EMI (Electro-Magnetic Interference) shielding film and preparation process

By adopting a specific stacked structure and material combination in the EMI shielding film, including aluminum-doped zinc oxide, indium tin oxide and nickel chromium layers, the problem of increased resistance caused by the aging of the EMI shielding film is solved, achieving efficient electromagnetic interference shielding and stability. sex.

CN118741996APending Publication Date: 2024-10-01ZHEJIANG RIJIU NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410908062.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The existing EMI shielding film ages after long-term use, resulting in an increase in resistance, weakening the shielding effect, and making it difficult to achieve both aging resistance and low resistance.

Method used

The EMI shielding film adopts a laminated structure, including a base material layer and a base layer composed of a first conductive layer, a silicon-aluminum mixed layer, a second conductive layer, a shielding layer and an anti-oxidation layer. The silicon-aluminum molar ratio in the silicon-aluminum mixed layer is 85 -98:15-2, the conductive layer uses aluminum-doped zinc oxide, indium tin oxide and silver layers, and the anti-oxidation layer is a nickel-chromium layer. The thickness and uniformity of the film layer are controlled by magnetron sputtering coating technology.

Benefits of technology

It achieves good aging resistance and conductive properties of the EMI shielding film, maintains a stable shielding effect, delays the aging process, and ensures the stability of conductivity and shielding performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118741996A_ABST
    Figure CN118741996A_ABST
Patent Text Reader

Abstract

The invention discloses an EMI shielding film and a preparation technology, the EMI shielding film comprises a base material layer, an upper coating layer and a base layer which are arranged in a stacked mode, and the base layer is sequentially provided with a first conductive layer, a silicon-aluminum mixed layer, a second conductive layer, a shielding layer and an anti-oxidation layer from bottom to top; and the molar ratio of silicon to aluminum in the silicon-aluminum mixed layer is (85-98): (15-2). The preparation method comprises the following steps: respectively coating the upper coating layer and the lower coating layer on the two surfaces of the base material layer, and attaching the lower protective film to the lower coating layer; sequentially plating a base coat, a first conductive layer, a silicon-aluminum mixed layer, a second conductive layer, a shielding layer and an anti-oxidation layer on the upper coating layer; and a protective film is attached to the anti-oxidation layer. The shielding film provided by the invention has excellent electrical conductivity and aging resistance, and can present a better shielding effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of shielding films, and in particular relates to an EMI shielding film and a preparation process thereof. Background Art

[0002] At present, due to the increasing complexity of the electromagnetic environment, electromagnetic pollution has inevitably become the fourth largest hazard after water pollution, noise pollution and air pollution. For example, the panel of a common plasma color TV uses the principle of generating plasma discharge by high voltage from a mixed gas such as neon-xenon during operation. Its circuit and panel inevitably generate some high-frequency electromagnetic waves, causing certain electromagnetic pollution.

[0003] EMI shielding film, or electromagnetic interference shielding film, can be used for electromagnetic shielding of other electronic products and electronic devices such as plasma color TV windows. Among them, ultra-low resistance EMI shielding film can achieve electromagnetic interference shielding with extremely low resistance, reducing the impact of electromagnetic interference on the stable operation of precision equipment and even human health. When electromagnetic waves propagate to the shielding material, the attenuation mechanism of electromagnetic waves is: reflection loss of electromagnetic waves caused by impedance mismatch on the surface of the shielding material; shielding material absorbs and attenuates electromagnetic waves entering the material; multiple reflections and attenuation inside the shielding material. Among them, when reflection loss occurs, the shielding material has carriers that can move freely in the magnetic field and needs to have good conductivity.

[0004] Therefore, conductivity will affect the shielding effect of EMI shielding film. The smaller the square resistance of EMI shielding film, the higher the conductivity and the better the corresponding shielding effect. However, EMI shielding film will age after long-term use. Aging will increase the resistance of EMI shielding film, thereby weakening the shielding effect of EMI shielding film. Therefore, how to make EMI shielding film have both good anti-aging performance and low resistance is a problem that needs to be solved.

[0005] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention and should not be regarded as an acknowledgment or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art. Summary of the invention

[0006] The object of the present invention is to provide an EMI shielding film and a preparation process, which can have good aging resistance and excellent electrical conductivity and have a better shielding effect.

[0007] In order to achieve the above object, a technical solution provided by a specific embodiment of the present invention is as follows:

[0008] An EMI shielding film comprises a laminated substrate layer, an upper coating layer and a primer layer, wherein the primer layer is provided with a first conductive layer, a silicon-aluminum mixed layer, a second conductive layer, a shielding layer and an anti-oxidation layer in order from bottom to top;

[0009] The molar ratio of silicon to aluminum in the silicon-aluminum mixed layer is 85-98:15-2.

[0010] In one or more embodiments of the present invention, the first conductive layer is an aluminum-doped zinc oxide layer.

[0011] In one or more embodiments of the present invention, the molar ratio of zinc oxide to aluminum in the aluminum-doped zinc oxide layer is 82-99:18-1.

[0012] In one or more embodiments of the present invention, the second conductive layer is an indium tin oxide layer.

[0013] In one or more embodiments of the present invention, the shielding layer is a silver layer.

[0014] In one or more embodiments of the present invention, the anti-oxidation layer is a nickel-chromium layer.

[0015] In one or more embodiments of the present invention, the molar ratio of nickel to chromium in the nickel-chromium layer is 75-20:25-5.

[0016] In one or more embodiments of the present invention, the thickness of the first conductive layer is 3-105nm; and / or the thickness of the silicon-aluminum mixed layer is 16-150nm; and / or the thickness of the second conductive layer is 5-98nm; and / or the thickness of the shielding layer is 1-100nm; and / or the thickness of the anti-oxidation layer is 2-85nm.

[0017] In one or more embodiments of the present invention, the substrate layer is selected from a PET layer, a PI layer, a TAC layer, a COP layer and a PC layer; and / or, the base layer material is selected from SiO2, Ti, TiO2, Si, Al2O3, MgF2, SiO, HfO2, SnO2 and Y2O3; the upper coating layer is formed by an acrylic resin coating liquid;

[0018] And / or, the thickness of the substrate layer is 5.7-250 μm; and / or, the thickness of the primer layer is 0.5-13 nm; and / or, the thickness of the top coating layer is 50-290 nm.

[0019] Another specific embodiment of the present invention provides a technical solution as follows:

[0020] A preparation process of an EMI shielding film comprises the following steps:

[0021] An upper coating layer and a lower coating layer are coated on both sides of the substrate layer, and a lower protective film is attached to the lower coating layer;

[0022] A primer layer, a first conductive layer, a silicon-aluminum mixed layer, a second conductive layer, a shielding layer, and an anti-oxidation layer are sequentially plated on the upper coating layer;

[0023] A protective film is attached to the anti-oxidation layer.

[0024] Compared with the prior art, the shielding film of the present invention utilizes a specific sequence of silicon-aluminum mixed layers and other layer structures, has excellent anti-aging properties, stable conductive properties, and can present a stable and excellent shielding effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0026] Figure 1 A structural diagram of an EMI shielding film in one embodiment of the present invention;

[0027] Figure 2 This is a diagram showing the optical test results of the shielding film in Comparative Example 1;

[0028] Figure 3 This is a diagram showing the optical test results of the shielding film in Example 1.

[0029] Description of main reference numerals:

[0030] 1-lower protective film, 2-lower coating layer, 3-substrate layer, 4-upper coating layer, 5-base layer, 6-first conductive layer, 7-silicon-aluminum mixed layer, 8-second conductive layer, 9-shielding layer, 10-anti-oxidation layer, 11-upper protective film. DETAILED DESCRIPTION

[0031] The specific embodiments of the present invention are described in detail below, but it should be understood that the protection scope of the present invention is not limited by the specific embodiments.

[0032] Unless explicitly stated otherwise, throughout the specification and claims, the term “comprise” or variations such as “include” or “comprising”, etc., will be understood to include the stated elements or components but not to exclude other elements or components.

[0033] An embodiment of the present invention provides an EMI shielding film, comprising a laminated substrate layer, an upper coating layer and a primer layer, wherein the primer layer is provided with a first conductive layer, a silicon-aluminum mixed layer, a second conductive layer, a shielding layer and an anti-oxidation layer in order from bottom to top;

[0034] The molar ratio of silicon to aluminum in the silicon-aluminum mixed layer is 85-98:15-2.

[0035] Specifically, the higher the conductivity of the shielding film, the higher the shielding effectiveness. The first conductive layer and the second conductive layer can give the shielding film better conductivity, thereby ensuring the shielding performance of the shielding film; the silicon-aluminum mixed layer has good conductivity and can effectively shield electromagnetic interference. At the same time, the silicon-aluminum mixed layer has excellent thermal stability, corrosion resistance and tensile hardness, which can improve the stability of the shielding film; by controlling the silicon-aluminum molar ratio, the silicon-aluminum mixed layer has good conductivity and thermal stability; the shielding layer is close to the top layer of the shielding film, and can shield most of the electromagnetic waves. The remaining electromagnetic waves are attenuated by the second conductive layer, the silicon-aluminum mixed layer and the first conductivity, so that the shielding film has a higher shielding effectiveness; the antioxidant layer is located on the outer layer of the shielding film, and can play an antioxidant role, protect the stability of the overall structure and performance of the shielding film, thereby delaying the aging of the shielding film, so that the shielding film can maintain a higher conductivity, thereby ensuring its stable shielding performance.

[0036] In one embodiment, the first conductive layer is an aluminum-doped zinc oxide layer.

[0037] In one embodiment, the molar ratio of zinc oxide to aluminum in the aluminum-doped zinc oxide layer is 82-99:18-1.

[0038] Specifically, aluminum-doped zinc oxide has excellent conductivity, strong high-temperature stability, good radiation protection performance, and its performance is less affected by climate and usage environment. By limiting the molar ratio of zinc oxide and aluminum, the structure of the first conductive layer is made dense and the conductivity is improved, thereby improving the shielding effectiveness of the shielding film.

[0039] In one embodiment, the second conductive layer is an indium tin oxide layer.

[0040] Specifically, indium tin oxide has excellent electrical conductivity, can effectively cut off electromagnetic waves and achieve a shielding effect; at the same time, it has high hardness, wear resistance, and good chemical etching properties, which can simultaneously improve the shielding effectiveness and aging resistance of the shielding film.

[0041] In one embodiment, the shielding layer is a silver layer.

[0042] Specifically, the silver layer is a dense conductive layer with excellent conductivity and high reflectivity, which can greatly improve the shielding effect of the shielding film. Moreover, silver has strong antioxidant properties, which can improve the aging resistance of the shielding film to a certain extent.

[0043] In one embodiment, the anti-oxidation layer is a nickel-chromium layer.

[0044] In one embodiment, the molar ratio of nickel to chromium in the nickel-chromium layer is 75-20:25-5.

[0045] Specifically, when the nickel-chromium alloy is deposited on the shielding layer, nickel and oxygen, chromium and oxygen will generate oxides, thereby forming a dense oxide film on the shielding layer. The oxide film has excellent stability and can effectively prevent further oxidation of the internal material, thereby playing a role in protecting the shielding film. The molar ratio of nickel and chromium in the nickel-chromium layer will affect the conductivity, corrosion resistance and high temperature resistance of the nickel-chromium layer. Selecting an appropriate ratio can effectively ensure that the shielding film has good conductivity and aging resistance.

[0046] In one embodiment, the thickness of the first conductive layer is 3-105 nm; the thickness of the silicon-aluminum mixed layer is 16-150 nm; the thickness of the second conductive layer is 5-98 nm; the thickness of the shielding layer is 1-100 nm; and the thickness of the anti-oxidation layer is 2-85 nm.

[0047] Specifically, when electromagnetic waves enter the shielding film, the appropriate thickness is conducive to gradually weakening the intensity of the electromagnetic waves, so that the shielding film has a lower resistance; by controlling the thickness of each layer, the shielding film can exert a better shielding effect.

[0048] In one embodiment, the substrate layer is selected from a PET layer, a PI layer, a TAC layer, a COP layer and a PC layer; the base layer material is selected from SiO2, Ti, TiO2, Si, Al2O3, MgF2, SiO, HfO2, SnO2 and Y2O3; the upper coating layer is formed by an acrylic resin coating liquid;

[0049] The thickness of the substrate layer is 5.7-250 μm; the thickness of the primer layer is 0.5-13 nm; and the thickness of the top coating layer is 50-290 nm.

[0050] Another embodiment of the present invention provides a process for preparing an EMI shielding film, comprising the following steps:

[0051] An upper coating layer and a lower coating layer are coated on both sides of the substrate layer, and a lower protective film is attached to the lower coating layer;

[0052] A primer layer, a first conductive layer, a silicon-aluminum mixed layer, a second conductive layer, a shielding layer, and an anti-oxidation layer are sequentially plated on the upper coating layer;

[0053] A protective film is attached to the anti-oxidation layer.

[0054] Specifically, during the coating process, magnetron sputtering coating technology is used to improve deposition efficiency, ensure the density and uniformity of the film layer, and accurately control the thickness of the film layer. The upper coating layer and the lower coating layer are both formed by coating an acrylic resin coating liquid. The acrylic resin is an existing product, and its main components are copolymer resins of (meth) acrylic esters and (meth) hydroxy acrylates.

[0055] In one embodiment, the lower protective film is a PET film, and the upper protective film is a CPP film.

[0056] Specifically, the lower protective film is attached to the lower coating layer before the coating operation is performed, which can protect the appearance of the film surface and the stability of the coating during the magnetron sputtering coating process. The CPP film selected for the upper protective film is a cast polypropylene protective film, which has excellent heat resistance, acid and alkali resistance, and can improve the performance stability of the shielding film.

[0057] The present invention is further described in detail below in conjunction with specific embodiments.

[0058] Example 1

[0059] An EMI shielding film comprises, from bottom to top, a PET film with a thickness of 50 μm, a lower coating layer with a thickness of 0.3 μm, a PET layer with a thickness of 15 μm, an upper coating layer with a thickness of 50 nm, a primer layer with a thickness of 0.5 nm, an aluminum-doped zinc oxide layer with a thickness of 3 nm, a silicon-aluminum mixed layer with a thickness of 16 nm, an indium tin oxide layer with a thickness of 20 nm, a silver layer with a thickness of 32 nm, a nickel-chromium layer with a thickness of 17 nm, and a CPP film with a thickness of 60 μm.

[0060] Among them, the lower coating layer and the upper coating layer are both formed by coating with an acrylic resin coating liquid; the base layer is formed by plating silicon dioxide; the molar ratio of zinc oxide and aluminum in the target material used for the aluminum-doped zinc oxide layer is 82:18; the molar ratio of silicon and aluminum in the target material used for the silicon-aluminum mixed layer is 85:15; the molar ratio of nickel and chromium in the target material used for the nickel-chromium layer is 75:25.

[0061] Example 2

[0062] An EMI shielding film comprises, from bottom to top, a PET film with a thickness of 30 μm, a lower coating layer with a thickness of 3.9 μm, a PET layer with a thickness of 204 μm, an upper coating layer with a thickness of 132 nm, a primer layer with a thickness of 13 nm, an aluminum-doped zinc oxide layer with a thickness of 45 nm, a silicon-aluminum mixed layer with a thickness of 64 nm, an indium tin oxide layer with a thickness of 5 nm, a silver layer with a thickness of 1 nm, a nickel-chromium layer with a thickness of 48 nm, and a CPP film with a thickness of 60 μm.

[0063] Among them, the lower coating layer and the upper coating layer are both formed by coating with an acrylic resin coating liquid; the base layer is formed by plating silicon dioxide; the molar ratio of zinc oxide and aluminum in the target material used for the aluminum-doped zinc oxide layer is 82:18; the molar ratio of silicon and aluminum in the target material used for the silicon-aluminum mixed layer is 85:15; the molar ratio of nickel and chromium in the target material used for the nickel-chromium layer is 75:25.

[0064] Example 3

[0065] The invention discloses an EMI shielding film, which comprises, from bottom to top, a PET film with a thickness of 105 μm, a lower coating layer with a thickness of 1.5 μm, a PET layer with a thickness of 5.7 μm, an upper coating layer with a thickness of 290 nm, a primer layer with a thickness of 8 nm, an aluminum-doped zinc oxide layer with a thickness of 76 nm, a silicon-aluminum mixed layer with a thickness of 150 nm, an indium tin oxide layer with a thickness of 98 nm, a silver layer with a thickness of 100 nm, a nickel-chromium layer with a thickness of 2 nm and a CPP film with a thickness of 60 μm.

[0066] Among them, the lower coating layer and the upper coating layer are both formed by coating with an acrylic resin coating liquid; the base layer is formed by plating silicon dioxide; the molar ratio of zinc oxide and aluminum in the target material used for the aluminum-doped zinc oxide layer is 82:18; the molar ratio of silicon and aluminum in the target material used for the silicon-aluminum mixed layer is 85:15; the molar ratio of nickel and chromium in the target material used for the nickel-chromium layer is 75:25.

[0067] Example 4

[0068] The invention discloses an EMI shielding film, which comprises, from bottom to top, a PET film with a thickness of 188 μm, a lower coating layer with a thickness of 2.7 μm, a PET layer with a thickness of 250 μm, an upper coating layer with a thickness of 212 nm, a primer layer with a thickness of 5 nm, an aluminum-doped zinc oxide layer with a thickness of 105 nm, a silicon-aluminum mixed layer with a thickness of 95 nm, an indium tin oxide layer with a thickness of 54 nm, a silver layer with a thickness of 67 nm, a nickel-chromium layer with a thickness of 85 nm, and a CPP film with a thickness of 60 μm.

[0069] Among them, the lower coating layer and the upper coating layer are both formed by coating with an acrylic resin coating liquid; the base layer is formed by plating silicon dioxide; the molar ratio of zinc oxide and aluminum in the target material used for the aluminum-doped zinc oxide layer is 82:18; the molar ratio of silicon and aluminum in the target material used for the silicon-aluminum mixed layer is 85:15; the molar ratio of nickel and chromium in the target material used for the nickel-chromium layer is 75:25.

[0070] Example 5

[0071] The only difference between this embodiment and Embodiment 1 is that the thickness of the silicon-aluminum mixed layer is 150 nm.

[0072] Example 6

[0073] The only difference between this embodiment and Embodiment 1 is that the thickness of the silicon-aluminum mixed layer is 10 nm.

[0074] Example 7

[0075] The only difference between this embodiment and embodiment 1 is that the molar ratio of silicon to aluminum in the target material used for the silicon-aluminum mixed layer is 98:2.

[0076] Example 8

[0077] The only difference between this embodiment and embodiment 1 is that the molar ratio of nickel to chromium in the target material used for the nickel-chromium layer is 20:5.

[0078] Example 9

[0079] The only difference between this embodiment and embodiment 1 is that the molar ratio of nickel to chromium in the target material used for the nickel-chromium layer is 20:1.

[0080] Example 10

[0081] The only difference between this embodiment and embodiment 1 is that the molar ratio of zinc oxide to aluminum in the target material used for the aluminum-doped zinc oxide layer is 99:1.

[0082] Embodiment 11

[0083] The only difference between this embodiment and embodiment 1 is that the molar ratio of zinc oxide to aluminum in the target material used for the aluminum-doped zinc oxide layer is 80:20.

[0084] Comparative Example 1

[0085] The only difference between this comparative example and Example 1 is that the silicon-aluminum mixed layer is a silicon dioxide layer and the target material used is a pure silicon target material.

[0086] Comparative Example 2

[0087] The only difference between this comparative example and Example 1 is that the molar ratio of silicon to aluminum in the target material used for the silicon-aluminum mixed layer is 85:20.

[0088] Comparative Example 3

[0089] The only difference between this comparative example and Example 1 is that the nickel-chromium layer is replaced by a silver layer.

[0090] Comparative Example 4

[0091] The only difference between this comparative example and Example 1 is that the silver layer is replaced by an indium tin oxide layer.

[0092] Comparative Example 5

[0093] The only difference between this comparative example and Example 1 is that the indium tin oxide layer is replaced by a silver layer.

[0094] The EMI shielding films in the embodiments and comparative examples were prepared by the above-mentioned preparation method, and their performances were tested.

[0095] (1) Optical test: Lay the back of the shielding film with OCA glue and then onto a black acrylic plate. After lamination, use a degassing machine to remove bubbles. After degassing, wipe the surface clean. Use an Olympus reflectometer to test the reflection curve and a transmittance meter to test the transmittance curve. The results are as follows: Figure 2 and Figure 3 shown.

[0096] Depend on Figure 2 and Figure 3 It can be seen that the shielding film of Example 1 and the shielding film of Comparative Example 1 have little difference in optical performance, and both exhibit good optical performance.

[0097] (2) 100-grid test: Apply OCA glue to the back of the shielding film and then to the transparent glass. After bonding, use a degassing machine to degas. After degassing, wipe the surface clean and then treat it under the following conditions: a. Boil in 100°C water for 1h and 2h; b. Place it at high temperature of 85°C and high humidity of 85% for 10 days and 15 days; c. Place it at high temperature of 95°C for 10 days and 15 days; d. Place it at low temperature of -40°C for 10 days and 15 days. After treatment, use a 100-grid knife to cut 100 grids, then use 3M681 tape to stick and press it, let it stand for 30s and then pull off the tape. No shedding is 5B; slight shedding, the total shedding area is less than 5% is 4B; slight shedding, the shedding area is 5%-15% is 3B; shedding in pieces, the shedding area is 15%-35% is 2B; shedding in pieces, the shedding area is 35%-65% is 1B; shedding area exceeds 65% is 0B. 5B is judged as OK, 3-4B is barely OK, and 2B or less is judged as NG. The test results are shown in Table 1.

[0098] Table 1 100-grid test results

[0099]

[0100] (3) Square resistance test: Cut the shielding film to a width of 1250 mm and place it on a flat plate with the coated surface facing up. The square resistance values ​​at 13 points are evenly tested. The test results are shown in Table 2.

[0101] Table 2 Square resistance test results

[0102]

[0103]

[0104] (4) Square resistance test after environmental measurement: OCA glue is applied to the back of the shielding film and then attached to the transparent glass. After attachment, the shielding film is degassed with a degassing machine. After degassing, the surface is wiped clean and then treated under the following conditions: a. Boiled in 100°C water for 1h and 2h; b. Placed at high temperature of 85°C and high humidity of 85% for 10 days and 15 days; c. Placed at high temperature of 95°C for 10 days and 15 days; d. Placed at low temperature of -40°C for 10 days and 15 days. After treatment, the square resistance of the shielding film is tested. The results are shown in Table 3.

[0105] Table 3 Square resistance test results after loop test (unit: Ω)

[0106]

[0107]

[0108]

[0109] In combination with Tables 1 to 3, it can be seen from Table 2 that the square resistance values ​​of the shielding films in Example 1 and Comparative Example 1 are basically the same at different points, with good uniformity, meeting the standard range requirement of 5.0±1.5Ω resistance; referring to Table 3, after being treated under different conditions, the shielding film in Example 1 shows relatively stable performance, and there is no shedding phenomenon of the shielding film before and after the treatment, while the shielding film in Comparative Example 1 shows obvious shedding phenomenon after treatment, and its stability is poorer than that of Example 1; at the same time, it can also be seen from Table 3 that the resistance value of the shielding film of Comparative Example 1 is significantly increased after treatment, indicating that the aging resistance of the shielding film is weak, indicating that the present invention can improve the aging resistance of the shielding film by using the silicon-aluminum mixed layer, so that the shielding film can maintain a higher conductivity, thereby having a better shielding effect.

[0110] Combined with Table 3, the increase in resistance of the shielding film in Comparative Example 2 after treatment indicates that the present invention can promote the silicon-aluminum mixed layer to increase the anti-aging performance of the shielding film by limiting the silicon-aluminum molar ratio in the silicon-aluminum mixed layer. The shielding films in Comparative Examples 3 to Comparative Examples 5 have a greater resistance after treatment than the shielding films in the embodiments, and after being boiled in water for 2 hours, treated with high temperature and high humidity for 15 days, treated at high temperature of 95°C, and treated at low temperature of -40°C, the resistance values ​​all exceed the standard range of 5.0±1.5Ω, indicating that the shielding film in the embodiments of the present invention has excellent anti-aging performance and good conductivity, and can thus exhibit a better shielding effect.

[0111] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.

[0112] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. An EMI shielding film, characterized in that: It comprises a substrate layer, an upper coating layer and a primer layer which are stacked, wherein the primer layer is provided with a first conductive layer, a silicon-aluminum mixed layer, a second conductive layer, a shielding layer and an anti-oxidation layer in order from bottom to top; The molar ratio of silicon to aluminum in the silicon-aluminum mixed layer is 85-98:15-2.

2. An EMI shielding film according to claim 1, characterized in that: The first conductive layer is an aluminum-doped zinc oxide layer.

3. An EMI shielding film according to claim 2, characterized in that: The molar ratio of zinc oxide to aluminum in the aluminum-doped zinc oxide layer is 82-99:18-1.

4. The EMI shielding film according to claim 1, characterized in that: The second conductive layer is an indium tin oxide layer.

5. The EMI shielding film according to claim 1, characterized in that: The shielding layer is a silver layer.

6. The EMI shielding film according to claim 1, characterized in that: The anti-oxidation layer is a nickel-chromium layer.

7. The EMI shielding film according to claim 6, characterized in that: The molar ratio of nickel to chromium in the nickel-chromium layer is 75-20:25-5.

8. The EMI shielding film according to claim 1, characterized in that: The thickness of the first conductive layer is 3-105nm; and / or the thickness of the silicon-aluminum mixed layer is 16-150nm; and / or the thickness of the second conductive layer is 5-98nm; and / or the thickness of the shielding layer is 1-100nm; and / or the thickness of the anti-oxidation layer is 2-85nm.

9. The EMI shielding film according to claim 1, characterized in that: The substrate layer is selected from PET layer, PI layer, TAC layer, COP layer and PC layer; and / or, the base layer material is selected from SiO2, Ti, TiO2, Si, Al2O3, MgF2, SiO, HfO2, SnO2 and Y2O3; the upper coating layer is formed by acrylic resin coating liquid; And / or, the thickness of the substrate layer is 5.7-250 μm; and / or, the thickness of the primer layer is 0.5-13 nm; and / or, the thickness of the top coating layer is 50-290 nm.

10. The process for preparing an EMI shielding film according to any one of claims 1 to 9, characterized in that: The steps include: An upper coating layer and a lower coating layer are coated on both sides of the substrate layer, and a lower protective film is attached to the lower coating layer; A primer layer, a first conductive layer, a silicon-aluminum mixed layer, a second conductive layer, a shielding layer, and an anti-oxidation layer are sequentially plated on the upper coating layer; A protective film is attached to the anti-oxidation layer.