Novel composite cement grinding aid and preparation method thereof
By combining red mud with plant straw modified biochar and alcoholamine compounds, a composite cement grinding aid is prepared, which solves the problems of insufficient functionality of existing grinding aids and complicated production processes, and achieves more efficient cement production and Increased strength.
Patent Information
- Application Number
- CN202411027016.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-07-30
AI Technical Summary
Existing cement grinding aids have a single functional group and a narrow range of applications, resulting in poor grinding effect. At the same time, due to the complex production process, there are products with unstable quality on the market, which affects the quality of building materials.
A new type of composite cement grinding aid is prepared by using solid waste red mud and plant straw comprehensively modified biochar materials, combined with alcoholamine compounds, and through a specific proportion of synergy, to improve the grindability and hydration power of the material, thereby improving Early and late strength of cement.
It improves the utilization rate of solid waste, reduces production costs, significantly increases the hourly output and strength of cement, extends the service life of base materials, and improves grinding efficiency and cement particle distribution.
Smart Images

Figure CN118754498A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of cement additives, and particularly relates to a novel composite cement grinding aid and a preparation method thereof. Background Art
[0002] Cement grinding aids can significantly reduce the electrostatic adsorption and balling phenomenon formed during the grinding process, and can reduce the tendency of re-agglomeration of ultrafine particles formed during the grinding process. Cement grinding aids can also significantly improve cement fluidity, improve the grinding effect of the mill and the powder selection efficiency of the powder classifier. As a chemical additive, grinding aids can also improve the distribution of cement particles and stimulate hydration dynamics, thereby improving the early and later strength of cement. Cement grinding aids have been developed to date, and they have a certain improvement effect on increasing the hourly output of cement mills and the strength of cement at various ages, and are widely used in the production lines of major cement plants.
[0003] There are many varieties of grinding aids, and their grinding aid effects vary greatly, which also have different degrees of influence on cement performance. However, most of the current domestic grinding aids are ethanolamines and alcohol compounds, but the functional groups of single ethanolamines and alcohol compounds are relatively simple, and the application range of materials is relatively narrow, which limits the grinding aid effect of the grinding aid. In addition, since the production process of cement grinding aids is relatively complicated and the manufacturing process level is uneven, there are many cement grinding aids with unstable quality on the market, and the use of these low-quality products may cause the quality of building materials to decrease. Therefore, preparing a cement grinding aid with more stable quality and more excellent grinding aid enhancement performance has a wide market value and application prospects. Summary of the invention
[0004] The purpose of the present invention is to provide a new composite cement grinding aid, which uses solid waste red mud and plant straw to comprehensively modify biochar materials as raw materials, which, on the one hand, improves the utilization rate of solid waste red mud and plant straw and reduces production costs; on the other hand, the biochar modified by red mud and the alcoholamine compound act synergistically according to a specific ratio to improve the grindability of the material and increase the hourly output of cement. At the same time, it can also improve the distribution of cement particles and stimulate the hydration dynamics, thereby improving the early strength and late strength of cement.
[0005] In order to achieve the above technical objectives, the technical solution adopted by the present invention is: A novel composite cement grinding aid is prepared from the following raw materials in parts by weight: 30-40 parts of alcoholamine compounds, 10-15 parts of sodium sulfite, 20-30 parts of red mud modified biochar, 5-10 parts of dilauryl thiodipropionate, 5-10 parts of sodium humate, 5-10 parts of molasses and 30-40 parts of water.
[0006] Preferably, the alcoholamine compound is composed of monoethanol diisopropanolamine and diisopropyl monoethanolamine in a mass ratio of 2:1.
[0007] Preferably, the red mud modified biochar is prepared by the following method: (1) Add red mud into deionized water and stir for 30 minutes to obtain a red mud suspension; (2) Clean the plant straw and grind it into fine powder, add the plant straw powder into the red mud suspension and continue stirring for 1 hour, then filter, and dry the solid mixture in an oven to obtain a pretreated mixture; (3) The pretreated mixture was placed in a nitrogen tubular furnace and heated to 750 °C at a set heating rate. The mixture was kept warm for 2 h under nitrogen protection and then naturally cooled to room temperature and ground into fine powder. The powder was then sieved through a 40-mesh sieve to obtain red mud modified biochar.
[0008] Preferably, in step (1), the ratio of red mud to deionized water is 20 g:100 ml.
[0009] Preferably, the plant straw is corn straw or wheat straw.
[0010] Preferably, the usage ratio of the plant straw powder to the red mud suspension is 10g:100ml.
[0011] Preferably, in step (3), the heating rate of the nitrogen tubular furnace is 10°C / min to 350°C, and then 20°C / min to 750°C.
[0012] The present invention also provides a method for preparing the novel composite cement grinding aid, comprising the following steps: S1: The amine compounds are mixed in proportion, and then mixed with the red mud modified biochar, and stirred at a speed of 800 r / min for 15 min to obtain a uniformly dispersed mixture; S2: Evenly mix the remaining materials with the mixture obtained in S1 to obtain a new composite cement grinding aid.
[0013] The raw materials used in the present invention are all commercially available.
[0014] The designed dosage of the grinding aid of the present invention is 0.05-0.08%.
[0015] Red mud, also known as bauxite residue, is an industrial byproduct produced during the extraction of alumina from bauxite. As of 2020, the global stock of red mud has exceeded 5 billion tons, of which my country's stock exceeds 800 million tons. Due to the high cost of safe disposal of red mud, the current disposal method for red mud mainly adopts dry stacking, which causes serious waste of land resources and also brings a lot of pollution problems. Therefore, it is very necessary to make comprehensive resource utilization of red mud. Red mud itself has a unique structure rich in oxides (especially iron and aluminum oxides), surface hydroxyls and porosity. The biochar modified by red mud forms a stable chemical bond with the red mud, which improves the porosity and specific surface area of the biochar, enhances the reaction activity and adsorption capacity of the biochar, and can be adsorbed on the surface of cement particles, enhances the adsorption capacity of the material, prevents the spread of cracks, and improves the grindability of the material. At the same time, since red mud contains aluminum oxide and cement mineral component dicalcium silicate, dicalcium silicate has a seeding effect in the cement production process, which can improve the burnability of the raw material and reduce the burning temperature of the clinker. The alcoholamine compounds used in the present invention can work together with the red mud modified biochar to form a complex with iron and aluminum oxides, which can promote the hydration of C4AF to generate AFt, change the amount of Ca(OH)2 in the cement stone hydration process, and then accelerate the hydration of silicate minerals, stimulate the activity of cement materials, and thus increase the strength of cement.
[0016] The beneficial effects of the present invention are: 1) The present invention uses red mud modified biochar prepared by co-modifying solid waste red mud and plant straw as raw material, which improves the comprehensive utilization rate of solid waste and reduces the production cost of grinding aids. At the same time, the prepared red mud modified biochar forms a stable chemical bond with red mud, improves the porosity and specific surface area of the biochar, enhances the reaction activity and adsorption capacity of the biochar, can be adsorbed on the surface of cement particles, enhances the adsorption capacity of the material, prevents the spread of cracks, improves the grindability of the material, and can significantly increase the hourly output of cement production.
[0017] 2) The red mud modified biochar of the present invention has a synergistic effect with the alcoholamine compound, which can improve the grinding efficiency and significantly improve the strength of cement, thereby extending the service life of cement-based materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 The SEM comparison pictures of the biochar used in the present invention before and after modification with red mud, wherein a) is the biochar before modification, and b) is the biochar after modification with red mud; DETAILED DESCRIPTION The technical solution of the present invention is further described below in conjunction with specific embodiments, but is not limited thereto.
[0019] The red mud used in the present invention comes from the solid waste discharged from the Bayer process of preparing alumina in an aluminum plant in Shandong. Its specific chemical composition is shown in Table 1.
[0020] Table 1 Chemical composition of red mud Example 1 A novel composite cement grinding aid is prepared from the following raw materials in parts by weight: 30 parts of alcoholamine compounds, 10 parts of sodium sulfite, 20 parts of red mud modified biochar, 5 parts of dilauryl thiodipropionate, 5 parts of sodium humate, 5 parts of molasses, and 30 parts of water.
[0021] The alcoholamine compound is composed of monoethanol diisopropanolamine and diisopropyl monoethanolamine in a mass ratio of 2:1.
[0022] The red mud modified biochar is prepared by the following method: (1) Add red mud into deionized water and stir for 30 minutes to obtain a red mud suspension; (2) Clean the plant straw and grind it into fine powder, add the plant straw powder into the red mud suspension and continue stirring for 1 hour, then filter, and dry the solid mixture in an oven to obtain a pretreated mixture; (3) The pretreated mixture was placed in a nitrogen tubular furnace and heated to 750 °C at a set heating rate. The mixture was kept warm for 2 h under nitrogen protection and then naturally cooled to room temperature and ground into fine powder. The powder was then sieved through a 40-mesh sieve to obtain red mud modified biochar.
[0023] In the step (1), the ratio of red mud to deionized water is 20 g:100 ml.
[0024] The plant straw is corn straw or wheat straw.
[0025] The usage ratio of the plant straw powder to the red mud suspension is 10g:100ml.
[0026] In step (3), the heating rate of the nitrogen tubular furnace is 10°C / min to 350°C, and then 20°C / min to 750°C.
[0027] A method for preparing the novel composite cement grinding aid comprises the following steps: S1: The amine compounds are mixed in proportion, and then mixed with the red mud modified biochar, and stirred at a speed of 800 r / min for 15 min to obtain a uniformly dispersed mixture; S2: Evenly mix the remaining materials with the mixture obtained in S1 to obtain a new composite cement grinding aid.
[0028] Example 2 A novel composite cement grinding aid is prepared from the following raw materials in parts by weight: 40 parts of alcoholamine compounds, 15 parts of sodium sulfite, 30 parts of red mud modified biochar, 10 parts of dilauryl thiodipropionate, 10 parts of sodium humate, 10 parts of molasses, and 40 parts of water.
[0029] The alcoholamine compound is composed of monoethanol diisopropanolamine and diisopropyl monoethanolamine in a mass ratio of 2:1.
[0030] The red mud modified biochar is prepared by the following method: (1) Add red mud into deionized water and stir for 30 minutes to obtain a red mud suspension; (2) Clean the plant straw and grind it into fine powder, add the plant straw powder into the red mud suspension and continue stirring for 1 hour, then filter, and dry the solid mixture in an oven to obtain a pretreated mixture; (3) The pretreated mixture was placed in a nitrogen tubular furnace and heated to 750 °C at a set heating rate. The mixture was kept warm for 2 h under nitrogen protection and then naturally cooled to room temperature and ground into fine powder. The powder was then sieved through a 40-mesh sieve to obtain red mud modified biochar.
[0031] In the step (1), the ratio of red mud to deionized water is 20 g:100 ml.
[0032] The plant straw is corn straw or wheat straw.
[0033] The usage ratio of the plant straw powder to the red mud suspension is 10g:100ml.
[0034] In step (3), the heating rate of the nitrogen tubular furnace is 10°C / min to 350°C, and then 20°C / min to 750°C.
[0035] A method for preparing the novel composite cement grinding aid comprises the following steps: S1: The amine compounds are mixed in proportion, and then mixed with the red mud modified biochar, and stirred at a speed of 800 r / min for 15 min to obtain a uniformly dispersed mixture; S2: Evenly mix the remaining materials with the mixture obtained in S1 to obtain a new composite cement grinding aid.
[0036] Example 3 A novel composite cement grinding aid is prepared from the following raw materials in parts by weight: 35 parts of alcoholamine compounds, 12 parts of sodium sulfite, 25 parts of red mud modified biochar, 8 parts of dilauryl thiodipropionate, 8 parts of sodium humate, 7 parts of molasses, and 35 parts of water.
[0037] The alcoholamine compound is composed of monoethanol diisopropanolamine and diisopropyl monoethanolamine in a mass ratio of 2:1.
[0038] The red mud modified biochar is prepared by the following method: (1) Add red mud into deionized water and stir for 30 minutes to obtain a red mud suspension; (2) Clean the plant straw and grind it into fine powder, add the plant straw powder into the red mud suspension and continue stirring for 1 hour, then filter, and dry the solid mixture in an oven to obtain a pretreated mixture; (3) The pretreated mixture was placed in a nitrogen tubular furnace and heated to 750 °C at a set heating rate. The mixture was kept warm for 2 h under nitrogen protection and then naturally cooled to room temperature and ground into fine powder. The powder was then sieved through a 40-mesh sieve to obtain red mud modified biochar.
[0039] In the step (1), the ratio of red mud to deionized water is 20 g:100 ml.
[0040] The plant straw is corn straw or wheat straw.
[0041] The usage ratio of the plant straw powder to the red mud suspension is 10g:100ml.
[0042] In step (3), the heating rate of the nitrogen tubular furnace is 10°C / min to 350°C, and then 20°C / min to 750°C.
[0043] A method for preparing the novel composite cement grinding aid comprises the following steps: S1: The amine compounds are mixed in proportion, and then mixed with the red mud modified biochar, and stirred at a speed of 800 r / min for 15 min to obtain a uniformly dispersed mixture; S2: Evenly mix the remaining materials with the mixture obtained in S1 to obtain a new composite cement grinding aid.
[0044] Comparative Example 1 A new type of composite cement grinding aid is made from the following raw materials in parts by weight: A new type of composite cement grinding aid is made from the following raw materials in parts by weight: 35 parts of alcoholamine compounds, 12 parts of sodium sulfite, 25 parts of red mud, 8 parts of dilauryl thiodipropionate, 8 parts of sodium humate, 7 parts of molasses, and 35 parts of water.
[0045] The alcoholamine compound is composed of monoethanol diisopropanolamine and diisopropyl monoethanolamine in a mass ratio of 2:1.
[0046] A method for preparing the novel composite cement grinding aid comprises the following steps: S1: The amine compounds are mixed in proportion, and then mixed with red mud, and stirred at a speed of 800 r / min for 15 minutes to obtain a uniformly dispersed mixture; S2: Evenly mix the remaining materials with the mixture obtained in S1 to obtain a new composite cement grinding aid.
[0047] The comparative example 1 is basically the same as the example 3, except that the red mud used is unmodified red mud.
[0048] Comparative Example 2 A novel composite cement grinding aid is prepared from the following raw materials in parts by weight: 35 parts of alcoholamine compounds, 12 parts of sodium sulfite, 25 parts of biochar, 8 parts of dilauryl thiodipropionate, 8 parts of sodium humate, 7 parts of molasses, and 35 parts of water.
[0049] The alcoholamine compound is composed of monoethanol diisopropanolamine and diisopropyl monoethanolamine in a mass ratio of 2:1.
[0050] The biochar is prepared by the following method: the plant straw is cleaned and ground into fine powder, and then the plant straw powder is placed in a nitrogen tubular furnace and the heating rate is set to 750° C., and the temperature is kept warm for 2 hours under nitrogen protection, and then naturally cooled to room temperature and ground into fine powder, and the biochar is obtained by passing through a 40-mesh sieve.
[0051] The plant straw is corn straw or wheat straw; the heating rate of the nitrogen tubular furnace is 10°C / min to 350°C, and then 20°C / min to 750°C.
[0052] A method for preparing the novel composite cement grinding aid comprises the following steps: S1: The amine compounds are mixed in proportion, and then mixed with biochar, and stirred at a speed of 800 r / min for 15 min to obtain a uniformly dispersed mixture; S2: Evenly mix the remaining materials with the mixture obtained in S1 to obtain a new composite cement grinding aid.
[0053] The above comparative example is basically the same as Example 3, except that the biochar used is unmodified biochar.
[0054] Comparative Example 3 A novel composite cement grinding aid is prepared from the following raw materials in parts by weight: 35 parts of alcoholamine compounds, 12 parts of sodium sulfite, 25 parts of red mud modified biochar, 8 parts of dilauryl thiodipropionate, 8 parts of sodium humate, 7 parts of molasses, and 35 parts of water.
[0055] The alcoholamine compound is triethanolamine.
[0056] The red mud modified biochar is prepared by the following method: (1) Add red mud into deionized water and stir for 30 minutes to obtain a red mud suspension; (2) Clean the plant straw and grind it into fine powder, add the plant straw powder into the red mud suspension and continue stirring for 1 hour, then filter, and dry the solid mixture in an oven to obtain a pretreated mixture; (3) The pretreated mixture was placed in a nitrogen tubular furnace and heated to 750 °C at a set heating rate. The mixture was kept warm for 2 h under nitrogen protection and then naturally cooled to room temperature and ground into fine powder. The powder was then sieved through a 40-mesh sieve to obtain red mud modified biochar.
[0057] In the step (1), the ratio of red mud to deionized water is 20 g:100 ml.
[0058] The plant straw is corn straw or wheat straw.
[0059] The usage ratio of the plant straw powder to the red mud suspension is 10g:100ml.
[0060] In step (3), the heating rate of the nitrogen tubular furnace is 10°C / min to 350°C, and then 20°C / min to 750°C.
[0061] A method for preparing the novel composite cement grinding aid comprises the following steps: S1: The amine compounds are mixed in proportion, and then mixed with the red mud modified biochar, and stirred at a speed of 800 r / min for 15 min to obtain a uniformly dispersed mixture; S2: Evenly mix the remaining materials with the mixture obtained in S1 to obtain a new composite cement grinding aid.
[0062] The comparative example is substantially the same as Example 3, except that the alcoholamine compound used is triethanolamine.
[0063] Comparative Example 4 A novel composite cement grinding aid is prepared from the following raw materials in parts by weight: 35 parts of alcoholamine compounds, 12 parts of sodium sulfite, 25 parts of red mud modified biochar, 8 parts of dilauryl thiodipropionate, 8 parts of sodium humate, 7 parts of molasses, and 35 parts of water.
[0064] The alcoholamine compound is triisopropanolamine.
[0065] The red mud modified biochar is prepared by the following method: (1) Add red mud into deionized water and stir for 30 minutes to obtain a red mud suspension; (2) Clean the plant straw and grind it into fine powder, add the plant straw powder into the red mud suspension and continue stirring for 1 hour, then filter, and dry the solid mixture in an oven to obtain a pretreated mixture; (3) The pretreated mixture was placed in a nitrogen tubular furnace and heated to 750 °C at a set heating rate. The mixture was kept warm for 2 h under nitrogen protection and then naturally cooled to room temperature and ground into fine powder. The powder was then sieved through a 40-mesh sieve to obtain red mud modified biochar.
[0066] In the step (1), the ratio of red mud to deionized water is 20 g:100 ml.
[0067] The plant straw is corn straw or wheat straw.
[0068] The usage ratio of the plant straw powder to the red mud suspension is 10g:100ml.
[0069] In step (3), the heating rate of the nitrogen tubular furnace is 10°C / min to 350°C, and then 20°C / min to 750°C.
[0070] A method for preparing the novel composite cement grinding aid comprises the following steps: S1: The amine compounds are mixed in proportion, and then mixed with the red mud modified biochar, and stirred at a speed of 800 r / min for 15 min to obtain a uniformly dispersed mixture; S2: Evenly mix the remaining materials with the mixture obtained in S1 to obtain a new composite cement grinding aid.
[0071] The comparative example is substantially the same as Example 3, except that the alcoholamine compound used is triisopropanolamine.
[0072] Comparative Example 5 A novel composite cement grinding aid, whose raw material composition and preparation method are basically the same as those in Example 3, except that the alcoholamine compound is composed of monoethanol diisopropanolamine and diisopropyl monoethanolamine in a mass ratio of 1:2.
[0073] Comparative Example 6 A novel composite cement grinding aid, whose raw material composition and preparation method are basically the same as those in Example 3, except that the alcoholamine compound is composed of monoethanol diisopropanolamine and diisopropyl monoethanolamine in a mass ratio of 1:1.
[0074] Comparative Example 7 A novel composite cement grinding aid, whose raw material composition and preparation method are basically the same as those in Example 3, except that the alcoholamine compound is composed of monoethanol diisopropanolamine and diisopropyl monoethanolamine in a mass ratio of 3:1.
[0075] Comparative Example 8 A novel composite cement grinding aid, whose raw material composition and preparation method are basically the same as those in Example 3, except that the alcoholamine compound is monoethanol diisopropanolamine.
[0076] Comparative Example 9 A novel composite cement grinding aid, whose raw material composition and preparation method are basically the same as those in Example 3, except that the alcoholamine compound is diisopropyl monoethanolamine.
[0077] Performance Testing To further illustrate the effect of the grinding aid of the present invention, the above-mentioned Examples 1-3 and Comparative Examples 1-7 were respectively mixed into cement raw materials, with a dosage of 0.05 wt%, and a blank comparative example was set, i.e., no grinding aid was added; and the various properties thereof were statistically analyzed and compared. Cement raw material ratio: 68 wt% clinker, 5 wt% gypsum, 27 wt% slag. Cement was obtained by grinding in a Φ5370 mm vertical mill for 30 min. The sieve residue, setting time, strength and other data were tested. The sieve residue of cement was tested according to GB / T 1345-2005 "Cement fineness detection method sieve analysis method"; the standard consistency water requirement, stability and setting time of cement were determined according to GB / T 1346-2001 "cement standard consistency water requirement, stability and setting time". The strength of cement mortar was determined according to GB / T17671-1999 "cement mortar strength test method (ISO method)". The test results are shown in Table 1 below.
[0078] Table 1 Performance test results It can be seen from the data in Table 1 that the composite cement grinding aids prepared in Examples 1-3 of the present invention have different improvements in 3-day / 28-day flexural and compressive strengths compared with the blank examples in the same grinding time, among which the 45 μm sieve residue is significantly reduced, the average hourly output is 202.7 t / h, the average 28-day compressive strength is 59.4 MPa, and the average 28-day flexural strength is 8.2 MPa. From the data of comparative examples 1-2, it can be seen that compared with the blank example, the comparative example 1 using red mud alone has an increase of 10 t / h in output per unit and an increase of 2.1 MPa in compressive strength after 28 days; the comparative example 2 using biochar alone has an increase of 13 t / h in output per unit and an increase of 1.7 MPa in compressive strength after 28 days; and the average values of Examples 1-3 of the present invention are compared with the blank, with an increase of 37.7 t / h in output per unit and an increase of 9.2 MPa in compressive strength after 28 days, which are significantly greater than those of comparative example 1, comparative example 2 or the combination of the two. This shows that the biochar modified by red mud in the present invention forms a stable chemical bond with red mud, and the red mud is stably adsorbed on the surface of biochar (such as Figure 1As shown), the two substances work synergistically to improve the porosity and specific surface area of the modified biochar, enhance the reaction activity and adsorption capacity of the biochar, and can be adsorbed on the surface of cement particles, enhance the adsorption capacity of the material, prevent the spread of cracks, and improve the grindability of the material. At the same time, since red mud contains aluminum oxide and cement mineral component dicalcium silicate, dicalcium silicate has a seeding effect in the cement production process, which can improve the burnability of the raw material and reduce the burning temperature of the clinker. In addition, it can be seen from the data comparison of Comparative Examples 5-9 that the alcoholamine compounds used in the present invention can work together with red mud modified biochar to form complexes with iron and aluminum oxides, which can promote the hydration of C4AF to generate AFt, change the amount of Ca(OH)2 in the cement stone hydration process, and then accelerate the hydration of silicate minerals, stimulate the activity of cement materials, and thus increase the strength of cement; changing the composition or dosage ratio of the alcoholamine compounds cannot achieve the best use effect.
[0079] It should be noted that the above embodiments are only partial embodiments of the preferred methods of implementing the present invention, rather than all embodiments. Obviously, based on the above embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
Claims
1. A novel composite cement grinding aid, characterized in that: The invention is prepared from the following raw materials in parts by weight: 30-40 parts of alcoholamine compounds, 10-15 parts of sodium sulfite, 20-30 parts of red mud modified biochar, 5-10 parts of dilauryl thiodipropionate, 5-10 parts of sodium humate, 5-10 parts of molasses and 30-40 parts of water.
2. The novel composite cement grinding aid according to claim 1, characterized in that: The alcoholamine compound is composed of monoethanol diisopropanolamine and diisopropyl monoethanolamine in a mass ratio of 2:
1.
3. The novel composite cement grinding aid according to claim 1, characterized in that: The red mud modified biochar is prepared by the following method: (1) Add red mud into deionized water and stir for 30 minutes to obtain a red mud suspension; (2) Clean the plant straw and grind it into fine powder, add the plant straw powder into the red mud suspension and continue stirring for 1 hour, then filter, and dry the solid mixture in an oven to obtain a pretreated mixture; (3) The pretreated mixture was placed in a nitrogen tubular furnace and heated to 750 °C at a set heating rate. The mixture was kept warm for 2 h under nitrogen protection and then naturally cooled to room temperature and ground into fine powder. The powder was then sieved through a 40-mesh sieve to obtain red mud modified biochar.
4. The novel composite cement grinding aid according to claim 3, characterized in that: In the step (1), the ratio of red mud to deionized water is 20 g:100 ml.
5. The novel composite cement grinding aid according to claim 3, characterized in that: The plant straw is corn straw or wheat straw.
6. The novel composite cement grinding aid according to claim 3, characterized in that: The usage ratio of the plant straw powder to the red mud suspension is 10g:100ml.
7. The novel composite cement grinding aid according to claim 3, characterized in that: In step (3), the heating rate of the nitrogen tubular furnace is 10°C / min to 350°C, and then 20°C / min to 750°C.
8. A method for preparing the novel composite cement grinding aid according to any one of claims 1 to 7, characterized in that: The following steps are involved: S1: The amine compounds are mixed in proportion, and then mixed with the red mud modified biochar, and stirred at a speed of 800 r / min for 15 min to obtain a uniformly dispersed mixture; S2: Evenly mix the remaining materials with the mixture obtained in S1 to obtain a new composite cement grinding aid.
Citation Information
Patent Citations
Concrete grinding aid and preparation method thereof
CN101269928A
Method for preparation of cement grinding aid additive from glycerin rectification residue
CN105906228A
Composite modified biomass activated carbon for degrading formaldehyde and preparation method of activated carbon
CN109775706A
Preparation process and application of sludge biochar
CN114570329A
Method of manufacturing cement
JP2012197204A
Cited By
Agricultural and forestry waste-red mud composite self-sensing building material and preparation method thereof
CN119638332A
High-strength household environment-friendly ceramic and preparation method thereof
CN121974660A
Milling method for dry milling of a piece of milled material and method for producing a cement
EP4745106A1