A high-performance composite membrane and its preparation method

By using modified titanium dioxide and heat-resistant modifiers in the PVC-PVDF composite film, the seven-layer structure composite film is solved, and the problem of poor infrared and ultraviolet shielding effect is improved, and the heat resistance and dispersion are suitable for new Energy field.

CN118752874BActive Publication Date: 2024-11-19SHENZHEN ZHONGDE MEMBRANE STRUCTURE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411215939.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-11-19
Estimated Expiration
2044-09-02

AI Technical Summary

Technical Problem

The existing PVC-PVDF composite films are poor in infrared and ultraviolet shielding, and lack heat resistance and dispersion, resulting in limited application areas and shortened service life.

Method used

PVDF, PMMA and modified titanium dioxide are used as raw materials for surface treatment layer, and PVC and heat-resistant modifiers are used as raw materials for synthetic PVC layer to prepare a seven-layer structure composite film, and titanium dioxide is modified through fluorine doping and silane coupling agent to form a phenolic network Structure, improve dispersion and stability, and synthesize heat-resistant modifiers with core-shell structures to improve the heat resistance of PVC.

Benefits of technology

It has achieved significant improvements in infrared and ultraviolet shielding of composite films, extended service life, and improved heat resistance and adhesion of PVC, and is suitable for the new energy field.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to the field of new energy technology, and provides a high-performance composite film and a preparation method thereof. The composite film comprises a seven-layer structure from top to bottom, which are respectively: a PVDF surface treatment layer, a PVC layer, an adhesive layer, a PET base cloth layer, an adhesive layer, a PVC layer and an acrylic treatment layer; in terms of weight parts, the preparation of the PVDF surface treatment layer comprises the following raw materials: 21-27 parts of PVDF, 70-80 parts of PMMA, 1-5 parts of modified titanium dioxide, and 80-100 parts of solvent; the preparation of the PVC layer comprises the following raw materials: 45-53 parts of PVC, 28-33 parts of plasticizer, 3-7 parts of heat-resistant modifier, 0.1-0.4 parts of polyethylene wax, 4-7 parts of aluminum hydroxide, 4-7 parts of calcium carbonate, and 0.1-0.5 parts of antioxidant; the preparation of the acrylic treatment layer comprises the following raw materials: 70-80 parts of PMMA, 5-15 parts of PVC, 8-10 parts of diisononyl phthalate, and 0.1-0.5 parts of polyethylene wax. The composite film provided by the invention has the characteristics of good infrared and ultraviolet shielding effect and has good commercial application value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of new energy, and in particular to a high-performance composite membrane and a preparation method thereof. Background Art

[0002] Flexible fabric membrane is a lightweight, high-strength material. It is combined with a support system to form a spatial structure with a stable curved surface and can withstand a certain external load. This material consists of two parts: the central fabric substrate and the coating material. The base fabric is usually made of polyester fiber or glass fiber, while the coating material uses polyvinyl chloride resin (PVC), silicone and polytetrafluoroethylene resin (PTFE). Among them, PTFE is expensive and has high construction requirements. PVC is widely available and inexpensive, but its aging resistance, self-cleaning properties and dimensional stability are not ideal. In order to improve the performance of PVC membrane, a protective layer with good weather resistance is usually coated on its surface. The commonly used material is polyvinylidene fluoride (PVDF). The resulting PVC-PVDF composite membrane has good self-cleaning properties and UV resistance.

[0003] Although PVC-PVDF composite membrane has many excellent characteristics mentioned above, it still has certain defects. For example, in some fields that require strong shielding of infrared and ultraviolet radiation, the infrared and ultraviolet shielding effect of PVDF itself is slightly insufficient, and it is often necessary to add heat-resistant modifiers such as titanium dioxide that have ultraviolet and infrared shielding effects. However, heat-resistant modifiers are easy to agglomerate and have poor dispersion in PVDF. In addition, the poor heat resistance of PVC will limit the application field of the composite membrane and shorten its service life.

[0004] Patent CN 106903955B discloses a composite membrane structure that can be used for building surfaces and its application. The second layer of material in the composite membrane prepared in this application includes a PVC membrane material with glass fiber fabric as the substrate, and PVDF is coated on the outside of the membrane layer. Nano titanium dioxide is added during the last coating to achieve self-cleaning and photocatalytic effects. However, nano titanium dioxide has the problem of poor dispersibility, which may lead to a decrease in the self-cleaning and photocatalytic functions of the composite membrane; Patent CN110511694A discloses a PVDF composite PVC anti-ultraviolet sheet for waterproofing coil and a preparation method. The sheet prepared in this application consists of a PVDF membrane, a glue layer, a PVC main layer, an adhesive layer and a release layer, which overcomes the problem of short exposed sun-resistant life of PVC sheets, but does not solve the problem of poor high temperature resistance of PVC. The problem of insufficient durability and stability still exists only by bonding to increase the service life.

[0005] Therefore, there is an urgent need for a high-performance composite film with good infrared and ultraviolet shielding effects on the market. Summary of the invention

[0006] In view of the problems existing in the prior art, the present invention selects PVDF, PMMA and modified titanium dioxide as raw materials for synthesizing a PVDF surface treatment layer, selects PVC, a heat-resistant modifier and the like as raw materials for synthesizing a PVC layer, and selects PMMA and PVC and the like as raw materials for synthesizing an acrylic treatment layer, and prepares a composite film having a seven-layer structure from top to bottom including a PVDF surface treatment layer, a PVC layer, an adhesive layer, a PET base fabric layer, an adhesive layer, a PVC layer and an acrylic treatment layer, which has the characteristics of good infrared and ultraviolet shielding effects.

[0007] In order to achieve the above object, the technical solution adopted by the present invention is as follows:

[0008] On one hand, the present invention provides a high-performance composite film, which comprises a seven-layer structure from bottom to top, namely: a PVDF surface treatment layer, a PVC layer, an adhesive layer, a PET base fabric layer, an adhesive layer, a PVC layer and an acrylic treatment layer;

[0009] The PVDF surface treatment layer is prepared by the following raw materials: 21-27 parts of PVDF, 70-80 parts of PMMA, 1-5 parts of modified titanium dioxide, and 80-100 parts of solvent.

[0010] The PVC layer is prepared by the following raw materials: 45-53 parts of PVC, 28-33 parts of plasticizer, 3-7 parts of heat-resistant modifier, 0.1-0.4 parts of polyethylene wax, 4-7 parts of aluminum hydroxide, 4-7 parts of calcium carbonate, and 0.1-0.5 parts of antioxidant;

[0011] The acrylic treatment layer is prepared by using the following raw materials: 70-80 parts of PMMA, 5-15 parts of PVC, 8-10 parts of diisononyl phthalate, and 0.1-0.5 parts of polyethylene wax.

[0012] Wherein, the solvent is DMF; and the antioxidant is antioxidant 1076.

[0013] In some embodiments of the present invention, the method for preparing the modified titanium dioxide comprises the following steps:

[0014] (1) Add ammonium fluoride and octadecyl alcohol to a reaction vessel, add octadecene, oleic acid, oleylamine and tetraethyl titanate, stir, introduce inert gas, raise the temperature to 110-130° C., stop introducing inert gas, evacuate, continue introducing inert gas, raise the temperature to 290-310° C., keep warm, cool naturally, add acetone, centrifuge, add n-hexane and ethanol solution, heat to 50-70° C., centrifuge, take solid, dry, grind, and obtain fluorine-doped titanium dioxide;

[0015] (2) Take the fluorine-doped titanium dioxide of step (1), add anhydrous methanol, stir, add glacial acetic acid and N-octyltrimethoxysilane, heat to 40-50° C., reflux, centrifuge, wash, dry, and obtain a product for use;

[0016] (3) Add tannic acid and tin tetrachloride to deionized water, stir, add the product of step (2), heat to 30-40° C., stir, centrifuge, wash, and dry to obtain modified titanium dioxide.

[0017] In some embodiments of the present invention, in step (1), the mass ratio of ammonium fluoride to tetraethyl titanate is 1:(22-23).

[0018] Preferably, in step (1), the mass ratio of ammonium fluoride to tetraethyl titanate is 1:22.5.

[0019] In some embodiments of the present invention, in step (3), the mass ratio of the product, monobutyric acid and tin tetrachloride is 1:(3-4):(5-6).

[0020] Preferably, in step (3), the mass ratio of the product, monobutyric acid and tin tetrachloride is 1:3.4:5.2.

[0021] Titanium dioxide is often used as a heat-resistant modifier added to PVDF film layers due to its excellent properties such as good UV shielding, infrared blocking and high temperature resistance. However, titanium dioxide has a strong polarity and the molecules are attracted by van der Waals forces, which makes them prone to agglomeration. In addition, since PVDF is a non-polar material, the dispersion of titanium dioxide in PVDF is poor, resulting in a decrease in its UV shielding effect and infrared blocking effect.

[0022] On the one hand, the applicant synthesized fluorine-doped titanium dioxide, which improved the hydrophobicity and high temperature resistance of titanium dioxide. The improvement of the hydrophobicity of titanium dioxide is conducive to improving its compatibility in PVDF, thereby improving the dispersibility of titanium dioxide; further, the applicant introduced the silane coupling agent N-octyltrimethoxysilane to modify the fluorine-doped titanium dioxide, introduced a long-chain alkane structure and formed a -Si-O-Si- group, further improving the hydrophobicity of the modified titanium dioxide, thereby improving the dispersibility of the modified titanium dioxide in PVDF; on the other hand, the applicant reacted SnCl4 with monobutyric acid, which contains a large amount of catechol and pyrogallol structures, which can react with SnCl4. 4+ Chelate to form a phenolic network structure, Sn 4+It has good UV shielding effect, can improve the UV shielding property of titanium dioxide, and further react with fluorine-doped titanium dioxide modified by coupling agent to make the modified titanium dioxide have a network structure, thereby improving the dispersibility of the modified titanium dioxide, and the phenolic hydroxyl group of monobutyric acid can form coordination with the metal ions on the surface of titanium dioxide, thereby improving the overall stability of the modified titanium dioxide, and improving the UV shielding effect and infrared blocking effect of the modified titanium dioxide on PVDF.

[0023] In some embodiments of the present invention, the plasticizer is a mixture of diisononyl phthalate, triphenyl phosphate and diisooctyl adipate.

[0024] Preferably, the plasticizer comprises 24-26 parts of diisononyl phthalate, 1-2 parts of triphenyl phosphate, and 3-5 parts of diisooctyl adipate in parts by weight.

[0025] In some embodiments of the present invention, the method for preparing the heat-resistant modifier comprises the following steps:

[0026] 1) Add KH570 to a mixed solution of anhydrous methanol and deionized water, add acetic acid solution dropwise, adjust the pH to 4-5, stir, add methyl methacrylate, tetramethylammonium hydroxide aqueous solution and toluene, stir, distill, and obtain product 1 for standby use;

[0027] 2) Styrene, the product 1 of step 1), N-phenylmaleimide, triallyl isocyanurate, sodium dodecylbenzene sulfonate and deionized water are mixed, stirred, heated to 45-55° C., potassium persulfate is added, stirred, and product 2 is obtained for later use;

[0028] 3) adding styrene, the product 1 of step 1), N-phenylmaleimide, sodium dodecylbenzenesulfonate, deionized water and potassium persulfate to the product 2 of step 2) again, stirring, and obtaining the product 3 for use;

[0029] 4) Mix calcium chloride and deionized water, stir, heat to 60-70°C, add product 3 of step 3), stir, heat to 80-85°C, stop heating, stir, wash, dry, grind, and sieve to obtain a heat-resistant modifier.

[0030] Wherein, the mass ratio of styrene, product 1 and N-phenylmaleimide in step 3) to the same substances used in step 2) is (0.8-1):1.

[0031] Preferably, the mass ratio of styrene, product 1 and N-phenylmaleimide in step 3) to the same substances used in step 2) is 0.9:1.

[0032] In some embodiments of the present invention, in step 1), the mass ratio of KH570 to methyl methacrylate is 1:(0.2-0.6).

[0033] Preferably, in step 1), the mass ratio of KH570 to methyl methacrylate is 1:0.4.

[0034] In some embodiments of the present invention, in step 2), the mass ratio of styrene, product 1, N-phenylmaleimide and triallyl isocyanurate is 1: (0.2-0.3): (1.7-1.8): (0.06-0.1).

[0035] Preferably, in the step 2), the mass ratio of styrene, product 1, N-phenylmaleimide and triallyl isocyanurate is 1:0.25:1.73:0.08.

[0036] PVC, or polyvinyl chloride, is a thermoplastic formed by the polymerization of vinyl chloride monomer. It has good corrosion resistance, insulation, plasticity and mechanical properties, and is inexpensive and widely available. It is widely used in membrane materials and other fields. However, PVC has poor high temperature resistance and is prone to thermal degradation. It is often necessary to use heat-resistant modifiers to blend with PVC to improve the high temperature resistance of PVC, but the addition of heat-resistant modifiers will reduce the toughness of PVC.

[0037] The applicant hydrolyzed KH570 in a mixed solution of anhydrous ethanol and deionized water, and then reacted it with methyl methacrylate for a condensation reaction, and used an aqueous solution of tetramethylammonium hydroxide as a catalyst to synthesize a product 1 having a POSS structure. Silicon atoms and oxygen atoms alternately form the skeleton of the POSS silicon oxygen cage, and each silicon atom is also connected to some organic carbon groups, so that POSS has both a highly ordered inorganic silicon oxygen skeleton and the flexibility of organic groups, which can improve the heat resistance while avoiding the problem of decreased toughness of PVC, and the Si-O-Si structure and the C=O dipole moment on methyl methacrylate synergistically improve the heat resistance of product 1; further, the applicant used product 1, styrene and N-phenylmaleimide as basic raw materials, and used triallyl isocyanurate as a cross-linking agent to synthesize a rigid core (product 2), and then added Product 1, styrene and N-phenylmaleimide are added to synthesize a shell structure (product 3), thereby making the heat-resistant modifier have a core-shell structure. On the one hand, the cross-linking agent triallyl isocyanurate used in the core part of the heat-resistant modifier contains a large proportion of carbon-carbon double bonds, which can make the raw materials such as styrene well cross-linked together, and the isocyanate group and the phenyl group can effectively improve the heat resistance and toughness of the core part; on the other hand, the applicant controls the proportion of the shell-core raw materials used to make the heat-resistant modifier have a suitable particle size, so that it can be well dispersed and compatible in the PVC matrix, thereby greatly improving the heat resistance of PVC; further, the amine group in the N-phenylmaleimide in the heat-resistant modifier can produce a certain cross-linking effect with the phenolic hydroxyl group in the modified titanium dioxide, which can improve the adhesion between the PVDF layer and the PVC film layer to a certain extent.

[0038] In some embodiments of the present invention, the adhesive layer is an acrylate pressure-sensitive adhesive.

[0039] Another aspect of the present invention further provides a method for preparing the high-performance composite membrane described in the above technical solution, comprising the following steps:

[0040] S1, mixing PVDF, PMMA, modified titanium dioxide and solvent, stirring to obtain PVDF slurry for standby use;

[0041] S2, mixing PVC and plasticizer, stirring, adding heat-resistant modifier, polyethylene wax, aluminum hydroxide, calcium carbonate and antioxidant, stirring, and obtaining PVC slurry for standby use;

[0042] S3, PMMA, PVC, diisononyl phthalate and polyethylene wax are mixed, stirred, extruded at 140-150° C. to a thickness of 70-80 μm, and cooled to room temperature to obtain an acrylic treatment layer for standby use;

[0043] S4, coating the PVC slurry of step S2 on one side of the acrylic treatment layer of step S3, drying to obtain a PVC layer with a thickness of 200-250 μm, then coating the acrylate pressure-sensitive adhesive on the PVC layer, drying to obtain an adhesive layer with a thickness of 150-200 μm, then placing a PET base fabric layer with a thickness of 450-550 μm on the adhesive layer, hot pressing at 140-150° C., 6-8 MPa for 3-5 min to form, then coating the PVC slurry of step S2 on the PET base fabric layer, drying to form a PVC layer with a thickness of 200-250 μm, then coating the PVDF slurry of step S1 on the PVC layer, drying to form a PVDF surface treatment layer with a thickness of 70-100 μm, hot pressing at 140-150° C., 6-8 MPa for 3-5 min to form, and thus obtaining a high-performance composite membrane.

[0044] Compared with the prior art, the present invention has the following beneficial effects:

[0045] (1) The present invention uses PVDF, PMMA and modified titanium dioxide as raw materials for synthesizing a PVDF surface treatment layer, uses PVC, a heat-resistant modifier and the like as raw materials for synthesizing a PVC layer, and uses PMMA and PVC and the like as raw materials for synthesizing an acrylic treatment layer, and prepares a composite film having a seven-layer structure from top to bottom, including a PVDF surface treatment layer, a PVC layer, an adhesive layer, a PET base fabric layer, an adhesive layer, a PVC layer and an acrylic treatment layer. Through the synergistic effect of the various components, the composite film has the characteristics of good infrared and ultraviolet shielding effects.

[0046] (2) The present invention uses titanium dioxide as raw material, performs fluorine doping modification, and uses Sn 4+ The phenolic network structure is formed by chelation, and reacts with fluorine-doped titanium dioxide to synthesize modified titanium dioxide, thereby improving the dispersibility and stability of titanium dioxide in PVDF, thereby improving the ultraviolet shielding and infrared blocking effects of the composite film.

[0047] (3) The present invention synthesizes a heat-resistant modifier to improve the heat resistance of PVC, and at the same time solves the problem that the heat-resistant modifier easily reduces the toughness of PVC, and plays a role in improving the adhesion between the PVDF layer and the PVC film layer.

[0048] (4) The composite film prepared by the present invention has the advantage of good infrared and ultraviolet shielding effect, can be widely used in the field of new energy, and has good commercial application value. DETAILED DESCRIPTION

[0049] The present invention will be described below in conjunction with specific embodiments. It should be noted that the following embodiments are examples of the present invention and are only used to illustrate the present invention, but not to limit the present invention. Other combinations and various modifications within the concept of the present invention may be performed without departing from the spirit or scope of the present invention.

[0050] In the following embodiments and comparative examples, except for modified titanium dioxide and heat-resistant modifier, the other compound monomers and related reagents used can be purchased from the market, among which, the model of PVDF is Solef 9007, purchased from Dongguan Suguang Plastic Raw Materials Co., Ltd.; the model of PMMA is CM-207, purchased from Qingdao Zhongxin Huamei Plastic Co., Ltd.; the model of PVC is SG-7, purchased from Tianjin Dagu Chemical Co., Ltd.; polyethylene wax is purchased from Shandong Baolilai Plastic Additive Co., Ltd.; the thickness of the PET base fabric layer is 500 μm, purchased from Dongguan Wenxuan New Materials Co., Ltd.; and the acrylic pressure-sensitive adhesive is purchased from Suzhou Baoxin New Materials Co., Ltd.

[0051] Preparation Example 1

[0052] The synthesis method of modified titanium dioxide A comprises the following steps:

[0053] (1) 0.2 g of ammonium fluoride and 54 g of octadecyl alcohol were added to a reaction vessel, and 160 ml of octadecene, 10 ml of oleic acid, 10 ml of oleylamine and 4.5 g of tetraethyl titanate were added, stirred for 30 min, introduced with N2, heated to 120 °C, stopped introducing with N2, evacuated for 20 min, continued introducing with N2, heated to 300 °C, kept warm for 1 h, cooled naturally for 30 min, added with 30 ml of acetone, centrifuged once, added with 10 ml of n-hexane and 30 ml of 50 wt% ethanol solution, heated to 60 °C, centrifuged 4 times, took the solid, dried at 60 °C for 12 h, and ground for 5 min to obtain fluorine-doped titanium dioxide;

[0054] (2) Take 0.5 g of the fluorine-doped titanium dioxide prepared in step (1), add 50 ml of anhydrous methanol, stir for 45 min, add 1 ml of glacial acetic acid and 0.2 ml of N-octyltrimethoxysilane, heat to 45 ° C, reflux for 30 min, centrifuge, wash twice with anhydrous ethanol and deionized water, dry at 100 ° C for 24 h, and obtain the product for use;

[0055] (3) Mix 1.7 g of tannic acid, 2.6 g of tin tetrachloride and 100 ml of deionized water, stir for 1 h, add 0.5 g of the product of step (2), heat to 35 ° C, stir for 30 min, centrifuge, wash with deionized water 3 times, and dry at 60 ° C for 12 h to obtain modified titanium dioxide A.

[0056] Preparation Example 2

[0057] The specific implementation method of modified titanium dioxide B is the same as that of modified titanium dioxide A, except that in step (1), the mass of tetraethyl titanate is replaced by 4 g.

[0058] Preparation Example 3

[0059] The specific implementation method of modified titanium dioxide C is the same as that of modified titanium dioxide A, except that in step (3), the mass of tannic acid is replaced with 1.2 g.

[0060] Preparation Example 4

[0061] The specific implementation method of modified titanium dioxide D is the same as that of modified titanium dioxide A, except that in step (3), the mass of tin tetrachloride is replaced by 2 g.

[0062] Preparation Example 5

[0063] The synthesis method of heat-resistant modifier A comprises the following steps:

[0064] 1) Add 20g KH570 to a mixed solution of 180ml anhydrous methanol and 20ml deionized water, add 5wt% acetic acid solution dropwise, adjust the pH to 4.5, stir for 2h, add 8g methyl methacrylate, 1g 25wt% tetramethylammonium hydroxide aqueous solution and 20ml toluene, stir for 2h, distill, and obtain product 1 for use;

[0065] 2) 30 g of styrene, 7.5 g of the product 1 of step 1), 52 g of N-phenylmaleimide, 2.4 g of triallyl isocyanurate, 0.9 g of sodium dodecylbenzenesulfonate and 75 ml of deionized water were mixed, stirred for 3 h, heated to 50° C., 6.3 g of potassium persulfate was added, stirred for 3 h, and product 2 was obtained for later use;

[0066] 3) 27 g of styrene, 6.75 g of the product 1 of step 1), 46.8 g of N-phenylmaleimide, 0.9 g of sodium dodecylbenzenesulfonate, 70 ml of deionized water and 5.7 g of potassium persulfate were added to the product 2 of step 2) again, and the mixture was stirred for 3 h to obtain the product 3 for use;

[0067] 4) Mix 0.5 g of calcium chloride and 50 ml of deionized water, stir for 30 min, heat to 65 ° C, add 30 g of product 3 of step 3), stir for 1 h, heat to 80 ° C, stop heating, stir for 3 min, wash with deionized water 3 times, dry at 65 ° C for 10 h, grind, and pass through a 20-mesh sieve to obtain heat-resistant modifier A.

[0068] Preparation Example 6

[0069] Heat-resistant modifier B, the specific implementation manner is the same as that of heat-resistant modifier A, except that: in step 1), the mass of methyl methacrylate is replaced with 3 g.

[0070] Preparation Example 7

[0071] Heat-resistant modifier C, the specific implementation method is the same as that of heat-resistant modifier A, except that: in step 2), the mass of product 1 is replaced with 5g.

[0072] Preparation Example 8

[0073] Heat-resistant modifier D, the specific implementation manner is the same as that of heat-resistant modifier A, except that: in step 2), the mass of N-phenylmaleimide is replaced with 49 g.

[0074] Preparation Example 9

[0075] Heat-resistant modifier E, the specific implementation manner is the same as that of heat-resistant modifier A, except that: in step 2), the mass of triallyl isocyanurate is replaced with 1.5 g.

[0076] Example 1

[0077] A high-performance composite film, the composite film includes a seven-layer structure from bottom to top, namely: a PVDF surface treatment layer, a PVC layer, an adhesive layer, a PET base fabric layer, an adhesive layer, a PVC layer and an acrylic treatment layer;

[0078] The PVDF surface treatment layer includes the following raw materials in parts by weight: 24 parts of PVDF, 75 parts of PMMA, 3 parts of modified titanium dioxide A, and 90 parts of DMF;

[0079] The PVC layer includes the following raw materials: 49 parts of PVC, 30.5 parts of plasticizer, 5 parts of heat-resistant modifier A, 0.25 parts of polyethylene wax, 5.5 parts of aluminum hydroxide, 5.5 parts of calcium carbonate, 0.3 parts of antioxidant 1076,

[0080] The plasticizer includes 25 parts of diisononyl phthalate, 1.5 parts of triphenyl phosphate, and 4 parts of diisooctyl adipate;

[0081] The acrylic treatment layer includes the following raw materials: 75 parts of PMMA, 10 parts of PVC, 9 parts of diisononyl phthalate, and 0.3 parts of polyethylene wax.

[0082] The preparation method of the high performance composite membrane in this embodiment comprises the following steps:

[0083] S1, PVDF, PMMA, modified titanium dioxide A and DMF were mixed and stirred for 30 minutes to obtain PVDF slurry for standby use;

[0084] S2, PVC and plasticizer are mixed, stirred for 30 minutes, heat-resistant modifier A, polyethylene wax, aluminum hydroxide, calcium carbonate and antioxidant 1076 are added, and stirred for 30 minutes to obtain PVC slurry for standby use;

[0085] S3, PMMA, PVC, diisononyl phthalate and polyethylene wax are mixed, stirred for 30 minutes, extruded at 145° C. to a thickness of 75 μm, and cooled to room temperature to obtain an acrylic treatment layer for standby use;

[0086] S4, coating the PVC slurry of step S2 on one side of the acrylic treatment layer of step S3, drying at 65°C for 15 minutes to obtain a PVC layer with a thickness of 230 μm, then coating the acrylate pressure-sensitive adhesive on the PVC layer, drying at 65°C for 15 minutes to obtain an adhesive layer with a thickness of 180 μm, then placing a PET base fabric layer with a thickness of 500 μm on the adhesive layer, hot pressing at 145°C and 7 MPa for 4 minutes to form a PVC layer with a thickness of 230 μm, then coating the PVC slurry of step S2 on the PET base fabric layer, drying at 65°C for 15 minutes to form a PVC layer with a thickness of 230 μm, then coating the PVDF slurry of step S1 on the PVC layer, drying at 65°C for 15 minutes to form a PVDF surface treatment layer with a thickness of 85 μm, hot pressing at 145°C and 7 MPa for 4 minutes to form a high-performance composite membrane.

[0087] Example 2

[0088] A high-performance composite film, the composite film includes a seven-layer structure from bottom to top, namely: a PVDF surface treatment layer, a PVC layer, an adhesive layer, a PET base fabric layer, an adhesive layer, a PVC layer and an acrylic treatment layer;

[0089] The PVDF surface treatment layer includes the following raw materials in parts by weight: 21 parts of PVDF, 70 parts of PMMA, 3 parts of modified titanium dioxide A, and 80 parts of DMF;

[0090] The PVC layer includes the following raw materials: 45 parts of PVC, 28 parts of plasticizer, 3 parts of heat-resistant modifier A, 0.1 parts of polyethylene wax, 4 parts of aluminum hydroxide, 4 parts of calcium carbonate, 0.1 parts of antioxidant 1076,

[0091] The plasticizer includes 24 parts of diisononyl phthalate, 1 part of triphenyl phosphate, and 3 parts of diisooctyl adipate;

[0092] The acrylic treatment layer includes the following raw materials: 70 parts of PMMA, 5 parts of PVC, 8 parts of diisononyl phthalate, and 0.1 parts of polyethylene wax.

[0093] The preparation method of the high performance composite membrane in this embodiment comprises the following steps:

[0094] S1, PVDF, PMMA, modified titanium dioxide A and DMF were mixed and stirred for 30 minutes to obtain PVDF slurry for standby use;

[0095] S2, PVC and plasticizer are mixed, stirred for 30 minutes, heat-resistant modifier A, polyethylene wax, aluminum hydroxide, calcium carbonate and antioxidant 1076 are added, and stirred for 30 minutes to obtain PVC slurry for standby use;

[0096] S3, PMMA, PVC, diisononyl phthalate and polyethylene wax are mixed, stirred for 30 minutes, extruded at 140° C. to a thickness of 70 μm, and cooled to room temperature to obtain an acrylic treatment layer for standby use;

[0097] S4, coating the PVC slurry of step S2 on one side of the acrylic treatment layer of step S3, drying at 65°C for 15 min to obtain a PVC layer with a thickness of 200 μm, then coating the acrylate pressure-sensitive adhesive on the PVC layer, drying at 65°C for 15 min to obtain an adhesive layer with a thickness of 150 μm, then placing a PET base fabric layer with a thickness of 500 μm on the adhesive layer, hot pressing at 140°C and 6 MPa for 5 min to form a PVC layer with a thickness of 200 μm, then coating the PVC slurry of step S2 on the PET base fabric layer, drying at 65°C for 15 min to form a PVC layer with a thickness of 200 μm, then coating the PVDF slurry of step S1 on the PVC layer, drying at 65°C for 15 min to form a PVDF surface treatment layer with a thickness of 70 μm, hot pressing at 140°C and 6 MPa for 5 min to form a high-performance composite membrane.

[0098] Example 3

[0099] A high-performance composite film, the composite film includes a seven-layer structure from bottom to top, namely: a PVDF surface treatment layer, a PVC layer, an adhesive layer, a PET base fabric layer, an adhesive layer, a PVC layer and an acrylic treatment layer;

[0100] The PVDF surface treatment layer includes the following raw materials in parts by weight: 27 parts of PVDF, 80 parts of PMMA, 3 parts of modified titanium dioxide A, and 100 parts of DMF;

[0101] The PVC layer includes the following raw materials: 53 parts of PVC, 33 parts of plasticizer, 7 parts of heat-resistant modifier A, 0.4 parts of polyethylene wax, 7 parts of aluminum hydroxide, 7 parts of calcium carbonate, 0.5 parts of antioxidant 1076,

[0102] The plasticizer includes 26 parts of diisononyl phthalate, 2 parts of triphenyl phosphate, and 5 parts of diisooctyl adipate;

[0103] The acrylic treatment layer includes the following raw materials: 80 parts of PMMA, 15 parts of PVC, 10 parts of diisononyl phthalate, and 0.5 parts of polyethylene wax.

[0104] The preparation method of the high performance composite membrane in this embodiment comprises the following steps:

[0105] S1, PVDF, PMMA, modified titanium dioxide A and DMF were mixed and stirred for 30 minutes to obtain PVDF slurry for standby use;

[0106] S2, PVC and plasticizer are mixed, stirred for 30 minutes, heat-resistant modifier A, polyethylene wax, aluminum hydroxide, calcium carbonate and antioxidant 1076 are added, and stirred for 30 minutes to obtain PVC slurry for standby use;

[0107] S3, PMMA, PVC, diisononyl phthalate and polyethylene wax are mixed, stirred for 30 minutes, extruded at 150° C. to a thickness of 80 μm, and cooled to room temperature to obtain an acrylic treatment layer for standby use;

[0108] S4, coating the PVC slurry of step S2 on one side of the acrylic treatment layer of step S3, drying at 65°C for 15 minutes to obtain a PVC layer with a thickness of 250 μm, then coating the acrylate pressure-sensitive adhesive on the PVC layer, drying at 65°C for 15 minutes to obtain an adhesive layer with a thickness of 200 μm, then placing a PET base fabric layer with a thickness of 550 μm on the adhesive layer, hot pressing at 150°C and 8 MPa for 5 minutes to form a PVC layer with a thickness of 250 μm, then coating the PVC slurry of step S2 on the PET base fabric layer, drying at 65°C for 15 minutes to form a PVC layer with a thickness of 250 μm, then coating the PVDF slurry of step S1 on the PVC layer, drying at 65°C for 15 minutes to form a PVDF surface treatment layer with a thickness of 100 μm, hot pressing at 150°C and 8 MPa for 3 minutes to form a high-performance composite membrane.

[0109] Example 4

[0110] A high-performance composite film, the composite film includes a seven-layer structure from bottom to top, namely: a PVDF surface treatment layer, a PVC layer, an adhesive layer, a PET base fabric layer, an adhesive layer, a PVC layer and an acrylic treatment layer;

[0111] The PVDF surface treatment layer includes the following raw materials in parts by weight: 22 parts of PVDF, 72 parts of PMMA, 1 part of modified titanium dioxide A, and 85 parts of DMF;

[0112] The PVC layer includes the following raw materials: 46 parts of PVC, 30.5 parts of plasticizer, 5 parts of heat-resistant modifier A, 0.2 parts of polyethylene wax, 5 parts of aluminum hydroxide, 5 parts of calcium carbonate, 0.2 parts of antioxidant 1076,

[0113] The plasticizer is the same as in Example 1;

[0114] The acrylic treatment layer includes the following raw materials: 72 parts of PMMA, 6 parts of PVC, 8.5 parts of diisononyl phthalate, and 0.2 parts of polyethylene wax.

[0115] The preparation method of the high performance composite membrane in this embodiment is the same as that in Embodiment 1.

[0116] Example 5

[0117] A high-performance composite film, the composite film includes a seven-layer structure from bottom to top, namely: a PVDF surface treatment layer, a PVC layer, an adhesive layer, a PET base fabric layer, an adhesive layer, a PVC layer and an acrylic treatment layer;

[0118] The PVDF surface treatment layer includes the following raw materials in parts by weight: 26 parts of PVDF, 78 parts of PMMA, 5 parts of modified titanium dioxide A, and 95 parts of DMF;

[0119] The PVC layer includes the following raw materials: 52 parts of PVC, 30.5 parts of plasticizer, 5 parts of heat-resistant modifier A, 0.3 parts of polyethylene wax, 6 parts of aluminum hydroxide, 6 parts of calcium carbonate, 0.4 parts of antioxidant 1076,

[0120] The plasticizer is the same as in Example 1;

[0121] The acrylic treatment layer includes the following raw materials: 78 parts of PMMA, 13 parts of PVC, 9.5 parts of diisononyl phthalate, and 0.4 parts of polyethylene wax.

[0122] The preparation method of the high performance composite membrane in this embodiment is the same as that in Embodiment 1.

[0123] Example 6

[0124] This embodiment provides a high-performance composite membrane and a preparation method thereof. The specific implementation method is the same as that of Embodiment 1, except that modified titanium dioxide B replaces modified titanium dioxide A in equal amounts.

[0125] Example 7

[0126] This embodiment provides a high-performance composite membrane and a preparation method thereof. The specific implementation method is the same as that of Embodiment 1, except that modified titanium dioxide C replaces modified titanium dioxide A in equal amounts.

[0127] Example 8

[0128] This embodiment provides a high-performance composite membrane and a preparation method thereof. The specific implementation method is the same as that of Embodiment 1, except that modified titanium dioxide D replaces modified titanium dioxide A in equal amounts.

[0129] Example 9

[0130] This embodiment provides a high-performance composite membrane and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that the heat-resistant modifier A is replaced by the heat-resistant modifier B in equal amounts.

[0131] Example 10

[0132] This embodiment provides a high-performance composite membrane and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that the heat-resistant modifier A is replaced by the heat-resistant modifier C in equal amounts.

[0133] Embodiment 11

[0134] This embodiment provides a high-performance composite membrane and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that the heat-resistant modifier A is replaced by the heat-resistant modifier D in equal amounts.

[0135] Example 12

[0136] This embodiment provides a high-performance composite membrane and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that the heat-resistant modifier A is replaced by the heat-resistant modifier E in equal amounts.

[0137] Embodiment 13

[0138] This embodiment provides a high-performance composite membrane and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that an equal amount of N-phenylmaleimide is used to replace the heat-resistant modifier A.

[0139] Comparative Example 1

[0140] This comparative example provides a high-performance composite membrane and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that an equal amount of titanium dioxide is used to replace the modified titanium dioxide A.

[0141] Performance Testing

[0142] The infrared and ultraviolet shielding properties of the high-performance composite films of Examples 1-13 and Comparative Example 1 were tested. The test results are shown in Table 1.

[0143] The composite film was subjected to UV / NIR diffuse reflectance test using a Shimadzu UV-3600iPlus UV / NIR spectrophotometer from Japan.

[0144] Table 1

[0145] Group UV blocking rate (%) Infrared reflectivity (%) Example 1 99.99 80.545 Example 2 99.97 80.321 Example 3 99.97 80.243 Example 4 99.95 80.154 Example 5 99.96 80.035 Example 6 96.62 78.832 Example 7 96.60 78.825 Example 8 96.57 78.765 Example 9 97.32 79.254 Example 10 97.30 79.241 Embodiment 11 97.32 79.235 Example 12 97.29 79.230 Embodiment 13 97.15 78.125 Comparative Example 1 95.44 78.254

[0146] From the data in Table 1, it can be seen that the composite films in Examples 1-5 of the present invention have the characteristics of high ultraviolet blocking rate and high infrared reflectivity. In general, the infrared reflectivity of the composite films synthesized in the examples and comparative examples shows good results. 4+ The ratio of the modified titanium dioxide to react with tannic acid to form a phenolic chelating network reduces the dispersibility and stability of the modified titanium dioxide, resulting in a decrease in the UV shielding effect of the modified titanium dioxide on the composite film, and then the phenomenon of a decrease in the UV blocking rate of the composite film; Examples 9-12 change the ratio of the key components when synthesizing the heat-resistant modifier, which reduces the heat resistance and toughness of the heat-resistant modifier, and does not significantly improve the heat resistance of PVC, that is, the phenomenon of a decrease in the UV blocking rate of the composite film is manifested; Example 13 and Comparative Example 1 respectively use N-phenylmaleimide and titanium dioxide to replace the heat-resistant modifier A and modified titanium dioxide A, and the test finds that the UV shielding performance of the composite film shows poor results.

[0147] The above implementation modes are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with this technology to understand the content of the present invention and implement it, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.

Claims

1. A high-performance composite membrane, characterized in that: The composite film comprises a seven-layer structure from top to bottom, which are: a PVDF surface treatment layer, a PVC layer, an adhesive layer, a PET base fabric layer, an adhesive layer, a PVC layer and an acrylic treatment layer; The PVDF surface treatment layer is prepared from the following raw materials in parts by weight: 21-27 parts of PVDF, 70-80 parts of PMMA, 1-5 parts of modified titanium dioxide, and 80-100 parts of solvent; The PVC layer is prepared from the following raw materials: 45-53 parts of PVC, 28-33 parts of plasticizer, 3-7 parts of heat-resistant modifier, 0.1-0.4 parts of polyethylene wax, 4-7 parts of aluminum hydroxide, 4-7 parts of calcium carbonate, and 0.1-0.5 parts of antioxidant; The acrylic treatment layer is prepared from the following raw materials: 70-80 parts of PMMA, 5-15 parts of PVC, 8-10 parts of diisononyl phthalate, and 0.1-0.5 parts of polyethylene wax; The preparation method of the modified titanium dioxide comprises the following steps: (1) Add ammonium fluoride and octadecyl alcohol to a reaction vessel, add octadecene, oleic acid, oleylamine and tetraethyl titanate, stir, introduce inert gas, raise the temperature to 110-130° C., stop introducing inert gas, evacuate, continue introducing inert gas, raise the temperature to 290-310° C., keep warm, cool naturally, add acetone, centrifuge, add n-hexane and ethanol solution, heat to 50-70° C., centrifuge, take solid, dry, grind, and obtain fluorine-doped titanium dioxide; (2) Take the fluorine-doped titanium dioxide of step (1), add anhydrous methanol, stir, add glacial acetic acid and N-octyltrimethoxysilane, heat to 40-50° C., reflux, centrifuge, wash, dry, and obtain a product for use; (3) Add tannic acid and tin tetrachloride to deionized water, stir, add the product of step (2), heat to 30-40°C, stir, centrifuge, wash, and dry to obtain modified titanium dioxide. In the preparation method of modified titanium dioxide, the mass ratio of ammonium fluoride to tetraethyl titanate in step (1) is 1:(22-23), and in step (3), the mass ratio of the product, monobutyric acid and tin tetrachloride is 1:(3-4):(5-6); The preparation method of the heat-resistant modifier comprises the following steps: 1) Add KH570 to a mixed solution of anhydrous methanol and deionized water, add acetic acid solution dropwise, adjust the pH to 4-5, stir, add methyl methacrylate, tetramethylammonium hydroxide aqueous solution and toluene, stir, distill, and obtain product 1 for standby use; 2) Styrene, the product 1 of step 1), N-phenylmaleimide, triallyl isocyanurate, sodium dodecylbenzene sulfonate and deionized water are mixed, stirred, heated to 45-55° C., potassium persulfate is added, stirred, and product 2 is obtained for later use; 3) adding styrene, the product 1 of step 1), N-phenylmaleimide, sodium dodecylbenzenesulfonate, deionized water and potassium persulfate to the product 2 of step 2) again, stirring, and obtaining the product 3 for use; 4) Mix calcium chloride and deionized water, stir, heat to 60-70°C, add product 3 from step 3), stir, heat to 80-85°C, stop heating, stir, wash, dry, grind, and sieve to obtain a heat-resistant modifier. In the preparation method of the heat-resistant modifier, in step 1), the mass ratio of KH570 to methyl methacrylate is 1:(0.2-0.6), and in step 2), the mass ratio of styrene, product 1, N-phenylmaleimide and triallyl isocyanurate is 1:(0.2-0.3):(1.7-1.8):(0.06-0.1).

2. The high performance composite membrane according to claim 1, characterized in that: The plasticizer is a mixture of diisononyl phthalate, triphenyl phosphate and diisooctyl adipate.

3. The high performance composite membrane according to claim 1, characterized in that: The adhesive layer is an acrylic pressure-sensitive adhesive.