Electrolytic capacitor element and electrolytic capacitor
By using a porous part and conductive layer structure in the electrolytic capacitor, and using scaly insulating inorganic fillers to prevent moisture intrusion, the problem of metal foil corrosion caused by moisture in the electrolytic capacitor is solved, and the reliability and leakage current performance of the capacitor are improved.
Patent Information
- Application Number
- CN202280093297.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-07
- Filing Date
- 2022-11-17
- Publication Date
- 2024-10-01
AI Technical Summary
In electrolytic capacitors, moisture invades the metal foil through the carbon layer and causes corrosion, causing problems with poor leakage current.
It adopts a porous part, dielectric layer, solid electrolyte layer and conductive layer structure. The conductive layer contains a carbon layer and a scaly insulating inorganic filler. The insulating inorganic filler of the carbon layer forms an acute angle with the cross section of the metal foil, with an average value of 0 ° above and below 45 ° to prevent moisture intrusion.
Effectively prevent moisture intrusion, avoid metal foil corrosion, improve the long-term reliability of electrolytic capacitors and reduce leakage current.
Smart Images

Figure CN118742987A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an electrolytic capacitor element and an electrolytic capacitor. Background Art
[0002] Patent document 1 discloses an electrolytic capacitor comprising a capacitor element, wherein the capacitor element comprises an anode body, a dielectric layer covering at least a portion of the anode body, a solid electrolyte layer covering at least a portion of the dielectric layer, and a cathode lead layer covering at least a portion of the solid electrolyte layer, wherein the cathode lead layer comprises a conductive carbon layer covering at least a portion of the solid electrolyte layer, and a silver paste layer covering at least a portion of the carbon layer, wherein the carbon layer comprises carbon particles and silver.
[0003] Prior Art Literature
[0004] Patent Literature
[0005] Patent Document 1: International Publication No. 2019 / 167774 Summary of the invention
[0006] Problem that the invention aims to solve
[0007] In the electrolytic capacitor described in Patent Document 1, a metal foil such as aluminum is used as an anode body. When moisture enters an electrolytic capacitor including a metal foil, the metal foil is corroded, and LC failure (leakage current failure) becomes a problem.
[0008] In particular, moisture may reach the metal foil through the carbon layer, and it is desired to prevent moisture from entering through this path.
[0009] The present invention has been made to solve the above-mentioned problems, and an object of the present invention is to provide an electrolytic capacitor element and an electrolytic capacitor capable of preventing corrosion of a metal foil due to the intrusion of moisture.
[0010] Technical solutions to solve problems
[0011] The electrolytic capacitor element of the present invention comprises: a valve-acting metal substrate having a core portion including a metal foil and a porous portion formed along the surface of the metal foil; a dielectric layer formed on the porous portion; a solid electrolyte layer formed on the dielectric layer; and a conductive layer formed on the solid electrolyte layer, wherein the conductive layer comprises a carbon layer, wherein the carbon layer comprises a carbon filler and a flaky insulating inorganic filler, and in a cross section obtained by cutting the electrolytic capacitor element in a direction perpendicular to the main surface of the metal foil, an average value of acute angles formed by the long side direction of the cross section of the insulating inorganic filler present in the carbon layer formed on the main surface of the metal foil and the long side direction of the cross section of the metal foil is greater than 0° and less than 45°.
[0012] The electrolytic capacitor of the present invention includes a laminated body in which a plurality of electrolytic capacitor elements of the present invention are laminated, an anode external electrode, and a cathode external electrode.
[0013] Effects of the Invention
[0014] According to the present invention, it is possible to provide an electrolytic capacitor element and an electrolytic capacitor capable of preventing corrosion of a metal foil due to the intrusion of moisture. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 This is a perspective view schematically showing an example of a laminated body in which a plurality of electrolytic capacitor elements are laminated.
[0016] Figure 2 This is a perspective view schematically showing an example of a laminated body in which a plurality of electrolytic capacitor elements are laminated.
[0017] Figure 3 It is a cross-sectional view schematically showing an example of a laminated body in which a plurality of electrolytic capacitor elements are laminated.
[0018] Figure 4 It is an enlarged cross-sectional view schematically showing an example of a carbon layer.
[0019] Figure 5 This is a schematic diagram showing how the labyrinth effect is exerted by the scaly insulating inorganic filler.
[0020] Figure 6 It is a perspective view schematically showing the shape of a scaly insulating inorganic filler.
[0021] Figure 7 It is an enlarged cross-sectional view schematically showing another example of the carbon layer.
[0022] Figure 8 It is a cross-sectional view taken along the LT plane schematically showing another example of a laminated body in which a plurality of electrolytic capacitor elements are laminated.
[0023] Fig. 9 It is schematically shown Figure 8 An enlarged cross-sectional view of the area surrounded by area B in FIG.
[0024] Fig.10 WT is a cross-sectional view schematically showing an example of a laminated body in which a plurality of electrolytic capacitor elements are laminated.
[0025] Fig.11 It is schematically shown Fig.10 An enlarged cross-sectional view of the area surrounded by area D in FIG.
[0026] Fig.12 It is a perspective view schematically showing an example of an electrolytic capacitor. DETAILED DESCRIPTION
[0027] Hereinafter, the electrolytic capacitor element and the electrolytic capacitor of the present invention will be described.
[0028] However, the present invention is not limited to the following configurations, and can be applied with appropriate changes within the scope of the gist of the present invention. In addition, a combination of two or more of the preferred configurations of the present invention described below is also the present invention.
[0029] The electrolytic capacitor element of the present invention comprises: a valve-acting metal substrate having a core portion including a metal foil and a porous portion formed along the surface of the metal foil; a dielectric layer formed on the porous portion; a solid electrolyte layer formed on the dielectric layer; and a conductive layer formed on the solid electrolyte layer, wherein the conductive layer comprises a carbon layer, wherein the carbon layer comprises a carbon filler and a flaky insulating inorganic filler, and in a cross section obtained by cutting the electrolytic capacitor element in a direction perpendicular to the main surface of the metal foil, an average value of acute angles formed by the long side direction of the cross section of the insulating inorganic filler present in the carbon layer formed on the main surface of the metal foil and the long side direction of the cross section of the metal foil is greater than 0° and less than 45°.
[0030] Figure 1 as well as Figure 2 FIG. 1 is a perspective view schematically showing an example of a laminated body in which a plurality of electrolytic capacitor elements are laminated. Figure 1 In the figure, the first end face E101 as the cathode side end face is shown in front, Figure 2 In FIG. 1 , the second end face E102 serving as the anode side end face is shown in the foreground.
[0031] The stack 100 has a first main surface M101 and a second main surface M102 opposite to each other in the stacking direction (T direction), a first end surface E101 and a second end surface E102 opposite to each other in the length direction (L direction) perpendicular to the stacking direction, and a first side surface S101 and a second side surface S102 opposite to each other in the width direction (W direction) perpendicular to the stacking direction and the length direction.
[0032] Moisture may penetrate into the laminate 100. The direction of moisture penetration in this specification is Figure 1 as well as Figure 2 In the present specification, attention is paid to preventing corrosion of the metal foil caused by the intrusion of moisture from the first end face E101, the second end face E102, the first side face S101 or the second side face S102 of the laminate.
[0033] When the laminate is stored, or when the laminate is stored as an electrolytic capacitor after external electrodes are formed on the laminate, moisture may enter the laminate 100 .
[0034] Figure 3 It is a cross-sectional view schematically showing an example of a stacked body in which a plurality of electrolytic capacitor elements are stacked, and is a cross-sectional view taken along the LT plane cut along a plane along the longitudinal direction (L direction) and the stacking direction (T direction) of the stacked body.
[0035] Figure 3 Too Figure 1 AA line section view.
[0036] exist Figure 3 In FIG. 1 , arrows are also used to indicate directions in which moisture penetrates from the first end surface E101 and the second end surface E102 of the stacked body 100 .
[0037] Reference Figure 3 The structure of the electrolytic capacitor element and the structure of the laminate will be described.
[0038] Figure 3 The electrolytic capacitor element 1 shown includes: a valve-acting metal substrate 10 having a core 11 including a metal foil and a porous portion 12 formed along the surface of the metal foil; a dielectric layer 13 formed on the porous portion 12; a solid electrolyte layer 14 formed on the dielectric layer 13; and a conductive layer 16 formed on the solid electrolyte layer 14.
[0039] The core 11 of the valve-acting metal substrate 10 is led out to the second end surface E102 of the stacked body 100 to form the anode-side end surface. The core 11 is connected to the anode external electrode at the second end surface E102 of the stacked body 100.
[0040] The valve metal matrix contains a valve metal that exhibits a so-called valve action. Examples of the valve metal include metal monomers such as aluminum, tantalum, niobium, titanium, and zirconium, or alloys containing these metals. Among these, aluminum or aluminum alloys are preferred.
[0041] The core of the valve metal substrate is a metal foil. In addition, the porous portion may include an etching layer formed on the surface of the valve metal substrate, and a porous layer formed on the surface of the valve metal substrate by printing or sintering. When the valve metal is aluminum or an aluminum alloy, the etching layer is preferred, and when the valve metal is titanium or a titanium alloy, the porous layer is preferred.
[0042] The dielectric layer formed on the surface of the porous portion is porous reflecting the surface state of the porous portion and has a finely concavoconvex surface shape. The dielectric layer preferably includes an oxide film of the valve-acting metal.
[0043] Furthermore, from the viewpoint of improving manufacturing efficiency, a chemically-formed foil previously subjected to a chemical conversion treatment may be used as the valve-acting metal substrate having a dielectric layer formed on the surface.
[0044] As materials constituting the solid electrolyte layer, for example, conductive polymers having a skeleton of pyrrole, thiophene, aniline, etc. can be cited. As conductive polymers having a skeleton of thiophene, for example, PEDOT [poly (3, 4-ethylenedioxythiophene)] can be cited, and PEDOT:PSS composited with polystyrene sulfonic acid (PSS) as a dopant can also be cited.
[0045] The solid electrolyte layer is formed, for example, by a method of forming a polymer film of poly(3,4-ethylenedioxythiophene) or the like on the surface of the dielectric layer using a treatment solution containing a monomer such as 3,4-ethylenedioxythiophene, or by a method of applying a dispersion of a polymer such as poly(3,4-ethylenedioxythiophene) or the like on the surface of the dielectric layer and drying it. In addition, it is preferred that after forming a solid electrolyte layer for an inner layer that fills the micropores (recesses), a solid electrolyte layer for an outer layer that covers the entire dielectric layer is formed.
[0046] The solid electrolyte layer can be formed in a given area by applying the above-mentioned treatment liquid or dispersion liquid on the dielectric layer by sponge transfer, screen printing, spraying, dispenser coating, inkjet printing, etc. The thickness of the solid electrolyte layer is preferably 2 μm or more and preferably 20 μm or less.
[0047] The conductive layer includes a carbon layer. The conductive layer may be a carbon layer alone, or a composite layer in which a silver layer is disposed on the carbon layer. Figure 3 FIG. 4 shows a structure in which only the carbon layer 16 is used as the conductive layer 16 .
[0048] exist Figure 3 2 shows cathode foil 21 provided on conductive layer 16. Cathode foil 21 is preferably a metal foil, and preferably contains at least one metal selected from the group consisting of aluminum, copper, silver, and alloys containing these metals as main components.
[0049] Cathode foil 21 is drawn out to first end surface E101 and constitutes a cathode-side end surface. Cathode foil 21 is connected to a cathode external electrode at first end surface E101 of laminate 100 .
[0050] The valve-acting metal substrate 10 has porous portions 12 on both sides of a core portion 11 , a dielectric layer 13 is formed on the surface of each porous portion 12 , and a solid electrolyte layer 14 is provided on the dielectric layer 13 .
[0051] Conductive layer 16 and cathode foil 21 are provided on solid electrolyte layer 14 .
[0052] By repeatedly providing this structure, a plurality of electrolytic capacitor elements 1 are stacked, and stacked body 100 whose outer periphery is sealed with sealing material 130 is formed.
[0053] The carbon layer contains a carbon filler and a scaly insulating inorganic filler.
[0054] In addition, in a cross-section of the electrolytic capacitor element cut in a direction perpendicular to the main surface of the metal foil, an average value of acute angles formed by the long side direction of the cross section of the insulating inorganic filler present in the carbon layer formed on the main surface of the metal foil and the long side direction of the cross section of the metal foil is greater than 0° and less than 45°.
[0055] Hereinafter, specific matters of the present invention will be described.
[0056] Figure 4 is an enlarged cross-sectional view schematically showing an example of a carbon layer. Figure 4 , an enlarged cross-sectional view of the carbon layer in a cut surface of the electrolytic capacitor element cut in a direction perpendicular to the main surface of the metal foil is shown.
[0057] The carbon layer 16 includes spherical carbon fillers 40 and flaky insulating inorganic fillers 50 .
[0058] exist Figure 4 The arrow L in FIG. 1 shows a direction parallel to the main surface of the metal foil. Figure 4 The θ in the figure shows Figure 4 The angle formed by the longitudinal direction of the cross section of the one scaly insulating inorganic filler 50 shown and the longitudinal direction of the cross section of the metal foil is an acute angle.
[0059] The scaly insulating inorganic filler shown in the electron microscope image of the cross section taken in the direction perpendicular to the main surface of the metal foil was determined. Figure 4 When the angle θ is expressed in θ and the average value is taken, the value becomes greater than or equal to 0° and less than or equal to 45°.
[0060] As long as the angle formed by the long side direction of the cross section of the flaky insulating inorganic filler and the long side direction of the cross section of the metal foil in the above-mentioned cut surface is within the range specified in the present invention, the angle formed by the flat surface of the insulating inorganic filler and the main surface of the metal foil in three dimensions also becomes smaller. In other words, the flaky insulating inorganic filler is in a state of being oriented relative to the main surface of the metal foil.
[0061] Figure 5 This is a schematic diagram showing how the labyrinth effect is exerted by the scaly insulating inorganic filler.
[0062] The carbon layer 16 exists between the cathode foil 21 and the core 11 of the valve metal substrate. Figure 5In the figure, only the cathode foil 21 and the core 11 of the valve metal substrate, and the carbon layer 16 therebetween are schematically shown.
[0063] Furthermore, consider a case where moisture intrudes from the first end surface E101 and the second end surface E102 of the stacked body in the directions indicated by the arrows with respect to the carbon layer 16 .
[0064] exist Figure 5 Schematically shows a structure in which the angle formed by the long side direction of the cross section of the flaky insulating inorganic filler 50 and the long side direction of the cross section of the metal foil in the carbon layer 16 is 0°. If the flaky insulating inorganic filler is oriented in this way, the moisture that penetrates the carbon layer 16 from the first end face E101 and the second end face E102 of the stack is prevented from moving in the stacking direction in the carbon layer 16 and reaching the cathode foil 21 or the core 11. Moisture cannot pass through the flaky insulating inorganic filler 50, and in order to reach the cathode foil 21 or the core 11, the moisture has to avoid the flaky inorganic filler and pass through. Therefore, it becomes difficult for moisture to reach the cathode foil 21 or the core 11, and corrosion of the cathode foil 21 or the core 11 due to moisture can be prevented. Figure 5 In FIG. 1 , the direction of moisture intrusion from the end surface of the stack is indicated by an arrow, indicating that the moisture is prevented from diffusing in the stacking direction. However, similarly, moisture intrusion from the side surface of the stack can also be prevented from diffusing in the stacking direction.
[0065] The effect of preventing moisture that has penetrated from the end faces or side faces of a stacked body from diffusing in the stacking direction by disposing a scaly insulating inorganic filler is called a labyrinth effect.
[0066] The electrolytic capacitor element of the present invention includes a scaly insulating inorganic filler whose long side direction of the cross section is oriented in a specific direction (greater than 0° and less than 45°) relative to the long side direction of the cross section of the metal foil, so that a labyrinth effect can be exerted to prevent corrosion of the metal foil caused by the intrusion of moisture from the end surface or side surface of the stack.
[0067] Figure 6 It is a perspective view schematically showing the shape of a scaly insulating inorganic filler.
[0068] The flaky insulating inorganic filler 50 has a relatively wide surface relative to its thickness.
[0069] When the thickness of the flaky insulating inorganic filler 50 is t, the maximum length is l, and the maximum width is w, the product of the length and the width (l×w) is preferably larger than the thickness t. Specifically, (l×w) / t≥4 is preferred. In addition, (l×w) / t≤400 is preferred.
[0070] exist Figure 6In FIG. 1 , the thickness t, length l, and width w of the scaly insulating inorganic filler 50 are indicated by double arrows t, l, and w, respectively.
[0071] Although the value of the product of the length and the width (l×w) is larger than the plane area of the insulating inorganic filler, it is used as an approximate value of the area in consideration of the ratio between the plane area and the thickness of the insulating inorganic filler.
[0072] In addition, regarding the length l and the width w, the longer dimension is set to the length l, and the shorter dimension is set to the width w.
[0073] The ratio of the length l to the thickness t is preferably (l / t)≧2. Furthermore, (l / t)≦20 is preferred.
[0074] The ratio of the width w to the thickness t is preferably (w / t)≧2. Furthermore, (w / t)≦20 is preferred.
[0075] The length l of the scaly insulating inorganic filler is preferably 1 μm or more and preferably 20 μm or less.
[0076] The width w of the scaly insulating inorganic filler is preferably 1 μm or more and preferably 20 μm or less.
[0077] In addition, each size of the flaky insulating inorganic filler observed in the electron microscope image taken in the cross section cut in the direction perpendicular to the main surface of the metal foil is determined as the average value of the sizes of 10 or more fillers present in the image for the flaky insulating inorganic filler included in the carbon layer. The ratio of each size is also determined as the ratio of the average values of each size.
[0078] In addition, the shape of the filler observed in an electron microscope image taken on a cross section cut in a direction perpendicular to the main surface of the metal foil is as follows: Figure 4 In the case of a rectangular shape that is long in one direction, such as the flaky insulating inorganic filler 50 shown in the figure, the length of the long side is set to length l, and the length of the short side is set to thickness t. For fillers whose ratio of length l to thickness t is (l / t) ≥ 2, they can be regarded as flaky fillers even if the width w is unknown.
[0079] In addition, the length l of the flaky insulating inorganic filler is proportional to the thickness of the carbon layer ( Figure 4 Double arrow T 16 The dimensions shown) ratio (l / T 16 ) is preferably (l / T 16 )≥0.05.
[0080] The scaly insulating inorganic filler contains an insulating material.
[0081] As an insulating material, a material having a volume resistivity of 1×10 10 Materials with a thickness of Ω・cm or more.
[0082] The filler may be an insulating material as a whole, or may be a material that forms an insulating film on the surface of a conductor such as a metal to become an insulating material. An example of the latter is a material that forms a passivation film (aluminum oxide film) on the surface of aluminum.
[0083] Specific examples include ceramics or glass as insulating materials, and examples of ceramics include silicon dioxide, alumina, zirconium oxide, aluminum nitride, silicon nitride, cordierite, mullite, and yttrium oxide.
[0084] In particular, at least one material selected from the group consisting of silicon dioxide, alumina, and glass is preferred.
[0085] As the carbon filler contained in the carbon layer, materials commonly used as materials contained in the carbon layer of electrolytic capacitors can be used, and the shape thereof is not particularly limited. Figure 4 A spherical carbon filler 40 is shown in FIG. 4 as an example of the carbon filler.
[0086] The carbon filler may also be a flaky carbon filler.
[0087] Figure 7 It is an enlarged cross-sectional view schematically showing another example of the carbon layer.
[0088] exist Figure 7 In the figure, the Figure 4 The carbon fillers 40 are spherical in shape, while the carbon layer 16 includes flaky carbon fillers 45 .
[0089] In the case where the carbon filler is a flaky carbon filler, in the cut surface cut in a direction perpendicular to the main surface of the metal foil, the acute angle formed by the long side direction of the cross section of the flaky carbon filler and the long side direction of the cross section of the metal foil is preferably 0° or more and 45° or less. If the above conditions are met, the flaky carbon filler can also exert a labyrinth effect, and the corrosion of the metal foil caused by the intrusion of moisture from the end surface or side surface of the laminate can be further prevented.
[0090] The ratio of the weight of the flaky insulating inorganic filler in the carbon layer to the total weight of the carbon filler and the flaky insulating inorganic filler ((weight of flaky insulating inorganic filler) / (weight of carbon filler+weight of flaky insulating inorganic filler)) is preferably 0.01 or more and 0.5 or less.
[0091] By making the above ratio 0.01 or more and containing the flaky insulating inorganic filler in the carbon layer, the corrosion of the metal foil can be sufficiently prevented. As a result, the long-term reliability of the electrolytic capacitor can be improved. On the other hand, by making the above ratio 0.5 or less and containing the carbon filler as a conductive filler, the resistance value of the carbon layer can be reduced. As a result, the ESR of the electrolytic capacitor can be reduced.
[0092] The carbon layer may or may not contain non-scaly insulating inorganic fillers in addition to the scaly insulating inorganic fillers. When the carbon layer contains non-scaly insulating inorganic fillers, the weight ratio of the non-scaly insulating inorganic fillers is preferably 5% or less of the scaly insulating inorganic fillers.
[0093] The carbon layer may further contain a metal filler, and examples of the material of the metal filler include silver, copper, aluminum, etc. In addition, the metal filler is preferably not contained in the carbon layer because the metal filler itself may be electrochemically corroded by moisture.
[0094] Next, as an example of the electrolytic capacitor element and the laminate of the present invention, Figure 1 , Figure 2 as well as Figure 3 The methods shown are examples of different methods for explanation.
[0095] Figure 8 It is a cross-sectional view taken along the LT plane schematically showing another example of a laminated body in which a plurality of electrolytic capacitor elements are laminated.
[0096] Figure 8 The electrolytic capacitor element 2 shown includes: a valve-acting metal substrate 10 having a core 11 including a metal foil and a porous portion 12 formed along the surface of the metal foil; a dielectric layer 13 formed on the porous portion 12; a solid electrolyte layer 14 formed on the dielectric layer 13; and a conductive layer 16 formed on the solid electrolyte layer 14.
[0097] The conductive layer 16 includes a carbon layer 16a and a silver layer 16b.
[0098] Laminated body 200 is obtained by laminating a plurality of electrolytic capacitor elements 2 , and its outer periphery is sealed by outer casing 220 .
[0099] The outer casing 220 includes a first outer casing 221 and a second outer casing 222 that seal the periphery of the electrolytic capacitor element 2. The second outer casing 222 is located at the outermost periphery of the stack 200 and forms the first main surface M201, the second main surface M202, and the first side surface (S201: at the Figure 7 (not shown) and the second side (S202: Figure 7 (not shown in the figure).
[0100] The core 11 of the valve-acting metal substrate 10 is led out from the second end surface E202 of the stacked body 200 to form the anode-side end surface of the stacked body 200. The core 11 is connected to the anode external electrode at the second end surface E202 of the stacked body 200.
[0101] A mask layer 242 serving as an insulating member is provided near the anode-side end surface of the valve metal substrate 10 .
[0102] A collector electrode 230 is provided on the first end surface E201 of the stacked body 200 and is electrically connected to the plurality of cathodes of the plurality of electrolytic capacitor elements 2. Figure 8 As shown, the collector electrode 230 is exposed at the first end surface E201 of the stacked body 200 and constitutes the cathode side end surface of the stacked body 200. The collector electrode 230 is connected to the cathode external electrode at the first end surface E201 of the stacked body 200.
[0103] exist Figure 8 In the electrolytic capacitor element 2 shown, the dielectric layer 13 , the solid electrolyte layer 14 , and the conductive layer 16 are also provided on the side surface and one end surface of the valve-acting metal substrate 10 .
[0104] Moreover, in a cross section obtained by cutting the electrolytic capacitor element in a direction perpendicular to the main surface of the metal foil, the average value of acute angles formed by the long side direction of the cross section of the flaky insulating inorganic filler present in the carbon layer formed on the side surface and one end surface of the metal foil and the long side direction of the cross section of the metal foil is greater than 45° and less than 90°.
[0105] First, the above-mentioned “carbon layer formed on one end surface of the metal foil” will be described.
[0106] The area of interest is Figure 8 The region surrounded by region B is the region near the cathode-side end face of the metal foil. In addition, since no carbon layer exists in the region near the anode-side end face of the metal foil, no attention is paid.
[0107] Fig. 9 It is schematically shown Figure 8 An enlarged cross-sectional view of the area surrounded by area B in FIG.
[0108] "One end surface of the metal foil" refers to the end surface of the core portion of the metal foil. Fig. 9 , the position of the first end surface 11 e 1 of the metal foil, which is the end surface of the core 11 , is shown.
[0109] On the first end face 11e1 of the metal foil, a porous portion 12, a dielectric layer 13, a solid electrolyte layer 14, and a conductive layer 16 are formed along the surface. The conductive layer 16 includes a carbon layer 16a and a silver layer 16b.
[0110] "The carbon layer formed on one end surface of the metal foil" is Fig. 9 The area enclosed by area C in .
[0111] The carbon layer 16 a includes flaky insulating inorganic fillers 50 and flaky carbon fillers 45 .
[0112] exist Fig. 9 The arrow L in FIG. 1 shows the long side direction of the cross section of the metal foil (the direction parallel to the main surface of the metal foil). Fig. 9 In the figure, φ is used to indicate an acute angle among angles formed between the longitudinal direction of the cross section of one scaly insulating inorganic filler 50 existing in the carbon layer (region C) formed on one end surface of the metal foil and the longitudinal direction of the cross section of the metal foil.
[0113] The scaly insulating inorganic filler shown in the electron microscope image of the cross section taken in the direction perpendicular to the main surface of the metal foil was determined. Fig. 9 When the angle φ is used and the average value is taken, the value is greater than or equal to 45° and less than or equal to 90°.
[0114] When the scaly insulating inorganic filler contained in the carbon layer is oriented in this way, the labyrinth effect can prevent moisture entering from the first end surface E201 of the stacked body 200 from moving along the carbon layer 16a formed on one end surface of the metal foil in the thickness direction of the carbon layer and reaching the core 11.
[0115] In addition, Fig. 9 θ indicates the acute angle between the longitudinal direction of the cross section of a flaky insulating inorganic filler 50 existing in the carbon layer formed on the main surface of the metal foil and the longitudinal direction of the cross section of the metal foil. Figure 4 The angle is equal to or greater than 0° and equal to or less than 45° in the same manner as described above.
[0116] exist Fig. 9 , a mode in which the carbon layer 16a includes the flaky carbon filler 45 is shown. For the flaky carbon filler 45 present in the carbon layer (region C) formed on one end surface of the metal foil, the acute angle formed by the long side direction of the cross section of the flaky carbon filler 45 and the long side direction of the cross section of the metal foil is also preferably 45° or more and 90° or less. With this structure, it is possible to more effectively prevent corrosion of the metal foil caused by moisture intruding from the first end surface of the stack.
[0117] Next, “the carbon layer formed on the side surface of the metal foil” will be described.
[0118] Fig.10WT is a cross-sectional view schematically showing an example of a laminated body in which a plurality of electrolytic capacitor elements are laminated.
[0119] The area of concern is Fig.10 The area surrounded by area D and the area surrounded by area E. Area D and area E are areas near the side surface of the metal foil.
[0120] The region D is a region near the second side surface 11s2 of the metal foil, and the region E is a region near the first side surface 11s1 of the metal foil.
[0121] Fig.11 It is schematically shown Fig.10 An enlarged cross-sectional view of the area surrounded by area D in FIG.
[0122] The "side of the metal foil" is the side of the core that includes the metal foil. Fig.11 2 shows the position of the second side surface 11s2 of the metal foil, which is the side surface of the core 11.
[0123] On the second side surface 11s2 of the metal foil, a porous portion 12, a dielectric layer 13, a solid electrolyte layer 14, and a conductive layer 16 are formed along the surface. The conductive layer 16 includes a carbon layer 16a and a silver layer 16b.
[0124] The carbon layer formed on the side of the metal foil is Fig.11 The area enclosed by area F in .
[0125] The carbon layer 16a includes a flaky insulating inorganic filler 50 and a flaky carbon filler 45. Fig.11 In the figure, the acute angle among the angles formed between the longitudinal direction of the cross section of one scaly insulating inorganic filler 50 existing in the region and the longitudinal direction of the cross section of the metal foil is shown by φ.
[0126] The scaly insulating inorganic filler shown in the electron microscope image of the cross section taken in the direction perpendicular to the main surface of the metal foil was determined. Fig.11 When the angle φ is used and the average value is taken, the value is greater than or equal to 45° and less than or equal to 90°.
[0127] If the scaly insulating inorganic filler contained in the carbon layer is oriented in this way, the labyrinth effect can prevent moisture entering from the second side surface S202 of the stacked body 200 from moving along the carbon layer 16a formed on the second side surface of the metal foil in the thickness direction of the carbon layer and reaching the core 11.
[0128] The carbon layer formed on the first side surface 11 s 1 of the metal foil can also have the same structure as the carbon layer formed on the second side surface 11 s 2 of the metal foil, and can exert the same effect on moisture intruding from the first side surface S201 of the stacked body 200 .
[0129] The electrolytic capacitor of the present invention includes a laminated body in which a plurality of electrolytic capacitor elements of the present invention are laminated, an anode external electrode, and a cathode external electrode.
[0130] Fig.12 It is a perspective view schematically showing an example of an electrolytic capacitor.
[0131] Fig.12 The electrolytic capacitor 300 shown in FIG. Figure 1 , Figure 2 as well as Figure 3 ) is provided with an anode external electrode 320 on the second end surface E102, and a cathode external electrode 330 is provided on the first end surface E101.
[0132] The structures of the anode external electrode and the cathode external electrode are not particularly limited as long as they are structures of external electrodes conventionally used for electrolytic capacitors.
[0133] As the structure of the anode external electrode and the cathode external electrode, a structure in which a sputtered film and / or vapor-deposited film, a resin electrode layer, a plated layer, and the like are arbitrarily combined can be used.
[0134] When manufacturing the electrolytic capacitor element and the electrolytic capacitor of the present invention, a carbon filler and a flaky insulating inorganic filler are mixed with a carbon paste as a material for forming a carbon layer.
[0135] The carbon paste may contain resin components such as epoxy resin and phenolic resin.
[0136] The carbon layer can be formed by applying a carbon paste on the solid electrolyte layer by a method such as coating or dipping.
[0137] In order to obtain Figure 3 In the case of the structure of the stacked body 100 shown, it is preferable to form the carbon layer by applying a carbon paste on the solid electrolyte layer. The carbon paste can be applied by screen printing, sponge transfer, spraying, dispenser application, inkjet printing, or the like.
[0138] In screen printing, it is preferred that the carbon paste be applied with a squeegee to apply shear stress (shear stress) to the carbon paste in one direction, because this makes it easier to orient the flaky insulating inorganic filler in a state close to parallel to the printing surface.
[0139] Furthermore, if the mixing amounts of the carbon filler and the flaky insulating inorganic filler contained in the carbon paste are reduced, the flaky insulating inorganic filler is more likely to be oriented in a direction nearly parallel to the printing surface during drying.
[0140] In order to obtain Figure 8 In the case of the structure of the stacked body 200 shown, it is preferable to form the carbon layer by immersing the element after forming the dielectric layer and the solid electrolyte layer on the valve metal substrate in the carbon paste.
[0141] For the steps other than the formation of the carbon layer, methods conventionally performed when manufacturing an electrolytic capacitor element and an electrolytic capacitor can be used.
[0142] Description of Reference Numerals
[0143] 1.2 Electrolytic capacitor elements
[0144] 10 Valve action metal base
[0145] 11 core (metal foil)
[0146] 11e1 One end surface of the metal foil (1st end surface)
[0147] 11s1 First side of metal foil
[0148] 11s2 Second side of metal foil
[0149] 12 Porous part
[0150] 13 Dielectric layer
[0151] 14 Solid electrolyte layer
[0152] 16 Conductive layer (carbon layer)
[0153] 16a Carbon layer
[0154] 16b Silver layer
[0155] 21 Cathode foil
[0156] 40 Carbon filler (spherical)
[0157] 45 Carbon filler (flake-like)
[0158] 50 Flake-like insulating inorganic filler
[0159] 100 Laminated
[0160] M101 1st main surface
[0161] M102 2nd main surface
[0162] E101 1st end face
[0163] E102 2nd end face
[0164] S101 Side 1
[0165] S102 Side 2
[0166] 130 Sealing material
[0167] 200 Laminated
[0168] M201 1st main surface
[0169] M202 2nd main surface
[0170] E201 1st end face
[0171] E202 2nd end face
[0172] S201 Side 1
[0173] S202 Side 2
[0174] 220 Exterior body
[0175] 221 1st outer body
[0176] 222 2nd outer body
[0177] 230 Collector Electrode
[0178] 242 Mask layer
[0179] 300 Electrolytic Capacitors
[0180] 320 Anode External Electrode
[0181] 330 cathode external electrode.
Claims
1. An electrolytic capacitor element, comprising: a valve-acting metal substrate having a core portion including a metal foil and a porous portion formed along a surface of the metal foil; a dielectric layer formed on the porous portion; a solid electrolyte layer formed on the dielectric layer; and a conductive layer formed on the solid electrolyte layer, wherein: The conductive layer comprises a carbon layer, The carbon layer contains a carbon filler and a flaky insulating inorganic filler. In a cross section obtained by cutting the electrolytic capacitor element in a direction perpendicular to the main surface of the metal foil, The average value of acute angles formed between the longitudinal direction of the cross section of the insulating inorganic filler present in the carbon layer formed on the main surface of the metal foil and the longitudinal direction of the cross section of the metal foil is 0° to 45°.
2. The electrolytic capacitor element according to claim 1, wherein: The dielectric layer, the solid electrolyte layer and the conductive layer are also provided on the side surface and one end surface of the valve metal substrate. In a cross section obtained by cutting the electrolytic capacitor element in a direction perpendicular to the main surface of the metal foil, The average value of acute angles formed by the longitudinal direction of the cross section of the insulating inorganic filler and the longitudinal direction of the cross section of the metal foil in the carbon layer formed on the side surface and one end surface of the metal foil is 45° to 90°.
3. The electrolytic capacitor element according to claim 1 or 2, wherein: The carbon filler includes a flaky carbon filler.
4. The electrolytic capacitor element according to any one of claims 1 to 3, wherein: The insulating inorganic filler is at least one selected from the group consisting of silica, alumina, and glass.
5. An electrolytic capacitor comprising: A laminated body having a plurality of electrolytic capacitor elements stacked on top of each other according to any one of claims 1 to 4; an anode external electrode; and Cathode External Electrode.