Easily-processed aluminum alloy plate for printing
By adjusting the raw material composition and cold rolling process of aluminum alloy plates, the problem of cracks and holes easily appearing in aluminum alloy plates for printing during the cold rolling and thinning process has been solved, the mechanical properties and processing performance of the materials have been improved, and the base of aluminum alloy plates for printing has been ensured. The strength and surface quality meet the needs of aluminum plate printing process.
Patent Information
- Application Number
- CN202410769706.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-14
- Publication Date
- 2024-10-11
AI Technical Summary
Existing aluminum alloy sheets for printing are prone to cracks, holes and fracture defects during the cold rolling and thinning process, resulting in increased processing difficulty and poor material performance, which cannot meet the needs of the aluminum plate printing process.
By adjusting the raw material composition of the aluminum alloy plate, reducing the content of Mg, Cu, Mn, and Zn, increasing the content of Si, and adding additional elements such as Cr, Ni, B, Be, Bi, Cd, Ga, Sb, and V to improve the material With excellent crack resistance and molten fluidity, the aluminum plate base for printing is prepared using a cold rolling process to ensure material uniformity and small surface roughness.
It makes the aluminum alloy plate less prone to cracks and holes during the cold rolling and thinning process, improves the mechanical properties and processing performance of the material, ensures the strength and surface quality of the aluminum plate base for printing, and meets the needs of various aluminum plate printing processes.
Smart Images

Figure CN118756003A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of aluminum alloy plates, and in particular relates to an easily processable aluminum alloy plate for printing. Background Art
[0002] Common aluminum plate printing processes mainly include: thermal transfer, watermark transfer, UV printing, and metal embossing, etc. The aluminum alloy sheet required for aluminum plate printing is called printing aluminum plate base.
[0003] Generally, the thickness of the aluminum plate base for printing is 0.1-0.5mm, and its production method is mainly cold rolling, that is, it is made by cold rolling a thicker cast-rolled plate to make it thinner. The above-mentioned easy-to-process aluminum alloy plate refers to the cast-rolled plate.
[0004] On the other hand, the cast rolled sheet for printing not only needs to have sufficient and suitable mechanical properties, but also has other relatively special performance requirements as printing materials, such as: small surface roughness, sufficient processing performance, and outstanding crack resistance. Otherwise, when the cast rolled sheet of about 10mm is cold-rolled and thinned to 0.1-0.5mm aluminum sheet base for printing, a large number of cracks and / or holes are likely to appear during the process, making the aluminum alloy sheet completely unusable for printing operations.
[0005] For example, the Chinese invention patent application with application publication number CN117684055A and application publication date 2024.03.12 discloses an aluminum alloy plate and strip for a treatment-free printing plate and a preparation method thereof. In terms of mass percentage, the aluminum alloy plate and strip includes: Si content of 0.02% to 0.10%, Fe content of 0.10% to 0.35%, Cu content of <0.05%, Mn content of <0.02%, Mg content of 0.17% to 0.35%, Zn content of <0.02%, Ti content of <0.03%, and the balance is Al and several unavoidable impurities, the total content of impurities is <0.15%, and the content of a single impurity is <0.05%.
[0006] The aluminum alloy sheet and strip material in the invention patent application has high resistance to softening deformation, high resolution and printing resistance, thus solving the problem of the difficulty in matching the tensile strength and grit properties of the aluminum alloy sheet and strip material used for the unprocessed printing plate.
[0007] However, in the actual production and use of the aluminum alloy sheet and strip, there are at least the following deficiencies, which are also the technical problems to be solved by the present invention, namely: In the raw material ratio, in order to ensure sufficient high resistance to softening and deformation, a higher Cu element ratio and Mg element ratio are set. However, if the Cu content is too high, the tendency of thermal cracking will increase, and if the Mg content is too high, it will increase the difficulty of processing and easily cause defects such as cracks and fractures.
[0008] So to sum up, there is an urgent need for a cast-rolled plate with all mechanical properties meeting the standards and good material uniformity, so as to ensure that the aluminum plate base for printing obtained after cold rolling and thinning is not prone to defects such as cracks, holes and fractures, so that the latter can be effectively used in various aluminum plate printing processes. Summary of the invention
[0009] The invention provides an easy-to-process aluminum alloy plate for printing. The raw material composition of the aluminum alloy plate comprises the following components by weight: Si 0.0452-0.0460%, Mg 0.0006-0.0009%, Cu≤0.0002%, Mn 0.0028-0.0035%, Fe0.320-0.335%, Ti 0.0242-0.0254%, Zn 0.0014-0.0020%, Cr≤0.0005%, Ni 0.005-0.006%, B0.001-0.002%, Be≤0.0001%, Bi≤0.001%, Cd≤0.001%, Ga≤0.015%, Sb 0.005-0.006%, V0.025-0.028%, the total amount of impurity elements is ≤0.20%, and the balance is ≥99% of Al.
[0010] The easy-to-process aluminum alloy plate has the following advantages: first, the material has good uniformity and is not prone to defects such as cracks, breaks, and holes; second, the mechanical properties are sufficient, and the printing aluminum plate base obtained by cold rolling and thinning has sufficient strength and low surface roughness, which can meet the needs of various aluminum plate printing processes.
[0011] The technical solution adopted by the present invention to solve the above problems is: an easy-to-process aluminum alloy plate for printing, the raw material composition includes the following components by weight: Si 0.0452-0.0460%, Mg 0.0006-0.0009%, Cu≤0.0002%, Mn 0.0028-0.0035%, Fe 0.320-0.335%, Ti 0.0242-0.0254%, Zn 0.0014-0.0020%, Cr≤0.0005%, Ni 0.005-0.006%, B0.001-0.002%, Be≤0.0001%, Bi≤0.001%, Cd≤0.001%, Ga≤0.015%, Sb 0.005-0.006%, V 0.025-0.028%, the total amount of impurity elements ≤ 0.20%, the balance is Al.
[0012] It is common sense that excessive Mg and Cu elements will increase the cracking risk of aluminum alloys. Therefore, in the present invention, the easy-to-process aluminum alloy sheet has a relatively increased Si content and reduced Mg, Cu, Mn, and Zn contents compared to ordinary 1XXX series aluminum alloys, so that the crack resistance of the easy-to-process aluminum alloy sheet is significantly improved, and the material strength and hardness are appropriately improved.
[0013] However, the relatively low content of Mg, Cu, Mn, and Zn has very limited or even insufficient effect on improving the strength, hardness, and wear resistance of the material. Therefore, the easy-to-process aluminum alloy sheet is supplemented with relatively many types of other elements with extremely low content, namely: Cr, Ni, B, Be, Bi, Cd, Ga, Sb, and V.
[0014] In addition, it is precisely because of the relatively large amount of Si added that the molten fluidity of the plate is improved, which is reflected in the easy-to-process aluminum alloy plate, that is, the internal composition of the material is relatively uniform, and ultimately ensures that when the easy-to-process aluminum alloy plate is cold-rolled and thinned to prepare an aluminum plate base for printing, the processing performance is outstanding, and the thinning action is uniform, and cracks and holes are not easy to appear.
[0015] Finally, by defining the preparation method of the easy-to-process aluminum alloy sheet itself and the cold rolling process from the easy-to-process aluminum alloy sheet to the printing aluminum plate base, the printing aluminum plate base has a smaller surface roughness.
[0016] Otherwise, if the above surface roughness is too high, the plate will not be in smooth contact during the printing process and the quality of the printed product will be impaired.
[0017] A further preferred technical solution is that the easily machined aluminum alloy plate is a cast-rolled plate with a thickness of 6.0-10.0 mm.
[0018] A further preferred technical solution is that the easy-to-process aluminum alloy sheet is used to prepare an aluminum plate base for printing by a cold rolling method, and the thickness of the aluminum plate base for printing is 0.1-0.4 mm.
[0019] In the present invention, the specific operating parameters of the above cold rolling method are as follows: The rolling speed is 250-850m / min, the rolling times are ≥4 times, and the roughness of the roller is ≤0.25um.
[0020] A further preferred technical solution is a method for preparing the easily machinable aluminum alloy sheet, which comprises the following steps in sequence: S1, material melting: first adding and melting aluminum ingots in a melting furnace, and then adding and melting master alloys to obtain a melt; S2, first refining: firstly adding a refining agent to the molten metal, and performing a first slag removal operation, then adding a mixed gas, and performing a second slag removal operation, and then successively performing heat preservation and pouring operations to obtain a rough casting; S3, second refining: first add and melt the rough casting in a melting furnace, then add mixed gas, perform a third slag removal operation, and then perform heat preservation and pouring operations in sequence to obtain a precision casting; S4, homogenization treatment: firstly add the precision casting billet into the homogenization treatment furnace, and then perform heating, heat preservation, and cooling operations in sequence to obtain a qualified casting billet; S5, extrusion molding: on an extruder, the qualified ingot is sequentially extruded, quenched, and stretched to obtain a preliminary plate; S6. Aging treatment: heating, heat preservation, and cooling the preliminary plate in sequence to obtain the final easy-to-process aluminum alloy plate.
[0021] A further preferred technical solution is that in S1, the master alloy is an aluminum alloy, including Al-Cd alloy, Al-Cr alloy, and Al-Ni alloy, the melting temperature of the aluminum ingot is 700-720°C, and the melting temperature of the master alloy is 730-740°C.
[0022] In the present invention, the above-mentioned components such as Cd and Cr are added in the form of aluminum alloy. Compared with the method of directly adding the components such as Cd and Cr themselves, this method has at least the following advantages: First, it can obtain aluminum alloy materials with more uniform chemical composition distribution, so that more components such as Cd and Cr can be incorporated, fundamentally improving the performance of aluminum alloy materials; Second, the addition of the master alloy can reduce the burning loss of components such as Cd and Cr, thereby obtaining a more stable alloy composition; Third, some impurity gases can be removed from the intermediate alloy at the beginning of its preparation. Even if industrial-grade purity single substances such as Cd, Cr and other components are added, the impurity gases carried inside are generally redundant with the intermediate alloy.
[0023] A further preferred technical solution is that in S2, the refining agent is added by blowing nitrogen, and the mixed gas includes nitrogen and chlorine.
[0024] A further preferred technical solution is that in S3, the melting temperature of the rough casting is 720-750°C, and the mixed gas includes nitrogen and carbon monoxide gas.
[0025] A further preferred technical solution is that in S4, the heating temperature is 400-450°C, the insulation temperature is 320-350°C, the cooling method is air cooling, and the cooling time is 1.5-2.0h, until it cools to room temperature.
[0026] A further preferred technical solution is that in S5, the temperature of the extrusion operation is 450-480°C, the quenching method is water mist, and the stretching amount of the stretching operation is 2.0-2.5%.
[0027] A further preferred technical solution is that in S6, the temperature of the heating operation is 95-125°C, the temperature of the insulation is 65-80°C, the cooling method is air blowing cooling, and the cooling time is ≥5h, until it is cooled to room temperature.
[0028] In the present invention, from the initial raw material composition ratio, to the preparation of the cast rolled plate, to the cold rolling preparation of the aluminum plate base for printing, the above whole process is ensured by the following methods to ensure that the final aluminum plate base for printing has sufficient mechanical properties, outstanding processing properties, and small surface roughness. At the same time, the following are also the beneficial effects of the present application compared with the prior art: First, reduce the content of Mg, Cu, Mn and Zn, so that the aluminum plate base for printing has initial and sufficient crack resistance, uniform material internal component distribution, and ultimately outstanding processing performance; Second, the above properties are supplemented by adding relatively many kinds of other elements with extremely low contents, namely: Cr, Ni, B, Be, Bi, Cd, Ga, Sb, and V. At the same time, the other elements will not have a significant impact on the comprehensive properties of the aluminum plate base for printing; Third, due to the relatively large amount of Si added, the molten fluidity of the cast-rolled plate is improved, which is reflected in the cast-rolled plate, that is, the internal composition of the material is relatively uniform, which ultimately ensures that when the cast-rolled plate is cold-rolled and thinned to prepare the aluminum plate base for printing, the processing performance is outstanding, and the thinning action is uniform, and cracks and holes are not easy to appear; Fourth, through the limitation of the cast-rolled plate preparation method and the limitation of the above-mentioned cold rolling process, the aluminum plate base for printing has a smaller surface roughness, so that smooth contact can be achieved during the printing process, thereby ensuring the quality of the printed product. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 The cast-rolled plate in Example 1 of the present invention is the average value of the results of testing each component after taking three test points at two positions A and B with a distance greater than 0.5m.
[0030] Figure 2 The microstructure of the cast-rolled plate along the length direction in Example 1 of the present invention.
[0031] Figure 3 The microstructure of the cast-rolled plate along the cross-sectional direction in Example 1 of the present invention.
[0032] Figure 4 The following are the average results of the performance tests of the aluminum plate-based products for printing in the four embodiments and four comparative examples of the present invention. DETAILED DESCRIPTION
[0033] The following descriptions are merely preferred embodiments of the present invention and are not intended to limit the scope of the present invention.
[0034] Example 1 As attached Figure 1-4 As shown, an easy-to-process aluminum alloy plate for printing, whose raw material composition includes the following components by weight: Si 0.0455%, Mg 0.0009%, Cu≤0.0002%, Mn 0.0031%, Fe 0.334%, Ti 0.0249%, Zn0.0018%, Cr≤0.0005%, Ni 0.005%, B 0.001%, Be≤0.0001%, Bi≤0.001%, Cd≤0.001%, Ga≤0.015%, Sb 0.005%, V0.025%, the total amount of impurity elements ≤0.20%, and the balance is Al.
[0035] In this embodiment, the above Si, Mg, Cu, Mn, Fe, Ti, and Zn elements do not need to be added additionally, and are included in the aluminum ingot when Al is supplemented. In other words, the aluminum ingot used for the easy-to-process aluminum alloy sheet needs to be tested for elements and selected for products to ensure that the final raw material composition ratio meets the above requirements.
[0036] The easily machined aluminum alloy plate is a cast-rolled plate with a thickness of 6.7 mm.
[0037] The easy-to-process aluminum alloy sheet is used to prepare an aluminum plate base for printing by a cold rolling method, and the thickness of the aluminum plate base for printing is 0.2 mm.
[0038] The method for preparing the cast-rolled plate comprises the following steps in sequence: S1, material melting: first adding and melting aluminum ingots in a melting furnace, and then adding and melting master alloys to obtain a melt; S2, first refining: firstly adding a refining agent to the molten metal, and performing a first slag removal operation, then adding a mixed gas, and performing a second slag removal operation, and then successively performing heat preservation and pouring operations to obtain a rough casting; S3, second refining: first add and melt the rough casting in a melting furnace, then add mixed gas, perform a third slag removal operation, and then perform heat preservation and pouring operations in sequence to obtain a precision casting; S4, homogenization treatment: firstly add the precision casting billet into the homogenization treatment furnace, and then perform heating, heat preservation, and cooling operations in sequence to obtain a qualified casting billet; S5, extrusion molding: on an extruder, the qualified ingot is sequentially extruded, quenched, and stretched to obtain a preliminary plate; S6. Aging treatment: heating, heat preservation, and cooling the preliminary plate in sequence to obtain the final easy-to-process aluminum alloy plate.
[0039] In S1, the intermediate alloy is an aluminum alloy, specifically: Al-Cr alloy, Al-Ni alloy, Al-B-Bi alloy, Al-Be alloy, Al-Cd alloy, and Al-Ga-Sb-V alloy. The melting temperature of the aluminum ingot is 720°C, and the melting temperature of the intermediate alloy is 740°C.
[0040] In S2, the refining agent is added by blowing nitrogen, the mixed gas includes nitrogen and chlorine, and the refining agent is a commercially available product.
[0041] In S3, the melting temperature of the raw ingot is 750°C, and the mixed gas includes nitrogen and carbon monoxide gas.
[0042] In S4, the heating temperature is 450°C, the insulation temperature is 320°C, the cooling method is air cooling, and the cooling time is 2.0h, until it cools to room temperature.
[0043] In S5, the temperature of the extrusion operation is 460°C, the quenching method is water mist, and the stretching amount of the stretching operation is 2.0%.
[0044] In S6, the temperature of the heating operation is 125°C, the temperature of the insulation is 70°C, the cooling method is air blowing cooling, and the cooling time is ≥ 6 hours until it cools to room temperature. The air temperature of the air blowing cooling method is adjusted according to the real-time temperature of the preliminary plate to ensure a sufficiently slow cooling speed.
[0045] In addition, the cold rolling method from cast rolled plate to aluminum plate base for printing has the following specific working parameters: The rolling speed is 300m / min, the rolling times are 4 times, and the roughness of the roller is ≤0.25um.
[0046] Finally, take 20 aluminum plates for printing in this embodiment and Figure 4 The items in the test were tested for performance and the average values were recorded. The results are shown in the attached Figure 4 The table in .
[0047] Example 2 As attached Figure 4As shown, an easy-to-process aluminum alloy plate for printing, the raw material composition of which includes the following components by weight: Si 0.0458%, Mg 0.0008%, Cu≤0.0002%, Mn 0.0031%, Fe 0.333%, Ti 0.0251%, Zn0.0019%, Cr≤0.0005%, Ni 0.005%, B 0.001%, Be≤0.0001%, Bi≤0.001%, Cd≤0.001%, Ga≤0.015%, Sb 0.005%, V 0.028%, the total amount of impurity elements ≤0.20%, and the balance is Al.
[0048] In this embodiment, the above Si, Mg, Cu, Mn, Fe, Ti, and Zn elements do not need to be added additionally, and are included in the aluminum ingot when Al is supplemented. In other words, the aluminum ingot used for the easy-to-process aluminum alloy sheet needs to be tested for elements and selected for products to ensure that the final raw material composition ratio meets the above requirements.
[0049] The easily machined aluminum alloy plate is a cast-rolled plate with a thickness of 7.2 mm.
[0050] The easy-to-process aluminum alloy sheet is used to prepare an aluminum plate base for printing by a cold rolling method, and the thickness of the aluminum plate base for printing is 0.25 mm.
[0051] The method for preparing the cast-rolled plate comprises the following steps in sequence: S1, material melting: first adding and melting aluminum ingots in a melting furnace, and then adding and melting master alloys to obtain a melt; S2, first refining: firstly adding a refining agent to the molten metal, and performing a first slag removal operation, then adding a mixed gas, and performing a second slag removal operation, and then successively performing heat preservation and pouring operations to obtain a rough casting; S3, second refining: first add and melt the rough casting in a melting furnace, then add mixed gas, perform a third slag removal operation, and then perform heat preservation and pouring operations in sequence to obtain a precision casting; S4, homogenization treatment: firstly add the precision casting billet into the homogenization treatment furnace, and then perform heating, heat preservation, and cooling operations in sequence to obtain a qualified casting billet; S5, extrusion molding: on an extruder, the qualified ingot is sequentially extruded, quenched, and stretched to obtain a preliminary plate; S6. Aging treatment: heating, heat preservation, and cooling the preliminary plate in sequence to obtain the final easy-to-process aluminum alloy plate.
[0052] In S1, the intermediate alloy is an aluminum alloy, specifically: Al-Cr alloy, Al-Ni alloy, Al-B-Bi alloy, Al-Be alloy, Al-Cd alloy, and Al-Ga-Sb-V alloy. The melting temperature of the aluminum ingot is 720°C, and the melting temperature of the intermediate alloy is 730°C.
[0053] In S2, the refining agent is added by blowing nitrogen, the mixed gas includes nitrogen and chlorine, and the refining agent is a commercially available product.
[0054] In S3, the melting temperature of the raw ingot is 740°C, and the mixed gas includes nitrogen and carbon monoxide gas.
[0055] In S4, the heating temperature is 420°C, the insulation temperature is 340°C, the cooling method is air cooling, and the cooling time is 2.0h, until it cools to room temperature.
[0056] In S5, the temperature of the extrusion operation is 470°C, the quenching method is water mist, and the stretching amount of the stretching operation is 2.1%.
[0057] In S6, the temperature of the heating operation is 125°C, the temperature of the insulation is 65°C, the cooling method is air cooling, and the cooling time is ≥ 6 hours until it cools to room temperature. The air temperature of the air cooling method is adjusted according to the real-time temperature of the preliminary plate to ensure a sufficiently slow cooling speed.
[0058] In addition, the cold rolling method from cast rolled plate to aluminum plate base for printing has the following specific working parameters: The rolling speed is 350m / min, the rolling times are 5 times, and the roughness of the roller is ≤0.25um.
[0059] Finally, take 20 aluminum plates for printing in this embodiment and Figure 4 The items in the test were tested for performance and the average values were recorded. The results are shown in the attached Figure 4 The table in .
[0060] Example 3 As attached Figure 4 As shown, an easy-to-process aluminum alloy plate for printing, the raw material composition of which includes the following components by weight: Si 0.0460%, Mg 0.0008%, Cu≤0.0002%, Mn 0.0031%, Fe0.329%, Ti 0.0253%, Zn0.0019%, Cr≤0.0005%, Ni 0.005%, B 0.001%, Be≤0.0001%, Bi≤0.001%, Cd≤0.001%, Ga≤0.015%, Sb 0.005%, V0.027%, the total amount of impurity elements ≤0.20%, and the balance is Al.
[0061] In this embodiment, the above Si, Mg, Cu, Mn, Fe, Ti, and Zn elements do not need to be added additionally, and are included in the aluminum ingot when Al is supplemented. In other words, the aluminum ingot used for the easy-to-process aluminum alloy sheet needs to be tested for elements and selected for products to ensure that the final raw material composition ratio meets the above requirements.
[0062] The easily machined aluminum alloy plate is a cast-rolled plate with a thickness of 8.4 mm.
[0063] The easy-to-process aluminum alloy sheet is used to prepare an aluminum plate base for printing by a cold rolling method, and the thickness of the aluminum plate base for printing is 0.32 mm.
[0064] The method for preparing the cast-rolled plate comprises the following steps in sequence: S1, material melting: first adding and melting aluminum ingots in a melting furnace, and then adding and melting master alloys to obtain a melt; S2, first refining: firstly adding a refining agent to the molten metal, and performing a first slag removal operation, then adding a mixed gas, and performing a second slag removal operation, and then successively performing heat preservation and pouring operations to obtain a rough casting; S3, second refining: first add and melt the rough casting in a melting furnace, then add mixed gas, perform a third slag removal operation, and then perform heat preservation and pouring operations in sequence to obtain a precision casting; S4, homogenization treatment: firstly add the precision casting billet into the homogenization treatment furnace, and then perform heating, heat preservation, and cooling operations in sequence to obtain a qualified casting billet; S5, extrusion molding: on an extruder, the qualified ingot is sequentially extruded, quenched, and stretched to obtain a preliminary plate; S6. Aging treatment: heating, heat preservation, and cooling the preliminary plate in sequence to obtain the final easy-to-process aluminum alloy plate.
[0065] In S1, the intermediate alloy is an aluminum alloy, specifically: Al-Cr alloy, Al-Ni alloy, Al-B-Bi alloy, Al-Be alloy, Al-Cd alloy, and Al-Ga-Sb-V alloy. The melting temperature of the aluminum ingot is 700°C, and the melting temperature of the intermediate alloy is 730°C.
[0066] In S2, the refining agent is added by blowing nitrogen, the mixed gas includes nitrogen and chlorine, and the refining agent is a commercially available product.
[0067] In S3, the melting temperature of the raw ingot is 725°C, and the mixed gas includes nitrogen and carbon monoxide gas.
[0068] In S4, the heating temperature is 465°C, the insulation temperature is 330°C, the cooling method is air cooling, and the cooling time is 2.0h, until it cools to room temperature.
[0069] In S5, the temperature of the extrusion operation is 475°C, the quenching method is water mist, and the stretching amount of the stretching operation is 2.2%.
[0070] In S6, the temperature of the heating operation is 120°C, the temperature of the insulation is 65°C, the cooling method is air cooling, and the cooling time is ≥ 6 hours until it cools to room temperature. The air temperature of the air cooling method is adjusted according to the real-time temperature of the preliminary plate to ensure a sufficiently slow cooling speed.
[0071] In addition, the cold rolling method from cast rolled plate to aluminum plate base for printing has the following specific working parameters: The rolling speed is 400m / min, the rolling times are 5 times, and the roughness of the roller is ≤0.25um.
[0072] Finally, take 20 aluminum plates for printing in this embodiment and Figure 4 The items in the test were tested for performance and the average values were recorded. The results are shown in the attached Figure 4 The table in .
[0073] Example 4 As attached Figure 4 As shown, an easy-to-process aluminum alloy plate for printing, the raw material composition of which includes the following components by weight: Si 0.0460%, Mg 0.0009%, Cu≤0.0002%, Mn 0.0031%, Fe0.332%, Ti 0.0250%, Zn0.0020%, Cr≤0.0005%, Ni 0.005%, B 0.001%, Be≤0.0001%, Bi≤0.001%, Cd≤0.001%, Ga≤0.015%, Sb 0.005%, V0.026%, the total amount of impurity elements ≤0.20%, and the balance is Al.
[0074] In this embodiment, the above Si, Mg, Cu, Mn, Fe, Ti, and Zn elements do not need to be added additionally, and are included in the aluminum ingot when Al is supplemented. In other words, the aluminum ingot used for the easy-to-process aluminum alloy sheet needs to be tested for elements and selected for products to ensure that the final raw material composition ratio meets the above requirements.
[0075] The easily machined aluminum alloy plate is a cast-rolled plate with a thickness of 8.4 mm.
[0076] The easy-to-process aluminum alloy sheet is used to prepare an aluminum plate base for printing by a cold rolling method, and the thickness of the aluminum plate base for printing is 0.12 mm.
[0077] The method for preparing the cast-rolled plate comprises the following steps in sequence: S1, material melting: first adding and melting aluminum ingots in a melting furnace, and then adding and melting master alloys to obtain a melt; S2, first refining: firstly adding a refining agent to the molten metal, and performing a first slag removal operation, then adding a mixed gas, and performing a second slag removal operation, and then successively performing heat preservation and pouring operations to obtain a rough casting; S3, second refining: first add and melt the rough casting in a melting furnace, then add mixed gas, perform a third slag removal operation, and then perform heat preservation and pouring operations in sequence to obtain a precision casting; S4, homogenization treatment: firstly add the precision casting billet into the homogenization treatment furnace, and then perform heating, heat preservation, and cooling operations in sequence to obtain a qualified casting billet; S5, extrusion molding: on an extruder, the qualified ingot is sequentially extruded, quenched, and stretched to obtain a preliminary plate; S6. Aging treatment: heating, heat preservation, and cooling the preliminary plate in sequence to obtain the final easy-to-process aluminum alloy plate.
[0078] In S1, the intermediate alloy is an aluminum alloy, specifically: Al-Cr alloy, Al-Ni alloy, Al-B-Bi alloy, Al-Be alloy, Al-Cd alloy, and Al-Ga-Sb-V alloy. The melting temperature of the aluminum ingot is 700°C, and the melting temperature of the intermediate alloy is 730°C.
[0079] In S2, the refining agent is added by blowing nitrogen, the mixed gas includes nitrogen and chlorine, and the refining agent is a commercially available product.
[0080] In S3, the melting temperature of the raw ingot is 750°C, and the mixed gas includes nitrogen and carbon monoxide gas.
[0081] In S4, the heating temperature is 465°C, the insulation temperature is 320°C, the cooling method is air cooling, and the cooling time is 2.0h, until it cools to room temperature.
[0082] In S5, the temperature of the extrusion operation is 480°C, the quenching method is water mist, and the stretching amount of the stretching operation is 2.2%.
[0083] In S6, the temperature of the heating operation is 120°C, the temperature of the insulation is 80°C, the cooling method is air cooling, and the cooling time is ≥6h, until it cools to room temperature. The air temperature of the air cooling method is adjusted according to the real-time temperature of the preliminary plate to ensure a sufficiently slow cooling speed.
[0084] In addition, the cold rolling method from cast rolled plate to aluminum plate base for printing has the following specific working parameters: The rolling speed is 400m / min, the rolling times are 4 times, and the roughness of the roller is ≤0.25um.
[0085] Finally, take 20 aluminum plates for printing in this embodiment and Figure 4 The items in the test were tested for performance and the average values were recorded. The results are shown in the attached Figure 4 The table in .
[0086] Comparative Example 1 The cast plate and the aluminum plate base for printing in this comparative example are different from those in Example 1 in the following only: The raw material composition of the cast and rolled plate includes the following components by weight: Si 0.02%, Mg 0.2%, Cu 0.05%, Mn 0.02%, Fe 0.1%, Ti 0.03%, Zn 0.02%, the total amount of impurity elements ≤ 0.20%, and the balance is Al.
[0087] That is, the raw material is directly the existing aluminum ingot with relatively high content of Mg, Cu, Mn and Zn. Accordingly, the subsequent intermediate alloy does not need to be used.
[0088] Finally, take 20 aluminum plates for printing in this embodiment and Figure 4 The items in the test were tested for performance and the average values were recorded. The results are shown in the attached Figure 4 The table in .
[0089] Comparative Example 2 The cast plate and the aluminum plate base for printing in this comparative example are different from those in Example 1 in the following only: The raw material composition of the cast rolled plate includes the following components by weight: Si 0.0455%, Mg 0.0009%, Cu≤0.0002%, Mn 0.0031%, Fe 0.334%, Ti 0.0249%, Zn 0.0018%, the total amount of impurity elements ≤0.20%, and the balance is Al.
[0090] That is, the raw material is directly the aluminum ingot used in Example 1. Accordingly, the subsequent intermediate alloy does not need to be used.
[0091] Finally, take 20 aluminum plates for printing in this embodiment and Figure 4 The items in the test were tested for performance and the average values were recorded. The results are shown in the attached Figure 4 The table in .
[0092] Comparative Example 3 The cast plate and the aluminum plate base for printing in this comparative example are different from those in Example 1 in only one respect, namely, The following steps are omitted: S4, homogenization treatment.
[0093] Finally, take 20 aluminum plates for printing in this embodiment and Figure 4 The items in the test were tested for performance and the average values were recorded. The results are shown in the attached Figure 4 The table in .
[0094] Comparative Example 4 The cast plate and the aluminum plate base for printing in this comparative example are different from those in Example 1 in only one respect, namely, The specific working parameters of the cold rolling method from cast plate to aluminum plate base for printing are as follows: rolling speed is 800m / min, rolling times are 2 times, and the roughness of the rolling roller is greater than 0.35um.
[0095] Finally, take 20 aluminum plates for printing in this embodiment and Figure 4 The items in the test were tested for performance and the average values were recorded. The results are shown in the attached Figure 4 The table in .
[0096] Results Analysis First, as attached Figure 1-4 As shown, it is shown that the cast-rolled plate in Example 1 has sufficient material uniformity and a dense microstructure, which is a necessary condition for producing an aluminum plate base for printing with outstanding mechanical properties and excellent processing properties.
[0097] Second, as attached Figure 4 As shown, the overall performance of the printing aluminum plate bases in the four comparative examples is not as good as that of the embodiment, which indicates that the above-mentioned raw material composition, homogenization treatment, and limitation of the cold rolling method are all necessary for the performance of the printing aluminum plate base.
[0098] Third, as attached Figure 4 As shown, the aluminum plate base for printing in Comparative Example 1 has the largest elongation after breaking, which will lead to instability in the aluminum plate printing process and greatly affect the quality of the printed product.
[0099] The embodiments of the present invention are described in detail above in conjunction with the accompanying drawings, but the present invention is not limited to the above embodiments. Various modifications can be made within the knowledge of ordinary technicians in the technical field without departing from the purpose of the present invention. These are all non-creative modifications and are protected by patent law as long as they are within the scope of the claims of the present invention.
Claims
1. An easy-to-process aluminum alloy sheet for printing, Features The raw material composition includes the following components by weight: Si 0.0452-0.0460%, Mg 0.0006-0.0009%, Cu≤0.0002%, Mn 0.0028-0.0035%, Fe0.320-0.335%, Ti 0.0242-0.0254%, Zn 0.0014-0.0020%, Cr≤0.0005%, Ni 0.005-0.006%, B 0.001-0.002%, Be≤0.0001%, Bi≤0.001%, Cd≤0.001%, Ga≤0.015%, Sb 0.005-0.006%, V0.025-0.028%, the total amount of impurity elements ≤0.20%, and the balance is Al.
2. The easy-to-process aluminum alloy sheet for printing according to claim 1, Features: The easily machined aluminum alloy plate is a cast-rolled plate with a thickness of 6.0-10.0 mm.
3. The easy-to-process aluminum alloy sheet for printing according to claim 1, Features: The easy-to-process aluminum alloy sheet is used to prepare an aluminum plate base for printing by a cold rolling method, and the thickness of the aluminum plate base for printing is 0.1-0.4 mm.
4. The easy-to-process aluminum alloy sheet for printing according to claim 1, Features The method for preparing the easy-to-process aluminum alloy plate comprises the following steps in sequence: S1, material melting: first adding and melting aluminum ingots in a melting furnace, and then adding and melting master alloys to obtain a melt; S2, first refining: firstly adding a refining agent to the molten metal, and performing a first slag removal operation, then adding a mixed gas, and performing a second slag removal operation, and then successively performing heat preservation and pouring operations to obtain a rough casting; S3, second refining: first add and melt the rough casting in a melting furnace, then add mixed gas, perform a third slag removal operation, and then perform heat preservation and pouring operations in sequence to obtain a precision casting; S4, homogenization treatment: firstly add the precision casting billet into the homogenization treatment furnace, and then perform heating, heat preservation, and cooling operations in sequence to obtain a qualified casting billet; S5, extrusion molding: on an extruder, the qualified ingot is sequentially extruded, quenched, and stretched to obtain a preliminary plate; S6. Aging treatment: heating, heat preservation, and cooling the preliminary plate in sequence to obtain the final easy-to-process aluminum alloy plate.
5. The easy-to-process aluminum alloy sheet for printing according to claim 4, Features: In S1, the master alloy is an aluminum alloy, including Al-Cd alloy, Al-Cr alloy, and Al-Ni alloy. The melting temperature of the aluminum ingot is 700-720°C, and the melting temperature of the master alloy is 730-740°C.
6. The easy-to-process aluminum alloy sheet for printing according to claim 4, Features: In S2, the refining agent is added by nitrogen blowing, and the mixed gas includes nitrogen and chlorine.
7. The easy-to-process aluminum alloy sheet for printing according to claim 4, Features: In S3, the melting temperature of the raw ingot is 720-750°C, and the mixed gas includes nitrogen and carbon monoxide gas.
8. The easy-to-process aluminum alloy sheet for printing according to claim 4, Features: In S4, the heating temperature is 400-450°C, the insulation temperature is 320-350°C, the cooling method is air cooling, and the cooling time is 1.5-2.0h, until it cools to room temperature.
9. The easy-to-process aluminum alloy sheet for printing according to claim 4, Features: In S5, the temperature of the extrusion operation is 450-480°C, the quenching method is water mist, and the stretching amount of the stretching operation is 2.0-2.5%.
10. The easy-to-process aluminum alloy sheet for printing according to claim 4, Features: In S6, the temperature of the heating operation is 95-125°C, the temperature of the insulation is 65-80°C, the cooling method is air blowing cooling, and the cooling time is ≥5h, until it is cooled to room temperature.