High-thermal-conductivity silicon carbide composite heat sink structure and preparation method and application thereof

By depositing a thermally conductive buffer film layer and a thermally conductive film layer on the silicon carbide substrate of the semiconductor laser, and using Ge-Ag-Sn solder, the existing technology solves the problem of high cost of heat sink structural materials, low thermal conductivity and easy diamond film layer. solve the problem of cracks and achieve efficient heat dissipation and high yield.

CN118739010AActive Publication Date: 2024-10-01SHIJIAZHUANG TUNGSTEN IRIDIUM ELECTRONIC TECHNOLOGY CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410711417.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-04
Publication Date
2024-10-01
Estimated Expiration
2044-06-04

AI Technical Summary

Technical Problem

Existing semiconductor laser heat sink structural materials are expensive, have low thermal conductivity, and the diamond film layer is prone to cracks or collapse during the welding process, which cannot meet the heat dissipation needs of high-power lasers.

Method used

A stepped heat transfer heat sink structure with silicon carbide as the substrate was designed. By sequentially depositing a thermal conductive buffer film layer and a thermal conductive film layer on the silicon carbide substrate, aniline-modified graphene and boron nitride-modified graphite were used. olefin material is used to improve thermal conductivity, and Ge-Ag-Sn solder is used to replace gold-tin solder to reduce stress effects.

Benefits of technology

It significantly improves the heat dissipation efficiency of the semiconductor laser, reduces the cost, avoids cracks or collapse of the diamond film layer during the welding process, and greatly improves the device yield.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of semiconductor laser material preparation, and particularly discloses a high-thermal-conductivity silicon carbide composite heat sink structure and a preparation method and application thereof. The invention designs a stepped heat transfer heat sink structure with silicon carbide as a substrate. The heat conduction buffer film layer and the heat conduction film layer are sequentially deposited and grown on the silicon carbide substrate, the silicon carbide substrate with low heat conductivity and the diamond heat conduction film layer with high heat conductivity are connected through the heat conduction buffer film layer, a new heat dissipation channel is introduced, and the heat dissipation efficiency of the device is remarkably improved. In addition, the invention further designs a novel metal solder, and the situation that the diamond film layer is cracked or cracked in the welding process is avoided. The semiconductor laser heat sink structure effectively solves the problems that in the prior art, materials of a semiconductor laser heat sink structure are high in cost and low in heat conductivity and cannot meet device requirements, and cracks and even crack when a chip is welded to a diamond film layer, and the yield of semiconductor laser devices is greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of semiconductor laser material preparation, and specifically discloses a high thermal conductivity silicon carbide composite heat sink structure and a preparation method and application thereof. Background Art

[0002] Semiconductor lasers have the advantages of high electro-optical conversion efficiency, small size, long life, adjustable wavelength and wide range, etc., which makes them widely used in the fields of communication industry, laser pumping, medical laser surgery, industrial cutting manufacturing, military defense, etc. However, with the rapid development of semiconductor laser theory, materials, and preparation technology, the performance parameters of semiconductor lasers such as output power, beam quality, and working life are also constantly improving, and the requirements for semiconductor laser packaging technology are also increasing.

[0003] Although semiconductor lasers have high electro-optical conversion efficiency, they still generate a lot of waste heat when working for a long time. If this waste heat cannot be dissipated in time, it will seriously affect the performance of the semiconductor laser. Especially for high-density packaged lasers such as horizontal or vertical stacked arrays, the temperature gradient caused by the repeated pulse power supply will easily cause heat accumulation inside the device. When the accumulation is serious, it will cause thermal stress and deformation of the chip, seriously reducing the beam quality and pumping efficiency of high-power semiconductor lasers. Therefore, the heat dissipation problem of semiconductor lasers has become a hot topic in the field of semiconductor laser research.

[0004] In the prior art, researchers have proposed many solutions to this problem. At present, high-power semiconductor lasers all use a conduction cooling method with hard solder packaging, that is, the laser chip is first packaged on a transition heat sink with hard solder to form a COS structure, and then the COS is packaged on a copper heat sink with a higher thermal conductivity coefficient to complete the secondary packaging, where the transition heat sink is located between the chip and the copper heat sink, and plays the dual role of heat dissipation transition and stress transition. The ideal transition heat sink material should have a high thermal conductivity and be able to match the expansion of the laser chip. The heat sink material with the highest thermal conductivity reported is diamond, and its thermal conductivity can reach 1200W / (mK)-2200W / (mK), but the cost of diamond heat sink materials is too expensive and the operating requirements are harsh, so it cannot be mass-produced. However, the thermal conductivity of common silicon carbide is poor, only about 390W / (mK), which cannot meet the needs of devices. There are also methods that combine the two, depositing diamond on a silicon carbide substrate or depositing silicon carbide on a diamond substrate to make a composite heat sink material, but the two are prone to high thermal resistance, and inevitably there will be a mismatch between the thermal expansion coefficient of the heat sink material and the semiconductor laser, resulting in poor device performance. In addition, the existing metal solder is mostly gold-tin solder, which is expensive and has high stress, which will produce stress on the diamond film layer, causing cracks or even collapse of the diamond film layer during the welding process.

[0005] Based on this, developing a heat sink material with high thermal conductivity, stable performance and the ability to improve the performance of semiconductor lasers is of great significance to the development of semiconductor lasers. Summary of the invention

[0006] In view of the problems in the prior art that the materials of the semiconductor laser heat sink structure are expensive, the thermal conductivity is low and cannot meet the device requirements, and the diamond film layer will crack or even collapse when welding the chip, the present invention provides a high thermal conductivity silicon carbide composite heat sink structure and its preparation method and application. The present invention designs a stepped heat transfer heat sink structure with silicon carbide as the substrate. Among them, a thermally conductive buffer film layer and a thermally conductive film layer are sequentially deposited and grown on the silicon carbide substrate, and the thermally conductive buffer film layer is used to connect the silicon carbide substrate with low thermal conductivity and the diamond thermally conductive film layer with high thermal conductivity, thereby introducing a new heat dissipation channel and significantly improving the heat dissipation efficiency of the device. In addition, the present invention also designs a new metal solder to avoid the situation where the diamond film layer cracks or collapses during the welding process.

[0007] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0008] The first aspect of the present invention provides a high thermal conductivity silicon carbide composite heat sink structure, which comprises, from bottom to top, a silicon carbide substrate, a thermal conductive buffer film layer, a thermal conductive film layer and a metal welding layer;

[0009] The material of the thermal conductive buffer film layer is a mixture of aniline-modified graphene and boron nitride-modified graphene;

[0010] The heat-conducting film layer is a diamond film layer;

[0011] The solder of the metal welding layer is Ge-Ag-Sn solder.

[0012] Compared with the prior art, the present invention deposits and grows a thermally conductive buffer film layer and a thermally conductive film layer on a silicon carbide substrate in sequence, wherein the thermally conductive buffer film layer is made of aniline-modified graphene and boron nitride-modified graphene, and the thermally conductive film layer is made of diamond. Since the thermal conductivity of diamond is as high as 2200W / (mK), and the thermal conductivity of silicon carbide is only 390W / (mK) at most, the thermal conductivity of the two is very different. If the diamond film is grown directly on the silicon carbide substrate, although the cost can be saved to a certain extent, the problem of mismatch between the thermal expansion coefficient of the heat sink material and the semiconductor chip is prone to occur, resulting in unsatisfactory heat dissipation effect. Therefore, the inventor added a thermally conductive buffer film layer between the silicon carbide substrate and the diamond thermally conductive film layer. The thermally conductive buffer film layer is made of aniline-modified graphene and boron nitride-modified graphene as raw materials. Graphene itself has good thermal conductivity, but a single graphene material may have a large thermal resistance at the interface in contact with the silicon carbide substrate, which limits the efficiency of heat conduction. Therefore, the present invention modifies it, using the N atoms in aniline to form a delocalized p-π conjugation with graphene, further improving the electronic heat transfer capacity of the graphene material; and the boron nitride-modified graphene can serve as a bridge for the graphene sheet layer, assisting it in forming a complete thermal conductive network and improving the thermal conductivity efficiency of the graphene; the two work together to greatly improve the thermal conductivity efficiency of the graphene material. The introduction of the thermally conductive buffer film layer adds a new heat dissipation channel, thereby further improving the heat dissipation efficiency of the heat sink structure.

[0013] In addition, since the commonly used gold-tin solder has excessive stress, it is easy to cause cracks or collapse of the diamond thermal conductive film layer when welding the chip. The present invention uses Ge-Ag-Sn solder. Compared with gold-tin solder, the cost of Ge-Ag-Sn solder is lower, and it can provide sufficient wetting properties for the composite heat sink structure and the semiconductor chip to form a metallurgical bond. More importantly, Ge-Ag-Sn solder can reduce the thermal stress caused by the mismatch of thermal expansion coefficients between the chip and the heat sink, effectively avoiding the collapse of the diamond thermal conductive film layer caused by excessive stress, and greatly improving the yield of semiconductor laser devices.

[0014] Preferably, the mass ratio of the aniline-modified graphene to the boron nitride-modified graphene is 1:2-1:3.

[0015] Preferably, the thickness of the thermally conductive buffer film is 5 μm-10 μm.

[0016] Preferably, the thickness of the thermal conductive film layer is 20 μm-30 μm.

[0017] Preferably, the thickness of the metal welding layer is 3 μm-5 μm.

[0018] Preferably, the preparation method of aniline-modified graphene comprises the following steps: dispersing graphene in an alcohol solvent, adding aniline and a promoter, and refluxing the reaction for 18h-24h under an inert atmosphere to obtain aniline-modified graphene.

[0019] Aniline-modified graphene is a process that utilizes the N atoms of the amino groups in aniline to form graphene in anisotropic 2 There are lone electron pairs in the orbital, which can conjugate with the large π bond on graphene to form a delocalized p-π conjugated system, becoming a weak charge transfer complex, which helps the electron heat transfer. In addition, since the N atom has two movable lone electrons, the heat transfer performance is even better.

[0020] Further preferably, the mass ratio of graphene to aniline is 0.1:1-0.3:3.5.

[0021] Further preferably, the mass volume ratio of the aniline to the accelerator is 1 g:3 mL-1.5 g:5 mL.

[0022] Further preferably, the mass volume ratio of the graphene to the alcohol solution is 0.1 g:130 mL-0.1 g:200 mL.

[0023] More preferably, the accelerator is isoamyl nitrite.

[0024] Preferably, the method for preparing the boron nitride modified graphene comprises the following steps:

[0025] S1. Dispersing boron nitride in organic alcohol, ultrasonicating, and centrifuging to obtain a pretreated boron nitride mixed solution;

[0026] S2, mixing the graphene and the cross-linking agent solution evenly, centrifuging at high speed, and discarding the supernatant to obtain pretreated graphene;

[0027] S3. Adding organic alcohol and the pretreated boron nitride mixed solution to the pretreated graphene at 60° C.-80° C., mixing evenly, centrifuging, filtering, and freeze-drying to obtain boron nitride modified graphene.

[0028] The present invention utilizes boron nitride nanosheets on the surface of boron nitride-modified graphene to act as bridges between graphene sheets, assisting them in forming a complete heat conduction network, thereby improving the thermal conductivity of the graphene material.

[0029] More preferably, the organic alcohol is isopropanol.

[0030] Further preferably, the mass volume ratio of the boron nitride and the organic alcohol is 1g:80mL-2g:250mL.

[0031] Further preferably, in S1, the rotation speed of the centrifugal treatment is 2000 rpm-3500 rpm, and the time of the centrifugal treatment is 20 min-30 min.

[0032] Further preferably, in S2, the cross-linking agent solution is an aqueous solution of polydiallyl dimethyl ammonium chloride with a mass concentration of 1%-2.5%.

[0033] Further preferably, in S2, the mass volume ratio of the graphene and the cross-linking agent solution is 0.1 g:100 mL-0.5 g:500 mL.

[0034] Further preferably, in S2, the rotation speed of the high-speed centrifugation is 8000 rpm-12000 rpm, and the time of the high-speed centrifugation is 10 min-15 min.

[0035] Further preferably, in S3, the mass volume ratio of the pretreated graphene and the organic alcohol is 0.5g:30mL-50mL.

[0036] Further preferably, in S3, the centrifugal speed is 1500 rpm-2500 rpm, and the centrifugal time is 20 min-30 min.

[0037] Preferably, the mass percentage of each component in the Ge-Ag-Sn solder is as follows: 10%-15% Ge, 5%-10% Ag and the balance Sn.

[0038] A second aspect of the present invention provides a method for preparing the high thermal conductivity silicon carbide composite heat sink structure, comprising the following steps:

[0039] Step 1: using plasma enhanced chemical vapor deposition technology to deposit a thermally conductive buffer film layer on the surface of a clean and dry silicon carbide substrate to obtain a first processed heat sink;

[0040] Step 2: placing the first treated heat sink in a microwave plasma chemical vapor deposition chamber to grow a thermal conductive film layer to obtain a second treated heat sink;

[0041] Step three: prepare a metal welding layer on the surface of the second treated heat sink by electron beam evaporation to obtain the high thermal conductivity silicon carbide composite heat sink structure.

[0042] Preferably, in step 1, the substrate temperature for depositing the thermally conductive buffer film layer is 430° C.-480° C., the substrate bias voltage is 90V-110V, and the radio frequency power is 100-110W.

[0043] Preferably, in step 2, the microwave power for growing the thermal conductive film layer is 2kW-4kW, the deposition temperature is 850°C-920°C; the hydrogen flow rate is 350sccm-450sccm, and the methane flow rate is 22sccm-25sccm.

[0044] Preferably, in step 3, the process parameters of the electron beam evaporation method are: vacuum degree is 1.0×10 -3 Pa-5.0×10 -3 Pa, evaporation distance is 40cm-60cm, electron gun voltage is 8kV-12kV, electron beam spot shape is circular, and evaporation rate is 0.2nm / s-0.8nm / s.

[0045] A third aspect of the present invention provides an application of the high thermal conductivity silicon carbide composite heat sink structure in a semiconductor laser.

[0046] In summary, the present invention designs a stepped heat transfer heat sink structure with silicon carbide as the substrate. The present invention deposits and grows a thermally conductive buffer film layer and a thermally conductive film layer on the silicon carbide substrate in sequence, thereby improving the thermal conductivity of the heat sink structure. The high thermal conductivity silicon carbide composite heat sink structure provided by the present invention effectively solves the problems of the high cost of materials of semiconductor laser heat sink structures in the prior art, low thermal conductivity that cannot meet device requirements, and cracks or even collapse of the diamond film layer when welding chips, and provides new materials for the preparation of semiconductor lasers.

[0047] The present invention designs a step-type heat transfer heat sink structure with silicon carbide as the substrate. Among them, a thermally conductive buffer film layer and a thermally conductive film layer are sequentially deposited and grown on the silicon carbide substrate, and the silicon carbide substrate with low thermal conductivity and the diamond thermally conductive film layer with high thermal conductivity are connected by the thermally conductive buffer film layer. The different intrinsic thermal conductivities of the materials of each layer are used to achieve the purpose of step-type heat dissipation, which is more conducive to the heat dissipation of the device. In addition, the present invention also designs a new metal solder, which can not only provide sufficient wetting performance between the heat sink structure and the chip, but also reduce the thermal stress caused by the mismatch of thermal expansion coefficients between the chip and the heat sink, and avoid the situation where the diamond film layer cracks or collapses during the welding process. The technical solution of the present invention effectively solves the problems of the high cost of materials of the semiconductor laser heat sink structure in the prior art, the low thermal conductivity that cannot meet the device requirements, and the cracks or even collapse of the diamond film layer when welding the chip, greatly improves the yield rate of semiconductor laser devices, and provides new preparation materials and theoretical basis for efficient heat dissipation of semiconductor lasers. DETAILED DESCRIPTION

[0048] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0049] The preparation methods of aniline-modified graphene and boron nitride-modified graphene used in the following examples and comparative examples are as follows:

[0050] Preparation method of aniline-modified graphene:

[0051] 0.1 g of graphene was dispersed in 150 mL of anhydrous ethanol, and 1.5 g of aniline and 5 mL of isoamyl nitrite were added. The mixture was refluxed for 22 h under an inert atmosphere, cooled to room temperature, filtered, and the solid filtrate was washed three times with anhydrous ethanol and purified with a 0.5 μm dialysis membrane to obtain aniline-modified graphene.

[0052] Preparation method of boron nitride modified graphene

[0053] S1. Disperse 1.5 g of boron nitride in 150 mL of isopropanol, perform ultrasonic treatment, and centrifuge at 2500 rpm for 25 min to obtain a pretreated boron nitride mixed solution;

[0054] S2, 0.3 g of graphene and 150 mL of 1% polydiallyl dimethyl ammonium chloride solution were mixed evenly, stirred for 8 h, and then centrifuged at a speed of 10000 rpm for 10 min, and the supernatant was discarded to obtain pretreated graphene;

[0055] S3. At 70° C., add 20 mL of isopropanol and the pretreated boron nitride mixed solution to the pretreated graphene, mix well, centrifuge at 2000 rpm for 20 min, filter, and freeze-dry to obtain boron nitride modified graphene.

[0056] Example 1

[0057] This embodiment provides a high thermal conductivity silicon carbide composite heat sink structure, which specifically includes the following contents:

[0058] Step 1: Deposit a thermally conductive buffer film layer with a thickness of 8 μm on the surface of a clean and dry silicon carbide substrate using plasma enhanced chemical vapor deposition technology; obtain a first processed heat sink; wherein the substrate temperature for depositing the thermally conductive buffer film layer is 450° C., the substrate bias voltage is 100 V, and the radio frequency power is 100 W;

[0059] Step 2: placing the first treated heat sink in a microwave plasma chemical vapor deposition chamber to grow a diamond film layer with a thickness of 25 μm; obtaining a second treated heat sink; wherein the microwave power for growing the thermal conductive film layer is 3 kW, the deposition temperature is 900° C., the hydrogen flow rate is 400 sccm, and the methane flow rate is 24 sccm;

[0060] Step 3: Prepare a metal welding layer with a thickness of 4 μm on the surface of the second treated heat sink by electron beam evaporation to obtain the high thermal conductivity silicon carbide composite heat sink structure; wherein the vacuum degree is 3.0×10 -3 Pa, the evaporation distance is 55 cm, the electron gun voltage is 10 kV, the electron beam spot shape is circular, and the evaporation rate is 0.6 nm / s.

[0061] Wherein, the material of the thermal conductive buffer film layer is aniline-modified graphene and boron nitride-modified graphene in a mass ratio of 1:2;

[0062] The solder of the metal welding layer is Ge-Ag-Sn solder, and the mass percentage of each component is as follows: 12% Ge, 5% Ag and 83% Sn.

[0063] Example 2

[0064] This embodiment provides a high thermal conductivity silicon carbide composite heat sink structure, which specifically includes the following contents:

[0065] Step 1: Deposit a 10 μm thick thermally conductive buffer film layer on the surface of a clean and dry silicon carbide substrate using plasma enhanced chemical vapor deposition technology; obtain a first processed heat sink; wherein the substrate temperature for depositing the thermally conductive buffer film layer is 435° C., the substrate bias voltage is 105 V, and the radio frequency power is 100 W;

[0066] Step 2: placing the first treated heat sink in a microwave plasma chemical vapor deposition chamber to grow a diamond film layer with a thickness of 30 μm; obtaining a second treated heat sink; wherein the microwave power for growing the thermal conductive film layer is 3 kW, the deposition temperature is 870°C; the hydrogen flow rate is 420 sccm, and the methane flow rate is 25 sccm;

[0067] Step 3: Prepare a metal welding layer with a thickness of 3 μm on the surface of the second treated heat sink by electron beam evaporation to obtain the high thermal conductivity silicon carbide composite heat sink structure; wherein the vacuum degree is 1.0×10 -3 Pa, the evaporation distance is 50 cm, the electron gun voltage is 12 kV, the electron beam spot shape is circular, and the evaporation rate is 0.5 nm / s.

[0068] Wherein, the material of the thermal conductive buffer film layer is aniline-modified graphene and boron nitride-modified graphene in a mass ratio of 1:3;

[0069] The solder of the metal welding layer is Ge-Ag-Sn solder, and the mass percentage of each component is as follows: 11% Ge, 8% Ag and 81% Sn.

[0070] Example 3

[0071] This embodiment provides a high thermal conductivity silicon carbide composite heat sink structure, which specifically includes the following contents:

[0072] Step 1: Deposit a 5 μm thick thermally conductive buffer film layer on the surface of a clean and dry silicon carbide substrate using plasma enhanced chemical vapor deposition technology to obtain a first processed heat sink; wherein the substrate temperature for depositing the thermally conductive buffer film layer is 450° C., the substrate bias voltage is 100 V, and the radio frequency power is 100 W;

[0073] Step 2: placing the first treated heat sink in a microwave plasma chemical vapor deposition chamber to grow a diamond film layer with a thickness of 20 μm; obtaining a second treated heat sink; wherein the microwave power for growing the thermal conductive film layer is 3 kW, the deposition temperature is 850°C; the hydrogen flow rate is 450 sccm, and the methane flow rate is 23 sccm;

[0074] Step 3: Prepare a metal welding layer with a thickness of 4 μm on the surface of the second treated heat sink by electron beam evaporation to obtain the high thermal conductivity silicon carbide composite heat sink structure; wherein the vacuum degree is 4.0×10 -3 Pa, the evaporation distance is 60 cm, the electron gun voltage is 12 kV, the electron beam spot shape is circular, and the evaporation rate is 0.8 nm / s.

[0075] Wherein, the material of the thermal conductive buffer film layer is aniline-modified graphene and boron nitride-modified graphene in a mass ratio of 1:2.5;

[0076] The solder of the metal welding layer is Ge-Ag-Sn solder, and the mass percentage of each component is as follows: 15% Ge, 5% Ag and 80% Sn.

[0077] Comparative Example 1

[0078] This comparative example provides a high thermal conductivity silicon carbide composite heat sink structure, which is different from Example 1 in that there is no thermal conductive buffer film layer, and specifically includes the following contents:

[0079] Step 1: Place a clean and dry silicon carbide substrate in a microwave plasma chemical vapor deposition chamber to grow a diamond film layer with a thickness of 25 μm; obtain a second processed heat sink; wherein the microwave power for growing the thermal conductive film layer is 3 kW, the deposition temperature is 900°C; the hydrogen flow rate is 400 sccm, and the methane flow rate is 24 sccm;

[0080] Step 2: Prepare a metal welding layer with a thickness of 4 μm on the surface of the second treated heat sink by electron beam evaporation to obtain the high thermal conductivity silicon carbide composite heat sink structure; wherein the vacuum degree is 3.0×10 -3 Pa, the evaporation distance is 55 cm, the electron gun voltage is 10 kV, the electron beam spot shape is circular, and the evaporation rate is 0.6 nm / s.

[0081] The solder of the metal welding layer is Ge-Ag-Sn solder, and the mass percentage of each component is as follows: 12% Ge, 5% Ag and 83% Sn.

[0082] Comparative Example 2

[0083] This comparative example provides a high thermal conductivity silicon carbide composite heat sink structure, which is different from Example 1 in that the material of the thermal conductive buffer film layer is an aniline-modified graphene layer, specifically including the following contents:

[0084] Step 1: Deposit a layer of aniline-modified graphene with a thickness of 8 μm on the surface of a clean and dry silicon carbide substrate using plasma enhanced chemical vapor deposition technology; obtain a first treated heat sink; wherein the substrate temperature for depositing the thermal conductive buffer film layer is 450° C., the substrate bias voltage is 100 V, and the radio frequency power is 100 W;

[0085] Step 2: placing the first treated heat sink in a microwave plasma chemical vapor deposition chamber to grow a diamond film layer with a thickness of 25 μm; obtaining a second treated heat sink; wherein the microwave power for growing the thermal conductive film layer is 3 kW, the deposition temperature is 900° C., the hydrogen flow rate is 400 sccm, and the methane flow rate is 24 sccm;

[0086] Step 3: Prepare a metal welding layer with a thickness of 4 μm on the surface of the second treated heat sink by electron beam evaporation to obtain the high thermal conductivity silicon carbide composite heat sink structure; wherein the vacuum degree is 3.0×10 -3 Pa, the evaporation distance is 55 cm, the electron gun voltage is 10 kV, the electron beam spot shape is circular, and the evaporation rate is 0.6 nm / s.

[0087] The solder of the metal welding layer is Ge-Ag-Sn solder, and the mass percentage of each component is as follows: 12% Ge, 5% Ag and 83% Sn.

[0088] Comparative Example 3

[0089] This comparative example provides a high thermal conductivity silicon carbide composite heat sink structure, which is different from Example 1 in that the material of the thermal conductive buffer film layer is a boron nitride modified graphene layer, specifically including the following contents:

[0090] Step 1: Deposit a layer of boron nitride modified graphene layer with a thickness of 8 μm on the surface of a clean and dry silicon carbide substrate using plasma enhanced chemical vapor deposition technology; obtain a first treated heat sink; wherein the substrate temperature for depositing the thermal conductive buffer film layer is 450° C., the substrate bias voltage is 100 V, and the radio frequency power is 100 W;

[0091] Step 2: placing the first treated heat sink in a microwave plasma chemical vapor deposition chamber to grow a diamond film layer with a thickness of 25 μm; obtaining a second treated heat sink; wherein the microwave power for growing the thermal conductive film layer is 3 kW, the deposition temperature is 900° C., the hydrogen flow rate is 400 sccm, and the methane flow rate is 24 sccm;

[0092] Step 3: Prepare a metal welding layer with a thickness of 4 μm on the surface of the second treated heat sink by electron beam evaporation to obtain the high thermal conductivity silicon carbide composite heat sink structure; wherein the vacuum degree is 3.0×10 -3 Pa, the evaporation distance is 55 cm, the electron gun voltage is 10 kV, the electron beam spot shape is circular, and the evaporation rate is 0.6 nm / s.

[0093] The solder of the metal welding layer is Ge-Ag-Sn solder, and the mass percentage of each component is as follows: 12% Ge, 5% Ag and 83% Sn.

[0094] Comparative Example 4

[0095] This comparative example provides a high thermal conductivity silicon carbide composite heat sink structure, which is different from Example 1 in that the raw material of the metal welding layer is AuSn solder, specifically including the following contents:

[0096] Step 1: Deposit a thermally conductive buffer film layer with a thickness of 8 μm on the surface of a clean and dry silicon carbide substrate using plasma enhanced chemical vapor deposition technology; obtain a first processed heat sink; wherein the substrate temperature for depositing the thermally conductive buffer film layer is 450° C., the substrate bias voltage is 100 V, and the radio frequency power is 100 W;

[0097] Step 2: placing the first treated heat sink in a microwave plasma chemical vapor deposition chamber to grow a diamond film layer with a thickness of 25 μm; obtaining a second treated heat sink; wherein the microwave power for growing the thermal conductive film layer is 3 kW, the deposition temperature is 900° C., the hydrogen flow rate is 400 sccm, and the methane flow rate is 24 sccm;

[0098] Step 3: Prepare a metal welding layer with a thickness of 4 μm on the surface of the second treated heat sink by electron beam evaporation to obtain the high thermal conductivity silicon carbide composite heat sink structure; wherein the vacuum degree is 3.0×10 -3Pa, the evaporation distance is 55 cm, the electron gun voltage is 10 kV, the electron beam spot shape is circular, and the evaporation rate is 0.6 nm / s.

[0099] The material of the thermal conductive buffer film layer is aniline-modified graphene and boron nitride-modified graphene in a mass ratio of 1:2.

[0100] The solder of the metal welding layer is AuSn solder, and the mass percentage of each component is as follows: 80% Au and 20% Sn.

[0101] To further demonstrate the technical effect of the present invention, the present invention uses a thermal conductivity meter from German C-Therm to test the thermal conductivity of the high thermal conductivity silicon carbide composite heat sink structure obtained in Examples 1-3 and Comparative Examples 1-4; the present invention also counts the device yield rate of using the high thermal conductivity silicon carbide composite heat sink structure obtained in Examples 1-3 and Comparative Examples 1-4 to prepare semiconductor lasers, and the results are shown in Table 1.

[0102] Table 1 Thermal conductivity and yield test results

[0103] project Thermal conductivity W / (mK) Device yield (%) Example 1 987 99.7 Example 2 976 99.4 Example 3 943 99.6 Comparative Example 1 634 98.4 Comparative Example 2 792 98.9 Comparative Example 3 801 99.1 Comparative Example 4 923 70.3

[0104] According to Table 1, the thermal conductivity of the high thermal conductivity silicon carbide composite heat sink structure provided by the present invention can be as high as 987W / (mK), which is much higher than the thermal conductivity of the silicon carbide substrate alone, and the composite heat sink structure provided by the present invention does not require the expensive cost of depositing all diamond film layers. Moreover, the present application uses stress-interleaved metal solder to avoid excessively high scrap rates of the device, providing new materials for high thermal conductivity semiconductor lasers.

[0105] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modification, equivalent substitution or improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A high thermal conductivity silicon carbide composite heat sink structure, characterized in that: From bottom to top, it includes a silicon carbide substrate, a thermal conductive buffer film layer, a thermal conductive film layer and a metal welding layer; The material of the thermal conductive buffer film layer is a mixture of aniline-modified graphene and boron nitride-modified graphene; The heat-conducting film layer is a diamond film layer; The solder of the metal welding layer is Ge-Ag-Sn solder.

2. The high thermal conductivity silicon carbide composite heat sink structure according to claim 1, characterized in that: The mass ratio of the aniline-modified graphene to the boron nitride-modified graphene is 1:2-1:3; and / or The thickness of the thermally conductive buffer film is 5 μm-10 μm; and / or The thickness of the thermal conductive film layer is 20 μm-30 μm; and / or The thickness of the metal welding layer is 3 μm-5 μm.

3. The high thermal conductivity silicon carbide composite heat sink structure according to claim 1, characterized in that: The preparation method of aniline-modified graphene comprises the following steps: dispersing graphene in an alcohol solvent, adding aniline and a promoter, and performing a reflux reaction for 18 hours to 24 hours under an inert atmosphere to obtain aniline-modified graphene.

4. The high thermal conductivity silicon carbide composite heat sink structure according to claim 3, characterized in that: The mass ratio of graphene to aniline is 0.1:1-0.3:3.5; and / or The mass volume ratio of aniline to accelerator is 1g:3mL-1.5g:5mL; and / or The mass volume ratio of the graphene to the alcohol solution is 0.1 g:130 mL-0.1 g:200 mL; and / or The accelerator is isoamyl nitrite.

5. The high thermal conductivity silicon carbide composite heat sink structure according to claim 1, characterized in that: The preparation method of the boron nitride modified graphene comprises the following steps: S1. Dispersing boron nitride in organic alcohol, ultrasonicating, and centrifuging to obtain a pretreated boron nitride mixed solution; S2, mixing the graphene and the cross-linking agent solution evenly, centrifuging at high speed, and discarding the supernatant to obtain pretreated graphene; S3. Adding organic alcohol and the pretreated boron nitride mixed solution to the pretreated graphene at 60° C.-80° C., mixing evenly, centrifuging, filtering, and freeze-drying to obtain boron nitride modified graphene.

6. The high thermal conductivity silicon carbide composite heat sink structure according to claim 5, characterized in that: The organic alcohol is isopropanol; and / or The mass volume ratio of the boron nitride to the organic alcohol is 1g:80mL-2g:250mL; and / or In S1, the rotation speed of the centrifugal treatment is 2000 rpm-3500 rpm, and the time of the centrifugal treatment is 20 min-30 min; and / or In S2, the cross-linking agent solution is a polydiallyl dimethyl ammonium chloride aqueous solution with a mass concentration of 1% to 2.5%; and / or In S2, the mass volume ratio of the graphene and the cross-linking agent solution is 0.1 g: 100 mL-0.5 g: 500 mL; and / or In S2, the rotation speed of the high-speed centrifugation is 8000 rpm-12000 rpm, and the time of the high-speed centrifugation is 10 min-15 min; and / or In S3, the mass volume ratio of the pretreated graphene and the organic alcohol is 0.1 g:10 mL-0.5 g:50 mL; and / or In S3, the centrifugal speed is 1500rpm-2500rpm, and the centrifugal time is 20min-30min.

7. The high thermal conductivity silicon carbide composite heat sink structure according to claim 1, characterized in that: The mass percentage of each component in the Ge-Ag-Sn solder is as follows: 10%-15% of Ge, 5%-10% of Ag and the balance of Sn.

8. A method for preparing a high thermal conductivity silicon carbide composite heat sink structure according to any one of claims 1 to 7, characterized in that: The steps include: Step 1: using plasma enhanced chemical vapor deposition technology to deposit a thermally conductive buffer film layer on the surface of a clean and dry silicon carbide substrate to obtain a first processed heat sink; Step 2: placing the first treated heat sink in a microwave plasma chemical vapor deposition chamber to grow a thermally conductive film layer to obtain a second treated heat sink; Step three: prepare a metal welding layer on the surface of the second treated heat sink by electron beam evaporation to obtain the high thermal conductivity silicon carbide composite heat sink structure.

9. The method for preparing a high thermal conductivity silicon carbide composite heat sink structure according to claim 8, characterized in that: In step 1, the substrate temperature for depositing the thermal conductive buffer film layer is 430° C.-480° C., the substrate bias voltage is 90V-110V, and the RF power is 100-110W; and / or In step 2, the microwave power for growing the thermal conductive film layer is 2kW-4kW, the pressure is 25kPa-30kPa, the deposition temperature is 850°C-920°C; the hydrogen flow rate is 350sccm-450sccm, and the methane flow rate is 22sccm-25sccm; and / or In step 3, the process parameters of the electron beam evaporation method are: vacuum degree is 1.0×10 -3 Pa-5.0×10 -3 Pa, evaporation distance is 40cm-60cm, electron gun voltage is 8kV-12kV, electron beam spot shape is circular, and evaporation rate is 0.2nm / s-0.8nm / s.

10. Use of the high thermal conductivity silicon carbide composite heat sink structure according to any one of claims 1 to 7 in a semiconductor laser.

Citation Information

Patent Citations

  • Boron nitride / graphene composite heat-conducting silicone grease and preparation method thereof

    CN105400202A

  • Preparation method of high-thermal-conductivity filler for thermally conductive polymer material

    CN110819018A

  • Preparation method of gallium nitride epitaxial structure

    CN114262937A

  • Graphene-based composite heat-conducting film and production process thereof

    CN116836430A

  • Semiconductor laser provided with diamond heat dissipating part

    JP1999026887A