the stretching vibration of the CH bond of PAN, while the absorption peak at 2098 cm -1 The absorption peak at is the stretching vibration of the C≡N bond. The FTIR graph proves that both C≡N and CH functional groups exist in the composite material prepared in Example 3, which explains the successful construction of the composite fiber membrane by polyacrylonitrile and zinc ferrocyanide without changing the original structure of the material.

[0083] The polyacrylonitrile and ferric zinc ferrocyanide composite material (FeZnHCF-PAN) in Example 3 was tested by transmission electron microscopy to obtain a TEM image, as shown in FIG. Figure 5 As shown. Figure 5 It can be seen that the ferric zinc ferrocyanide prepared in Example 3 is in the form of densely arranged nanoparticles with a particle size of about 50 nm, and is successfully encapsulated in the polyacrylonitrile in the composite material.

[0084] The water contact angle test was performed on the electrodes prepared in Example 1 and Comparative Examples 1-2, and the results were as follows: Figure 6 As shown, a is the result of the water contact angle of comparative example 2, b is the result of the water contact angle of comparative example 1, and c is the result of the water contact angle of embodiment 1. Figure 6It can be seen that the protective layer (composite material) in the electrode prepared in Example 1 is non-wettable with water, which also reflects the hydrophobicity of the material caused by the intrinsic characteristics of the rich carbon skeleton in the polyacrylonitrile and the composite material. This hydrophobicity can reduce the contact area between the water in the electrolyte and the metal zinc sheet, thereby improving the corrosion resistance of the zinc negative electrode and the ability to inhibit the hydrogen evolution reaction.

[0085] Using ZnSO4 solution as the electrolyte, symmetrical cells were assembled using the electrodes prepared in Example 1 and Comparative Examples 1-2, and the electrochemical performance was tested. Figure 7 The Tafel plots of Example 1 and Comparative Examples 1 to 2 are shown in FIG. Figure 7 From the Tafel spectrum, it can be seen that although the corrosion voltage of comparative example 1 (-0.985V) is not much different from that of comparative example 2 (-0.987V), the corrosion current of comparative example 1 (1.13mA / cm 2 ) is higher than the corrosion current of Comparative Example 2 (2.23 mA / cm 2 ), which indicates that the protective layer does have a certain corrosion resistance. Compared with pure zinc, the corrosion voltage (-0.977V) of the electrode of Example 1 is the most right-shifted, and the corrosion current is the lowest, which means that the electrode prepared by spinning Example 1 can effectively inhibit the hydrogen evolution reaction, has excellent corrosion resistance, and can improve the stability of aqueous zinc ion batteries.

[0086] The batteries prepared in Example 1 and Comparative Examples 1-2 were subjected to a chronoamperometric test to obtain a CA graph, as shown in FIG. Figure 8 As shown. Figure 8 It can be seen that when an overpotential of -150 mV is applied, the current density of the pure zinc electrode shows a trend of continuous increase within 150 s, indicating that there is a long-term 2D diffusion, and the result of 2D diffusion will lead to Zn 2+ Due to the lateral diffusion, zinc ions will be preferentially deposited at positions with lower nucleation potential, resulting in disordered growth of dendrites, affecting its cyclic stability. The 2D diffusion in Comparative Example 1 was completed within 20s, and the current density of Example 1 showed a relatively stable trend, which shows that Comparative Example 1 and Example 1 began stable 3D diffusion afterwards. The result of this diffusion is different from that of 2D diffusion. On the contrary, 3D diffusion is conducive to zinc deposition around the initial position of zinc ions, increasing the number of nucleations, thereby inducing uniform deposition of zinc ions and reducing the growth of zinc dendrites. By comparing the CA spectra, it is shown that the composite material of polyacrylonitrile and Prussian blue can effectively regulate zinc ion deposition, reduce the growth of zinc dendrites, and achieve a synergistic protective effect on the zinc negative electrode.

[0087] After the batteries prepared in Example 1 and Comparative Examples 1-2 were cycled for 100 cycles, XRD morphology characterization test was performed on the electrodes to obtain XRD spectra, as shown in FIG. Fig. 9 As shown. Fig. 9 It can be seen that more Zn4SO4(OH)6·xH2O by-products are generated on the bare zinc surface, while the by-products of polyacrylonitrile and composite material protective layers are significantly reduced, which shows that the protective layer has corrosion resistance and can effectively inhibit the generation of negative electrode side reactions; this is consistent with the results of the Tafel test.

[0088] After the batteries prepared in Example 1 and Comparative Examples 1-2 were cycled for 100 cycles, Zn electroplating / stripping was performed on the negative electrode sheets, and the morphology and phase of the zinc deposits were observed by scanning electron microscopy. Fig.10 The SEM images of the zinc negative electrode of the symmetrical battery prepared in Example 1 and Comparative Examples 1-2 after 100 cycles, wherein a is the SEM image of Comparative Example 2, b is the SEM image of Comparative Example 1, and c is the SEM image of Example 1. Fig.10 It can be seen that there are obvious protrusions on the surface of the electrode of Comparative Example 2, which may come from zinc dendrites and side reactions occurring on the surface of the zinc negative electrode. In contrast, no zinc dendrites are generated on the negative electrode surface of Comparative Example 1, and zinc agglomerates on the PAN surface, while no zinc dendrites and zinc agglomerates are generated on the negative electrode surface of Example 1. This is related to its nanoporous framework, which can effectively regulate zinc ion deposition, reduce 2D diffusion and dendrite growth, which intuitively shows the optimization and regulation of the composite spinning fiber membrane on zinc deposition behavior, thereby achieving a synergistic protection effect on the zinc negative electrode.

[0089] The battery cycle stability diagrams prepared in Examples 1 and 3 and Comparative Examples 1 to 2 are compared to obtain a symmetrical battery cycle stability diagram as shown in FIG. Figures 11 to 14 As shown; Fig.11 The symmetrical cell prepared from the FeZnHCF-PAN / Zn electrode prepared in Example 1 was 2 、0.5mAh / cm 2 Cyclic stability diagram under conditions, Fig.12 The symmetrical battery prepared by using FeZnHCF-PAN prepared in Example 3 as the separator and Zn as the electrode was 2 、1mAh / cm 2 Cyclic stability diagram under conditions, Fig.13 The symmetrical battery prepared from the PAN / Zn electrode prepared in Comparative Example 1 was 2 、0.5mAh / cm 2 Cyclic stability diagram under conditions, Fig.14 The symmetrical battery prepared from the Zn electrode of Comparative Example 2 is 0.5 mA / cm 2 、0.5mAh / cm 2 Cyclic stability diagram under conditions. Figures 11 to 13It can be seen that the Zn symmetric battery in Comparative Example 2 has a cliff-like voltage drop after 450 hours of cycling, which may be due to a short circuit in the battery; the PAN / Zn symmetric battery in Comparative Example 1 can last for 745 hours, indicating that the battery protected by the PAN spun fiber membrane is more stable than the pure zinc battery. The polarization curve of the FeZnHCF-PAN / Zn symmetric battery in Example 1 has been stable, and can reach a cycle time of more than 3000 hours, showing excellent cycle stability, which can greatly improve the service life of the battery. At high current density, the FeZnHCF-PAN in Example 3 can still be stably cycled for more than 1000 hours as a diaphragm.

[0090] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. People can also obtain other embodiments based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.

Claims

1. A composite material, characterized in that: The preparation method of the composite material comprises the following steps: Polyacrylonitrile and Prussian blue analogs are dissolved in an organic solvent and then electrostatic spinning is performed on the surface of a substrate, and the film is peeled off to obtain the composite material.

2. The composite material according to claim 1, characterized in that: The dissolution comprises the following steps: first dissolving polyacrylonitrile in an organic solvent to obtain a polyacrylonitrile solution; The Prussian blue analog is secondly dissolved in the polyacrylonitrile solution to obtain a spinning solution.

3. The composite material according to claim 1 or 2, characterized in that: The relative molecular weight of the polyacrylonitrile is 50,000 to 150,000; the organic solvent includes N,N-dimethylformamide, dimethyl sulfoxide or N-methylpyrrolidone; The mass ratio of polyacrylonitrile to the organic solvent is 8 to 10:100; The mass ratio of the polyacrylonitrile to the Prussian blue analogue is 1:0.3-1.

4. The composite material according to claim 2, characterized in that: The first dissolution is performed under the condition of a first stirring, wherein the temperature of the first stirring is 55 to 65° C. and the time is 1.5 to 2.5 hours.

5. The composite material according to claim 2, characterized in that: The second dissolving comprises a second stirring and a third stirring performed sequentially; The second stirring temperature is 55-65°C and the time is 1.5-2.5h; The temperature of the third stirring is 20-30° C., and the time is 6-12 hours.

6. The composite material according to claim 1 or 2, characterized in that: The electrospinning conditions include: voltage of 12 to 20 kV, distance of 8 to 20 cm, flow rate of 0.2 to 1.5 mL / h, and time of 20 min to 8 h.

7. The composite material according to claim 6, characterized in that: The substrate includes zinc foil, copper foil or aluminum foil; The composite material has a thickness of 5 to 700 μm.

8. Use of the composite material according to any one of claims 1 to 7 in an aqueous zinc ion battery.

9. The use according to claim 8, characterized in that: The composite material is used as a diaphragm of an aqueous zinc ion battery or a protective layer of a zinc negative electrode.

10. The use according to claim 8, characterized in that: When the composite material is used as a protective layer of a zinc negative electrode, the method for preparing a zinc negative electrode using the composite material as a protective layer comprises the following steps: Polyacrylonitrile and Prussian blue analogs are dissolved in an organic solvent and then electrospun on the surface of zinc foil to obtain a zinc negative electrode with the composite material as a protective layer.