Recycled rare earth modified high-conductivity 6101 aluminum alloy material and preparation method thereof
By extracting rare earth elements from rare earth magnetic waste and adding them to 6101 aluminum alloy, combining refining and heat treatment processes, the problems of taking into account strength and conductivity of 6101 aluminum alloy materials are solved, and low-cost and high-performance rare earth aluminum alloy materials are realized. The secondary rare earth resources are utilized to improve the mechanical and conductive properties of the materials.
Patent Information
- Application Number
- CN202411244301.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-09-06
AI Technical Summary
The existing 6101 aluminum alloy materials are difficult to take into account between improving strength and conductivity, and rare earth elements are relatively expensive, which limits the research and development and application of high-quality rare earth aluminum alloys.
By extracting rare earth elements Sm or La from rare earth magnetic waste, forming Mg-Sm or Mg-La intermediate alloy and adding it to the 6101 aluminum alloy, combining refining purification treatment and heat treatment processes, a high regeneration rare earth modification can be prepared. Conductive 6101 aluminum alloy material.
It has achieved low-cost, high conductivity and high-strength 6101 aluminum alloy material with tensile strength ≥210 MPa, conductivity ≥58% IACS, and utilized secondary rare earth metal resources to reduce production costs.
Smart Images

Figure CN118756016B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of secondary rare earth recycling and lightweight high-conductivity metal materials, and specifically relates to a high-conductivity 6101 aluminum alloy material modified by recycled rare earth and a preparation method thereof. Background Art
[0002] The electrical conductivity of aluminum is second only to silver, copper and gold. Its density is 25.7% of silver, 30.3% of copper and 13.9% of gold. In particular, the price of aluminum is much lower than these precious metals. Therefore, the development of lightweight, high-strength and high-conductivity aluminum alloy materials is of great significance to the development of industries such as rail transit, electric power and new energy vehicles. 6101 is a low-alloyed Al-Mg-Si aluminum alloy. Compared with other 6XXX aluminum alloys, 6101 aluminum alloy has the characteristics of high specific strength, strong corrosion resistance, excellent conductivity, heat treatment and good formability. In recent years, the rapid development of new energy electric vehicles, electric power, rail transit and other industries has put forward more stringent requirements on the electrical conductivity, mechanical properties, corrosion resistance and preparation cost of 6101 aluminum alloy. According to relevant patents (such as: Announcement No. CN105950893B), the conductivity of aluminum wires for electrical engineering in China can be increased by 0.1% IACS, which can reduce 10 billion kWh of electricity loss each year. In recent years, the composition optimization design of 6101 aluminum alloy and its preparation technology have attracted extensive attention and research from aluminum alloy material scientists and technicians.
[0003] Patents (CN118143074A, CN110093536B, CN115740057A) respectively disclose high-conductivity 6101 aluminum alloy coils for new energy, battery guide plates, and new energy vehicle power supply and their preparation methods. The preparation methods mainly include: preparing wire rods according to the national standard composition of 6101 aluminum alloy, continuously extruding wire rods, aging treatment of extruded profiles, etc., optimizing the extrusion process to improve the performance of the material, and obtaining aluminum coils for new energy with high conductivity, The tensile strength and elongation can be 57.8%IACS, 190MPa, and 13.5% respectively; the conductivity, tensile strength, yield strength, and elongation of the obtained aluminum coil for battery conductor can be 58.5%IACS, 185MPa, 150MPa, and 14% respectively; the conductivity, tensile strength, yield strength, and elongation of the obtained aluminum alloy coil for power supply of new energy vehicles can be 59.5%IACS, 105MPa, 55MPa, and 18% respectively.
[0004] The patent (CN116748326A) discloses a 6101-T63 state aluminum alloy conductive profile and its preparation method and application. The preparation method mainly includes: melting and casting aluminum rods according to the national standard composition of 6101 aluminum alloy, homogenization treatment, preheating cast rods and extrusion dies, extrusion, solution treatment, artificial aging treatment and other steps. The wall thickness of the conductive profile after forming is not more than 8mm, its conductivity is ≥56%IACS, tensile strength is ≥185MPa, yield strength is ≥150MPa, straightness is ≤0.5mm / m, and cross-sectional profile is ≤0.2mm.
[0005] The patent (CN117587306A) discloses a 6101 aluminum alloy plate with improved alloy strength and electrical conductivity and a preparation method thereof. The composition of the plate is as follows by mass percentage: 0.46~0.57% Mg, 0.39~0.42% Si, 0.06~0.36% Fe, 0.07% La, 0.13% Ce, Cu≤0.1%, Mn≤0.03%, Cr≤0.03%, the total amount of unavoidable impurities does not exceed 0.1%, and the balance is Al. The preparation method mainly includes the steps of preparing aluminum alloy ingots, homogenizing treatment, rolling deformation, etc. The method adds mixed rare earth containing La and Ce to the alloy before refining the 6101 aluminum alloy melt, and then homogenizes and rolls the alloy ingot. The tensile strength of the prepared alloy is 177.3MPa~201.8MPa, but the electrical conductivity is only 42.5%IACS~43.99%IACS.
[0006] Patents (CN108546850A and CN116356184A) respectively disclose a method for producing a highly conductive 6101 aluminum alloy sheet and a 6101 aluminum alloy sheet for vehicles and its preparation method and application. They both use the national standard composition of 6101 aluminum alloy to melt and cast aluminum alloy ingots, reduce the content of impurity elements and retain necessary strengthening elements in a specific proportion, optimize the proportion of Si, Fe, and Mg elements, and then go through the corresponding sheet rolling and heat treatment process. Among them, the sheet prepared by patent (CN108546850A) has an electrical conductivity of 59.75% IACS, a tensile strength of 116 MPa, a yield strength of 85 MPa, and an elongation of 29%, and the sheet prepared by patent (CN116356184A) has an electrical conductivity of ≥56%, a tensile strength of ≥185 MPa, and a yield strength of 155~175 MPa.
[0007] The patent (CN111850350A) discloses aluminum alloy materials for new energy vehicle fuses and their preparation methods. The alloy components are 0.4-0.75% magnesium, 0.4-0.75% silicon, 0.05-0.5% iron, 0.05-0.2% copper, 0.05-0.2% zinc, 0.01-0.1% manganese, 0.01-0.1% chromium, 0.04-0.1% boron and 0.03-0.15% mixed rare earth, and the balance is aluminum. After adding mixed rare earth elements to the 6101 aluminum alloy raw material, the tensile strength of the material is about 195MPa and the conductivity is about 56%IACS.
[0008] The patent (CN117265348A) discloses a medium-strength and high-conductivity aluminum alloy sheet and its preparation method. The alloy composition is as follows: 0.45~0.53% Mg, 0.4~0.46% Si, 0.1~0.5% Cu, Fe ≤ 0.16%, Zn ≤0.01%, Mn ≤ 0.03%, Cr ≤ 0.02%, and the balance is impurities and Al. The preparation method mainly includes the steps of aluminum alloy ingot preparation, heat treatment, rolling, solid solution aging treatment, etc. An appropriate amount of Cu element is added to the national standard composition of 6101 aluminum alloy. The conductivity of the prepared aluminum alloy sheet is above 53% IACS, the tensile strength is higher than 187MPa, and the hardness is greater than 71HV.
[0009] In addition, the paper (Zhang Ruifeng, Dong Yaguang, Tan Rui, Zhao Hongliang. Effect of mixed rare earth on the cast structure of 6101 aluminum alloy for overhead wires, Henan Science and Technology Innovation Drive, 2016.09) reported that the average grain size of the cast structure with 0.2% mixed rare earth added was 37.02 microns, which was 39.6% smaller than that without addition. The paper (Peng Xiaolan, Wang Hongcheng. Research on the performance optimization of Al-Mg-Si 6101 aluminum alloy for radiator, Journal of Dongguan University of Technology, 2015, 22(3):7-11) reported that adding appropriate amounts of B and Gd elements to 6101 aluminum alloy can improve the mechanical, electrical and thermal conductivity of 6101 aluminum alloy. In addition, the dissertation (Huang Jiajun, Research on Composition Improvement and Performance Balance Optimization of 6101 Alloy for Subway Conductor Rail, South China University of Technology, 2022.4) studied the effects of elements such as Ni, Ce, Cu and Zn on the microstructure and properties of 6101 aluminum alloy. The results show that Cu and Zn can promote alloy aging strengthening, but the conductivity of the alloy decreases after the content increases; the rare earth element Ce can improve the conductivity of the alloy, but significantly reduces the mechanical properties of the alloy; Ni is a better element for improving the microstructure of 6101 aluminum alloy and achieving performance balance optimization; after optimizing the alloy composition and heat treatment process, the conductivity and tensile strength of the material are 55.2%IACS and 242.2MPa respectively. The dissertation (Liu Zhenxing, Research on Aging Heat Treatment of 6101 Aluminum Alloy, Central South University, 2013.5) studied the effect of precipitation phase type and precipitation phase characteristics on the conductivity of 6101 aluminum alloy under different aging systems.
[0010] In summary, 6101 aluminum alloy has its own advantages and disadvantages in material preparation methods. Due to the inverted relationship between the strength and conductivity of the material, it is difficult to simultaneously improve the strength and conductivity, so that the comprehensive mechanical and conductive properties of the material are often insufficient. The appropriate addition of alloying elements is relatively simple, clean and efficient in synergistically improving the mechanical properties and conductive properties of aluminum alloys. In particular, the addition of an appropriate amount of rare earth elements can not only purify the aluminum alloy melt and refine the grains, but also have a metamorphic effect on the second phase and improve the corrosion resistance of the aluminum alloy. However, rare earth elements are more expensive than components such as Al, Mg, and Si in 6101 aluminum alloy, which brings certain restrictions to the research and development, production and application of high-quality rare earth aluminum alloys. With the continuous development of the aluminum industry and the improvement of requirements for aluminum alloy performance, preparation cost and cycle, it is urgently needed to develop new methods and technologies from the source of raw materials and preparation efficiency. Summary of the invention
[0011] The purpose of the present invention is to provide a high-conductivity 6101 aluminum alloy material modified by recycled rare earth and a preparation method thereof, so as to obtain a low-cost, high-conductivity 6101 aluminum alloy material modified by recycled rare earth, so as to meet the demand for high-conductivity 6101 aluminum alloy material and a low-cost preparation method thereof in industrial production.
[0012] In order to achieve the above object, the technical solution adopted by the present invention is:
[0013] A high-conductivity 6101 aluminum alloy material modified by recycled rare earth. The aluminum alloy composition comprises, by mass percentage, 0.03-0.3% of recycled rare earth element Sm or La, 0.05-0.1% of iron Fe, and the remainder of 6101 aluminum alloy.
[0014] The recycled rare earth modified high-conductivity 6101 aluminum alloy material, the added recycled rare earth elements Sm and La are respectively derived from the Mg-Sm intermediate alloy and Mg-La intermediate alloy formed by extracting the rare earth elements Sm and La from rare earth magnetic waste using Mg as a collector, and the rare earth magnetic waste is a samarium cobalt permanent magnet alloy or a lanthanum iron silicon alloy.
[0015] The method for preparing the recycled rare earth modified high-conductivity 6101 aluminum alloy material comprises the following steps:
[0016] (1) Prepare alloy raw materials according to the national standard composition requirements of 6101 aluminum alloy;
[0017] (2) Place the aluminum ingot into a smelting furnace for melting and adjust the melt temperature to 740°C~770°C;
[0018] (3) adding silicon and iron elements to the melt in the form of Al-Si master alloy and Al-Fe master alloy, and stirring the alloy melt to obtain a 6101 aluminum alloy melt;
[0019] (4) The alloy melt temperature is lowered to 690°C~720°C, and part of the magnesium content in the 6101 aluminum alloy is added in the form of Al-Mg master alloy;
[0020] (5) The melt temperature is heated to 740°C to 770°C, and a refining agent and argon gas are introduced into the melt for purification;
[0021] (6) The temperature of the aluminum alloy melt is adjusted to 690°C to 720°C, rare earth elements Sm or La and the remaining Mg in the 6101 aluminum alloy are added in the form of Mg-Sm master alloy or Mg-La master alloy, and the alloy melt is stirred and kept at a constant temperature to obtain an alloy melt with uniform composition;
[0022] (7) pouring the alloy melt into a mold, cooling it, and obtaining an aluminum alloy ingot after solidification;
[0023] (8) heating the aluminum alloy ingot to 460°C~490°C and keeping it at this temperature for 8~16 h for homogenization treatment;
[0024] (9) heating the homogenized ingot to 510°C to 540°C and keeping it at that temperature for 1 to 6 hours to perform solution quenching;
[0025] (10) performing rolling deformation treatment on the ingot after solution quenching treatment;
[0026] (11) The deformed alloy profile is heated to 175°C~210°C and kept at this temperature for 4~18 hours for aging treatment to obtain a recycled rare earth modified high conductive 6101 aluminum alloy material.
[0027] The preparation method of the recycled rare earth modified high-conductivity 6101 aluminum alloy material, in step (5), its composition, by mass percentage, is 40% sodium cryolite, 46% salt slag of Al5Ti1B master alloy prepared by fluoride salt reaction, 10% aluminum fluoride, 2% calcium fluoride, and 2% potassium feldspar.
[0028] The method for preparing the high-conductivity 6101 aluminum alloy material modified by recycled rare earth, in step (6), using Mg element to extract the rare earth elements Sm and La in the rare earth magnetic waste to prepare Mg-Sm and Mg-La master alloys respectively, comprises the following steps:
[0029] The first step is to sequentially clean, dry and crush the rare earth magnetic waste to obtain rare earth magnetic waste particles with an effective diameter of no more than 5 mm;
[0030] The second step is to place the rare earth magnetic waste particles in a magnesium melt at a temperature of 750-1050°C under argon protection, keep the temperature and stir for 10-45 minutes, and then let the melt stand for 20-60 minutes;
[0031] The third step is to pour the upper layer of magnesium melt containing rare earth elements into a mold to cool and solidify to form a Mg-Sm master alloy or a Mg-La master alloy.
[0032] In the preparation method of the recycled rare earth modified high-conductivity 6101 aluminum alloy material, in the first step, the crushing process needs to be carried out under an inert gas protection environment, and the diameter of the rare earth magnetic waste particles is 1-3 mm.
[0033] In the method for preparing the recycled rare earth modified high-conductivity 6101 aluminum alloy material, in the second step, the mass ratio of magnesium to rare earth magnetic waste is 0.2-0.8.
[0034] In the preparation method of the recycled rare earth modified high-conductivity 6101 aluminum alloy material, in the second step, the magnesium melt temperature and the insulation stirring time in the preparation process of the Mg-Sm master alloy or the Mg-La master alloy are 850° C., 35 min and 950° C., 25 min respectively.
[0035] In the preparation method of the recycled rare earth modified high-conductivity 6101 aluminum alloy material, in the third step, the upper layer of rare earth element-containing magnesium melt is poured into a water-cooled iron mold or copper mold for rapid cooling to obtain a magnesium-rare earth intermediate alloy with uniform tissue distribution.
[0036] The method for preparing the recycled rare earth modified high-conductivity 6101 aluminum alloy material, in the third step, the content of Sm or La in the prepared Mg-Sm master alloy or Mg-La master alloy is 10% to 40% by mass percentage, and the total content of impurity elements Co and Fe is < 0.1%.
[0037] The principle of the present invention is as follows:
[0038] The present invention is mainly based on the interaction law between metal atoms and the selective distribution of the third component in the two phases, so that the rare earth elements in the waste samarium cobalt and lanthanum iron silicon magnets are dissolved into another liquid metal. The interaction effect between atoms of different elements is related to the value of mixing enthalpy. When the mixing enthalpy is a positive value, it means that the two element atoms repel each other and are insoluble in each other, and when the mixing enthalpy is a negative value, it means that the two element atoms attract each other and have a strong affinity. Considering the application of rare earth metals in 6XXX series aluminum alloys, magnesium, a component in 6XXX aluminum alloys, is selected as a capture agent for rare earth elements in samarium cobalt and lanthanum iron silicon magnets. At the same time, magnesium is immiscible with other elements in the magnet except rare earth elements, so as to ensure that the content of impurity elements in the prepared Mg-Sm and Mg-La intermediate alloys is low. After the rare earth elements in the samarium cobalt and lanthanum iron silicon magnets dissolve into the magnesium melt, a magnesium-rare earth alloy liquid phase with a relatively low density is formed. After the rare earth in the magnet is extracted, the remaining Co-Fe-based alloy with a higher density is separated into two immiscible phases in the crucible, and then separated to obtain a magnesium-rare earth intermediate alloy that can be used for aluminum alloys and a reusable iron-cobalt alloy.
[0039] Compared with the two Chinese invention patents (CN116751994A, CN117025958A) applied by the inventor in the early stage, the collector used in the present invention is magnesium metal which can be used in aluminum alloy, and the specific implementation scheme and process parameters are different, with different innovations, goals and effects. The present invention uses magnesium to extract the rare earth elements Sm and La from samarium cobalt and lanthanum iron silicon alloy waste, and the formed Mg-Sm and Mg-La intermediate alloys have the characteristics of low production cost, simple preparation and significant effect in 6101 aluminum alloy.
[0040] The rare earth element Sm or La is added to the high-conductivity 6101 aluminum alloy of the present invention, and the improvement of the performance of the alloy is mainly attributed to the following aspects: 1) the size of the matrix α-Al grains is refined. After the rare earth element Sm or La is added, the nucleation rate of the primary phase α-Al can be increased, which plays a role in refining the matrix grains, thereby improving the strength and plastic deformation ability of the material; 2) after the rare earth element Sm or La is added, the precipitation activation energy can be reduced, the precipitation of the second phase in the matrix Al is promoted, and the solid solution amount of other elements in the Al matrix is reduced; on the one hand, the number density of the (Mg, Si) precipitation phase and the AlFeSi precipitation phase in the alloy is increased, thereby playing a precipitation strengthening effect; on the other hand, the solid solubility of elements such as Mg and Si in the matrix is reduced, which helps to reduce the scattering effect of the solid solution elements on electrons and improve the electrical conductivity of the alloy; 3) the addition of the rare earth element Sm or La helps to modify the iron-rich phase, thereby improving the mechanical and corrosion resistance properties of the aluminum alloy.
[0041] The advantages and beneficial effects of the present invention are as follows:
[0042] The present invention adds an appropriate amount of rare earth elements to the aluminum alloy, which can not only purify the aluminum alloy melt and refine the grains, but also have a metamorphic effect on the second phase and improve the corrosion resistance of the aluminum alloy, and has the effect of improving quality and efficiency. However, rare earth elements are relatively expensive and will increase production costs. To this end, the present invention not only provides a way to recycle and reuse secondary rare earth metal resources in waste samarium cobalt and lanthanum iron silicon magnets, gives full play to the role of secondary rare earth metals in aluminum alloys, but also provides a new method for the production of low-cost, high-quality rare earth aluminum alloy materials. The high-conductivity 6101 aluminum alloy material prepared by the present invention using recycled rare earth modification has excellent mechanical properties and electrical conductivity, high strength and good electrical conductivity, and its tensile strength is ≥210 MPa and electrical conductivity is ≥58%IACS. The present invention provides a new method for the development of low-cost, high-quality rare earth aluminum alloy materials, as well as the separation, recycling and reuse of strategically critical secondary metal resources, and has beneficial effects in the fields of new energy vehicles, electricity, rail transportation, resources and environment. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] Figure 1 The microstructure of the cast 6101 aluminum alloy modified with 0.05% (mass percentage) of the recycled rare earth element Sm prepared according to the method of Example 1. The black phase is the α-Al matrix, and the white phase is mainly the AlFeSi iron-rich phase.
[0044] Figure 2 This is the cast microstructure morphology of 6101 aluminum alloy modified with 0.1% (mass percentage) of recycled rare earth element Sm prepared according to the method of Example 2. The black phase is the α-Al matrix, and the white phase is mainly the AlFeSi iron-rich phase.
[0045] Figure 3The microstructure of the cast 6101 aluminum alloy modified with 0.25% (mass percentage) of the recycled rare earth element Sm prepared according to the method of Example 3. The black phase is the α-Al matrix, and the white phase is mainly the AlFeSi iron-rich phase.
[0046] Figure 4 The microstructure of the cast state of 6101 aluminum alloy modified with 0.05% (mass percentage) of recycled rare earth La prepared according to the method of Example 4. The black phase is the α-Al matrix, and the white phase is mainly the AlFeSi iron-rich phase.
[0047] Figure 5 This is the cast microstructure morphology of 6101 aluminum alloy modified with 0.1% (mass percentage) of recycled rare earth La prepared according to the method of Example 5. The black phase is the α-Al matrix, and the white phase is mainly the AlFeSi iron-rich phase.
[0048] Figure 6 This is the cast microstructure morphology of 6101 aluminum alloy modified with 0.1% (mass percentage) native rare earth La prepared according to the method of Comparative Example 1. The black phase is the α-Al matrix, and the white phase is mainly the AlFeSi iron-rich phase.
[0049] Figure 7 This is the cast microstructure morphology of 6101 aluminum alloy without any rare earth modification prepared according to the method of Comparative Example 2. The black phase is the α-Al matrix, and the white phase is mainly the AlFeSi iron-rich phase. DETAILED DESCRIPTION
[0050] In the specific implementation process, the present invention adopts a high-conductivity 6101 aluminum alloy material modified by recycled rare earth. The aluminum alloy composition includes components by mass percentage: rare earth element Sm or La 0.03-0.3%, iron Fe≤0.1%, and the balance is 6101 aluminum alloy. The added rare earth elements Sm and La are respectively derived from Mg-Sm master alloy and Mg-La master alloy formed by extracting rare earth elements Sm and La from rare earth magnetic waste using Mg element as a collector. Firstly, Mg element is used to extract rare earth elements Sm and La in rare earth magnetic waste (samarium-cobalt permanent magnet alloy or lanthanum-iron-silicon alloy) to prepare Mg-Sm and Mg-La master alloys; secondly, raw materials are prepared according to the national standard composition of 6101 aluminum alloy, and the aluminum ingot is melted, and the elements Si, Fe, and Mg are added to the aluminum melt in turn, and the alloy melt is stirred and kept warm; then, a refining agent and argon gas are introduced into the melt for refining; subsequently, the rare earth element Sm or La is added to the alloy melt in the form of recycled Mg-Sm master alloy or Mg-La master alloy, respectively, and after stirring and standing, a uniform melt is obtained, which is then cast into an ingot; finally, the ingot is subjected to homogenization, solution quenching, rolling deformation, and aging treatment in turn to obtain a low-cost, high-conductivity 6101 aluminum alloy material modified with recycled rare earth.
[0051] The method for extracting rare earth elements Sm and La from rare earth magnetic waste by using Mg element to prepare Mg-Sm and Mg-La master alloys respectively comprises the following steps:
[0052] (1) Cleaning, drying and crushing the rare earth magnetic waste (samarium-cobalt permanent magnet alloy or lanthanum-iron-silicon alloy) in sequence to obtain rare earth magnetic waste particles with an effective diameter of no more than 5 mm;
[0053] (2) Under argon protection, the rare earth magnetic waste particles are placed in a magnesium melt at a temperature of 750-1050°C. After heat preservation and stirring for 10-45 minutes, the melt is allowed to stand for 20-60 minutes.
[0054] (3) The upper layer of magnesium melt containing rare earth elements is poured into a mold and cooled and solidified to form a Mg-Sm master alloy or a Mg-La master alloy.
[0055] In the step (1) of extracting the rare earth elements Sm and La from the rare earth magnetic waste with the Mg element to prepare Mg-Sm and Mg-La master alloys respectively, the crushing process needs to be carried out under an inert gas protection environment, and the diameter of the rare earth magnetic waste particles is preferably 1-3 mm.
[0056] In the step (2) of extracting the rare earth elements Sm and La in the rare earth magnetic waste with the Mg element to prepare Mg-Sm and Mg-La master alloys respectively, the mass ratio of metallic magnesium to the rare earth magnetic waste is preferably 0.2-0.8.
[0057] In the step (2) of extracting the rare earth elements Sm and La from the rare earth magnetic waste with the Mg element to prepare Mg-Sm and Mg-La master alloys respectively, the magnesium melt temperature and the insulation stirring time in the preparation process of the Mg-Sm master alloy and the Mg-La master alloy are preferably 850°C, 35 min and 950°C, 25 min, respectively.
[0058] In step (3) of extracting rare earth elements Sm and La from rare earth magnetic waste using Mg element to prepare Mg-Sm and Mg-La master alloys respectively, the upper layer of magnesium melt containing rare earth elements is poured into a water-cooled iron mold or copper mold and rapidly cooled to obtain a magnesium rare earth master alloy with uniform microstructure distribution.
[0059] In the step (3) of extracting the rare earth elements Sm and La from the rare earth magnetic waste with the Mg element to prepare Mg-Sm and Mg-La master alloys respectively, the content of Sm or La in the prepared Mg-Sm master alloy or Mg-La master alloy is 10% to 40% by mass, and the total content of impurity elements (such as Co, Fe, etc.) is less than 0.1%.
[0060] A method for preparing a high-conductivity 6101 aluminum alloy material modified by recycled rare earth, the method comprising the following steps:
[0061] (1) Prepare alloy raw materials according to the national standard composition requirements of 6101 aluminum alloy;
[0062] (2) Place the aluminum ingot into a smelting furnace for melting and adjust the melt temperature to 740°C~770°C;
[0063] (3) adding silicon and iron elements to the melt in the form of Al-Si master alloy or Al-Fe master alloy, and stirring the alloy melt to obtain an aluminum alloy melt;
[0064] (4) The alloy melt temperature is lowered to 690°C~720°C, and part of the magnesium content in the 6101 aluminum alloy is added in the form of Al-Mg master alloy;
[0065] (5) heating the melt to a temperature of 740°C to 770°C, introducing a refining agent (in terms of mass percentage, the composition of which is 40% sodium cryolite, 46% salt slag for preparing Al5Ti1B master alloy by fluoride salt reaction, 10% aluminum fluoride, 2% calcium fluoride, and 2% potassium feldspar) into the melt and introducing argon gas for purification;
[0066] (6) The temperature of the aluminum alloy melt is adjusted to 690°C to 720°C, rare earth elements Sm or La and the remaining Mg in the 6101 aluminum alloy are added in the form of a prepared Mg-Sm master alloy or Mg-La master alloy, and the alloy melt is stirred and kept at a temperature to obtain an alloy melt with uniform composition;
[0067] (7) pouring the alloy melt into a mold, cooling it, and obtaining an aluminum alloy ingot after solidification;
[0068] (8) heating the aluminum alloy ingot to 460°C~490°C and keeping it at this temperature for 8~16 h for homogenization treatment;
[0069] (9) heating the homogenized ingot to 510°C to 540°C and keeping it at that temperature for 1 to 6 hours to perform solution quenching;
[0070] (10) performing rolling deformation treatment on the ingot after solution quenching treatment;
[0071] (11) The deformed alloy profile is heated to 175°C~210°C and kept at this temperature for 4~18 hours for aging treatment to obtain a recycled rare earth modified high conductive 6101 aluminum alloy material.
[0072] In addition, the salt slag of Al5Ti1B master alloy prepared by fluoride salt reaction has the following main components and contents: by mass percentage, 60%~90% potassium fluoroaluminate, 0%~24% potassium fluoride, 0%~27% aluminum fluoride, and 0~6% magnesium fluoride.
[0073] The present invention is described in detail below in conjunction with the accompanying drawings and embodiments, but the protection scope and application scope of the present invention are not limited to the following embodiments.
[0074] Example 1
[0075] In this embodiment, the composition of the high-conductivity 6101 aluminum alloy material modified by recycled rare earth is as follows: rare earth element Sm 0.05%, iron Fe 0.1%, and the balance is 6101 aluminum alloy. As follows: magnesium 0.6%, silicon 0.35%, and the balance is Al in the 6101 aluminum alloy.
[0076] In this embodiment, the preparation method of Mg-Sm master alloy comprises the following steps:
[0077] (1) The surface of the samarium cobalt permanent magnet alloy scrap is cleaned and dried in sequence, and then the samarium cobalt bulk alloy is crushed into particles with a diameter of 1 to 3 mm under an inert gas protection environment;
[0078] (2) The magnesium block was melted in a heating furnace under argon protection according to the mass ratio of metal magnesium to samarium-cobalt permanent magnet alloy particles of 0.6, and then the samarium-cobalt permanent magnet alloy particles were gradually added to the magnesium melt, kept at 850°C and stirred for 35 minutes, and then allowed to stand for 30 minutes;
[0079] (3) The upper layer of magnesium melt containing rare earth elements in the crucible is poured into a water-cooled iron mold for rapid cooling and solidification to obtain a Mg-Sm master alloy.
[0080] Calculated by mass percentage, the prepared Mg-Sm master alloy has the following components: rare earth element Sm 27%, impurity elements Fe 0.03% and Co 0.04%, and the balance Mg.
[0081] In this embodiment, the method for preparing a high-conductivity 6101 aluminum alloy material modified by the recycled rare earth element Sm comprises the following steps:
[0082] (1) Prepare raw materials according to ingredient requirements;
[0083] (2) Place the aluminum ingot into a melting furnace for melting and adjust the melt temperature to 750°C;
[0084] (3) adding silicon and iron elements to the melt in the form of Al-Si master alloy or Al-Fe master alloy, and stirring the alloy melt to obtain an aluminum alloy melt;
[0085] (4) The alloy melt temperature is lowered to 720°C, and a portion of the magnesium in the aluminum alloy is added in the form of an Al-Mg master alloy;
[0086] (5) heating the melt to 750°C, introducing a refining agent (in terms of mass percentage, the composition of which is 40% sodium cryolite, 46% salt slag for preparing Al5Ti1B master alloy by fluoride salt reaction, 10% aluminum fluoride, 2% calcium fluoride, and 2% potassium feldspar) and introducing argon gas for purification;
[0087] (6) adjusting the temperature of the aluminum alloy melt to 720° C., adding the rare earth element Sm and the remaining portion of Mg in the form of the Mg-Sm master alloy prepared above, and stirring the alloy melt and keeping it at a constant temperature to obtain an alloy melt with uniform composition;
[0088] (7) pouring the alloy melt into a mold, cooling it, and obtaining an aluminum alloy ingot after solidification;
[0089] (8) heating the aluminum alloy ingot to 470°C and keeping it at this temperature for 12 h for homogenization treatment;
[0090] (9) heating the homogenized ingot to 530°C and keeping it at that temperature for 4 h to perform a solution quenching treatment on it;
[0091] (10) performing rolling deformation treatment on the ingot after solution quenching treatment;
[0092] (11) The deformed alloy profile is heated to 195°C and kept at this temperature for 12 h for aging treatment to obtain a 6101 aluminum alloy material modified with a secondary rare earth metal Sm.
[0093] like Figure 1 As shown in FIG. 1 , the microstructure of the high-conductivity 6101 aluminum alloy material modified by the recycled rare earth element Sm in this embodiment has a tensile strength of 225 MPa and an electrical conductivity of 58.31% IACS.
[0094] Example 2
[0095] In this embodiment, the composition of the high-conductivity 6101 aluminum alloy material modified by recycled rare earth is as follows: rare earth element Sm 0.1%, iron Fe 0.1%, and the balance is 6101 aluminum alloy. As follows: magnesium 0.6%, silicon 0.35%, and the balance is Al in the 6101 aluminum alloy.
[0096] In this embodiment, the preparation method of Mg-Sm master alloy comprises the following steps:
[0097] (1) The surface of the samarium cobalt permanent magnet alloy scrap is cleaned and dried in sequence, and then the samarium cobalt bulk alloy is crushed into particles with a diameter of 1 to 3 mm under an inert gas protection environment;
[0098] (2) The magnesium block was melted in a heating furnace under argon protection according to the mass ratio of metal magnesium to samarium-cobalt permanent magnet alloy particles of 0.6, and then the samarium-cobalt permanent magnet alloy particles were gradually added to the magnesium melt, kept at 850°C and stirred for 35 minutes, and then allowed to stand for 30 minutes;
[0099] (3) The upper layer of magnesium melt containing rare earth elements in the crucible is poured into a water-cooled iron mold for rapid cooling and solidification to obtain a Mg-Sm master alloy.
[0100] Calculated by mass percentage, the prepared Mg-Sm master alloy has the following components: rare earth element Sm 27%, impurity elements Fe 0.02% and Co 0.05%, and the balance Mg.
[0101] In this embodiment, the method for preparing a high-conductivity 6101 aluminum alloy material modified by the recycled rare earth element Sm comprises the following steps:
[0102] (1) Prepare raw materials according to ingredient requirements;
[0103] (2) Place the aluminum ingot into a melting furnace for melting and adjust the melt temperature to 750°C;
[0104] (3) adding silicon and iron elements to the melt in the form of Al-Si master alloy or Al-Fe master alloy, and stirring the alloy melt to obtain an aluminum alloy melt;
[0105] (4) The alloy melt temperature is lowered to 720°C, and a portion of the magnesium in the aluminum alloy is added in the form of an Al-Mg master alloy;
[0106] (5) heating the melt to 750°C, introducing a refining agent (in terms of mass percentage, the composition of which is 40% sodium cryolite, 46% salt slag for preparing Al5Ti1B master alloy by fluoride salt reaction, 10% aluminum fluoride, 2% calcium fluoride, and 2% potassium feldspar) and introducing argon gas for purification;
[0107] (6) adjusting the temperature of the aluminum alloy melt to 720° C., adding the rare earth element Sm and the remaining portion of Mg in the form of the Mg-Sm master alloy prepared above, and stirring the alloy melt and keeping it at a constant temperature to obtain an alloy melt with uniform composition;
[0108] (7) pouring the alloy melt into a mold, cooling it, and obtaining an aluminum alloy ingot after solidification;
[0109] (8) heating the aluminum alloy ingot to 470°C and keeping it at this temperature for 12 h for homogenization treatment;
[0110] (9) heating the homogenized ingot to 530°C and keeping it at that temperature for 4 h to perform a solution quenching treatment on it;
[0111] (10) performing rolling deformation treatment on the ingot after solution quenching treatment;
[0112] (11) The deformed alloy profile is heated to 195°C and kept at this temperature for 12 h for aging treatment to obtain a 6101 aluminum alloy material modified with a secondary rare earth metal Sm.
[0113] like Figure 2 As shown in the figure, the microstructure of the highly conductive 6101 aluminum alloy material modified by the recycled rare earth element Sm in this embodiment has a tensile strength of 231 MPa and an electrical conductivity of 59.02% IACS. Compared with Example 1, the appropriate increase in the amount of Sm added in this embodiment can make the iron-rich phase finer, from needle-shaped to granular, and can also increase the material strength and electrical conductivity at the same time.
[0114] Example 3
[0115] In this embodiment, the composition of the high-conductivity 6101 aluminum alloy material modified by recycled rare earth is as follows: rare earth element Sm 0.25%, iron Fe 0.05%, and the balance is 6101 aluminum alloy. As follows: magnesium 0.6%, silicon 0.35%, and the balance is Al in the 6101 aluminum alloy.
[0116] In this embodiment, the preparation method of Mg-Sm master alloy comprises the following steps:
[0117] (1) The surface of the samarium cobalt permanent magnet alloy scrap is cleaned and dried in sequence, and then the samarium cobalt bulk alloy is crushed into particles with a diameter of 1 to 3 mm under an inert gas protection environment;
[0118] (2) The magnesium block was melted in a heating furnace under argon protection according to the mass ratio of metal magnesium to samarium-cobalt permanent magnet alloy particles of 0.6, and then the samarium-cobalt permanent magnet alloy particles were gradually added to the magnesium melt, kept at 850°C and stirred for 35 minutes, and then allowed to stand for 30 minutes;
[0119] (3) The upper layer of magnesium melt containing rare earth elements in the crucible is poured into a water-cooled iron mold for rapid cooling and solidification to obtain a Mg-Sm master alloy.
[0120] Calculated by mass percentage, the prepared Mg-Sm master alloy comprises: rare earth element Sm 27%, impurity elements Fe 0.01% and Co 0.03%, and the balance is Mg.
[0121] In this embodiment, the method for preparing a high-conductivity 6101 aluminum alloy material modified by the recycled rare earth element Sm comprises the following steps:
[0122] (1) Prepare raw materials according to ingredient requirements;
[0123] (2) Place the aluminum ingot into a melting furnace for melting and adjust the melt temperature to 750°C;
[0124] (3) adding silicon and iron elements to the melt in the form of Al-Si master alloy or Al-Fe master alloy, and stirring the alloy melt to obtain an aluminum alloy melt;
[0125] (4) The alloy melt temperature is lowered to 720°C, and a portion of the magnesium in the aluminum alloy is added in the form of an Al-Mg master alloy;
[0126] (5) heating the melt to 750°C, introducing a refining agent (in terms of mass percentage, the composition of which is 40% sodium cryolite, 46% salt slag for preparing Al5Ti1B master alloy by fluoride salt reaction, 10% aluminum fluoride, 2% calcium fluoride, and 2% potassium feldspar) and introducing argon gas for purification;
[0127] (6) adjusting the temperature of the aluminum alloy melt to 720° C., adding the rare earth element Sm and the remaining portion of Mg in the form of the Mg-Sm master alloy prepared above, and stirring the alloy melt and keeping it at a constant temperature to obtain an alloy melt with uniform composition;
[0128] (7) pouring the alloy melt into a mold, cooling it, and obtaining an aluminum alloy ingot after solidification;
[0129] (8) heating the aluminum alloy ingot to 470°C and keeping it at this temperature for 12 h for homogenization treatment;
[0130] (9) heating the homogenized ingot to 530°C and keeping it at that temperature for 4 h to perform a solution quenching treatment on it;
[0131] (10) performing rolling deformation treatment on the ingot after solution quenching treatment;
[0132] (11) The deformed alloy profile is heated to 195°C and kept at this temperature for 12 h for aging treatment to obtain a 6101 aluminum alloy material modified with a secondary rare earth metal Sm.
[0133] like Figure 3 As shown in the figure, the microstructure of the highly conductive 6101 aluminum alloy material modified by the recycled rare earth element Sm in this embodiment has a tensile strength of 214 MPa and an electrical conductivity of 58.11% IACS. Compared with Example 2, this embodiment continues to increase the amount of Sm added but produces more needle-shaped iron-rich phases, and the material strength and electrical conductivity are slightly reduced.
[0134] Example 4
[0135] In this embodiment, the composition of the high-conductivity 6101 aluminum alloy material modified by recycled rare earth is as follows: rare earth La 0.05%, iron Fe 0.08%, and the balance is 6101 aluminum alloy. As follows: in 6101 aluminum alloy, magnesium 0.6%, silicon 0.35%, and the balance is Al.
[0136] In this embodiment, the preparation method of Mg-La master alloy comprises the following steps:
[0137] (1) The lanthanum iron silicon alloy waste is sequentially surface cleaned and dried, and then the lanthanum iron silicon bulk alloy is crushed into particles with a diameter of 1 to 3 mm under an inert gas protection environment;
[0138] (2) The magnesium block was melted in a heating furnace under argon protection according to the mass ratio of metallic magnesium to lanthanum iron silicon alloy particles of 0.3, and then the lanthanum iron silicon alloy particles were gradually added to the magnesium melt, kept at 950 ° C and stirred for 35 minutes, and then allowed to stand for 30 minutes;
[0139] (3) The upper layer of magnesium melt containing rare earth elements in the crucible is poured into a water-cooled iron mold for rapid cooling and solidification to obtain a Mg-La intermediate alloy.
[0140] Calculated by mass percentage, the prepared Mg-La master alloy has the following components: 21% rare earth La, 0.04% impurity elements Fe and 0.02% Co, and the balance Mg.
[0141] In this embodiment, the method for preparing a high-conductivity 6101 aluminum alloy material modified by recycled rare earth La comprises the following steps:
[0142] (1) Prepare raw materials according to ingredient requirements;
[0143] (2) Place the aluminum ingot into a melting furnace for melting and adjust the melt temperature to 750°C;
[0144] (3) adding silicon and iron elements to the melt in the form of Al-Si master alloy or Al-Fe master alloy, and stirring the alloy melt to obtain an aluminum alloy melt;
[0145] (4) The alloy melt temperature is lowered to 720°C, and a portion of the magnesium in the aluminum alloy is added in the form of an Al-Mg master alloy;
[0146] (5) heating the melt to 750°C, introducing a refining agent (in terms of mass percentage, the composition of which is 40% sodium cryolite, 46% salt slag for preparing Al5Ti1B master alloy by fluoride salt reaction, 10% aluminum fluoride, 2% calcium fluoride, and 2% potassium feldspar) and introducing argon gas for purification;
[0147] (6) adjusting the temperature of the aluminum alloy melt to 720° C., adding the rare earth element La and the remaining portion of Mg in the form of the Mg-La master alloy prepared above, and stirring the alloy melt and keeping it at a constant temperature to obtain an alloy melt with uniform composition;
[0148] (7) pouring the alloy melt into a mold, cooling it, and obtaining an aluminum alloy ingot after solidification;
[0149] (8) heating the aluminum alloy ingot to 470°C and keeping it at this temperature for 12 h for homogenization treatment;
[0150] (9) heating the homogenized ingot to 530°C and keeping it at that temperature for 4 h to perform a solution quenching treatment on it;
[0151] (10) performing rolling deformation treatment on the ingot after solution quenching treatment;
[0152] (11) The deformed alloy profile is heated to 195°C and kept at this temperature for 12 h for aging treatment to obtain a 6101 aluminum alloy material modified with the secondary rare earth metal La.
[0153] like Figure 4 As shown in FIG. 1 , the microstructure of the high-conductivity 6101 aluminum alloy material modified by recycled rare earth La in this embodiment has a tensile strength of 219 MPa and an electrical conductivity of 58.45% IACS.
[0154] Example 5
[0155] In this embodiment, the composition of the high-conductivity 6101 aluminum alloy material modified by recycled rare earth is as follows: rare earth La 0.1%, iron Fe 0.06%, and the balance is 6101 aluminum alloy. As follows: in 6101 aluminum alloy, magnesium 0.6%, silicon 0.35%, and the balance is Al.
[0156] In this embodiment, the preparation method of Mg-La master alloy comprises the following steps:
[0157] (1) The lanthanum iron silicon alloy waste is sequentially surface cleaned and dried, and then the lanthanum iron silicon bulk alloy is crushed into particles with a diameter of 1 to 3 mm under an inert gas protection environment;
[0158] (2) The magnesium block was melted in a heating furnace under argon protection according to the mass ratio of metallic magnesium to lanthanum iron silicon alloy particles of 0.3, and then the lanthanum iron silicon alloy particles were gradually added to the magnesium melt, kept at 950 ° C and stirred for 35 minutes, and then allowed to stand for 30 minutes;
[0159] (3) The upper layer of magnesium melt containing rare earth elements in the crucible is poured into a water-cooled iron mold for rapid cooling and solidification to obtain a Mg-La intermediate alloy.
[0160] Calculated by mass percentage, the prepared Mg-La master alloy has the following components: 21% rare earth La, 0.01% impurity elements Fe and 0.02% Co, and the balance Mg.
[0161] In this embodiment, the method for preparing a high-conductivity 6101 aluminum alloy material modified by recycled rare earth La comprises the following steps:
[0162] (1) Prepare raw materials according to ingredient requirements;
[0163] (2) Place the aluminum ingot into a melting furnace for melting and adjust the melt temperature to 750°C;
[0164] (3) adding silicon and iron elements to the melt in the form of Al-Si master alloy or Al-Fe master alloy, and stirring the alloy melt to obtain an aluminum alloy melt;
[0165] (4) The alloy melt temperature is lowered to 720°C, and a portion of the magnesium in the aluminum alloy is added in the form of an Al-Mg master alloy;
[0166] (5) heating the melt to 750°C, introducing a refining agent (in terms of mass percentage, the composition of which is 40% sodium cryolite, 46% salt slag for preparing Al5Ti1B master alloy by fluoride salt reaction, 10% aluminum fluoride, 2% calcium fluoride, and 2% potassium feldspar) and introducing argon gas for purification;
[0167] (6) adjusting the temperature of the aluminum alloy melt to 720° C., adding the rare earth element La and the remaining portion of Mg in the form of the Mg-La master alloy prepared above, and stirring the alloy melt and keeping it at a constant temperature to obtain an alloy melt with uniform composition;
[0168] (7) pouring the alloy melt into a mold, cooling it, and obtaining an aluminum alloy ingot after solidification;
[0169] (8) heating the aluminum alloy ingot to 470°C and keeping it at this temperature for 12 h for homogenization treatment;
[0170] (9) heating the homogenized ingot to 530°C and keeping it at that temperature for 4 h to perform a solution quenching treatment on it;
[0171] (10) performing rolling deformation treatment on the ingot after solution quenching treatment;
[0172] (11) The deformed alloy profile is heated to 195°C and kept at this temperature for 12 h for aging treatment to obtain a 6101 aluminum alloy material modified with the secondary rare earth metal La.
[0173] like Figure 5As shown in the figure, the microstructure of the highly conductive 6101 aluminum alloy material modified by recycled rare earth La in this embodiment has a tensile strength of 231 MPa and an electrical conductivity of 59.02% IACS. Compared with Example 4, the appropriate increase in the amount of La added in this embodiment can make the iron-rich phase finer, from needle-shaped to granular, and can also increase the material strength and electrical conductivity at the same time.
[0174] Comparative Example 1
[0175] In this comparative example, the composition of the high-conductivity 6101 aluminum alloy material modified by the original rare earth La is as follows: 0.1% rare earth La, 0.1% iron Fe, and the balance is 6101 aluminum alloy. In terms of mass percentage, the 6101 aluminum alloy contains: 0.6% magnesium, 0.35% silicon, and the balance is Al.
[0176] In this comparative example, the preparation method of 6101 aluminum alloy material comprises the following steps:
[0177] (1) Prepare the raw materials according to the composition requirements of 6101 aluminum alloy;
[0178] (2) placing the aluminum ingot into a melting furnace for melting and adjusting the melt temperature to 750°C;
[0179] (3) adding silicon and iron elements to the melt in the form of Al-Si master alloy and Al-Fe master alloy, and stirring the alloy melt to obtain an aluminum alloy melt;
[0180] (4) lowering the alloy melt temperature to 720°C and adding magnesium in the form of an Al-Mg master alloy;
[0181] (5) heating the melt to 750°C, introducing a refining agent (in terms of mass percentage, the composition of which is 40% sodium cryolite, 46% salt slag for preparing Al5Ti1B master alloy by fluoride salt reaction, 10% aluminum fluoride, 2% calcium fluoride, and 2% potassium feldspar) into the melt and introducing argon gas for purification;
[0182] (6) adjusting the temperature of the aluminum alloy melt to 720° C., adding native rare earth La into the melt in the form of an Al-La master alloy, and stirring the alloy melt and keeping it at a constant temperature to obtain an alloy melt with uniform composition;
[0183] (7) pouring the alloy melt into a mold, cooling it, and obtaining an aluminum alloy ingot after solidification;
[0184] (8) heating the aluminum alloy ingot to 470°C and keeping it at this temperature for 12 h for homogenization treatment;
[0185] (9) heating the homogenized ingot to 530°C and keeping it at that temperature for 4 h to perform a solution quenching treatment;
[0186] (10) performing rolling deformation treatment on the ingot after the solution quenching treatment;
[0187] (11) The deformed alloy profile is heated to 195 °C and kept at this temperature for 12 h for aging treatment to obtain a 6101 aluminum alloy material modified with native rare earth metal La.
[0188] like Figure 6 As shown, the microstructure of the highly conductive 6101 aluminum alloy material modified by the original rare earth La in this comparative example has a tensile strength of 234 MPa and an electrical conductivity of 59.10% IACS. Compared with this comparative example 1, adding the same amount of recycled rare earth La and the original rare earth La respectively has almost the same effect, and the recycled rare earth has lower cost and low carbon and environmental protection than the original rare earth.
[0189] Comparative Example 2
[0190] In this comparative example, the composition of the high-conductivity 6101 aluminum alloy material without any rare earth modification is as follows: 0.1% iron Fe and the balance is 6101 aluminum alloy. As follows: 0.6% magnesium, 0.35% silicon and the balance is Al in the 6101 aluminum alloy.
[0191] In this comparative example, the preparation method of 6101 aluminum alloy material comprises the following steps:
[0192] (1) Prepare the raw materials according to the composition requirements of 6101 aluminum alloy;
[0193] (2) placing the aluminum ingot into a melting furnace for melting and adjusting the melt temperature to 750°C;
[0194] (3) adding silicon and iron elements to the melt in the form of Al-Si master alloy and Al-Fe master alloy, and stirring the alloy melt to obtain an aluminum alloy melt;
[0195] (4) lowering the alloy melt temperature to 720°C and adding magnesium in the form of an Al-Mg master alloy;
[0196] (5) heating the melt to 750°C, introducing a refining agent (in terms of mass percentage, the composition of which is 40% sodium cryolite, 46% salt slag for preparing Al5Ti1B master alloy by fluoride salt reaction, 10% aluminum fluoride, 2% calcium fluoride, and 2% potassium feldspar) into the melt and introducing argon gas for purification;
[0197] (6) adjusting the temperature of the aluminum alloy melt to 720° C., keeping the temperature and allowing the melt to stand, and obtaining an alloy melt having uniform composition;
[0198] (7) pouring the alloy melt into a mold, cooling it, and obtaining an aluminum alloy ingot after solidification;
[0199] (8) heating the aluminum alloy ingot to 470°C and keeping it at this temperature for 12 h for homogenization treatment;
[0200] (9) heating the homogenized ingot to 530°C and keeping it at that temperature for 4 h to perform a solution quenching treatment;
[0201] (10) performing rolling deformation treatment on the ingot after the solution quenching treatment;
[0202] (11) The deformed alloy profile is heated to 195 °C and kept at this temperature for 12 h for aging treatment to obtain a 6101 aluminum alloy material modified with native rare earth metal La.
[0203] like Figure 7 As shown, the microstructure of the high-conductivity 6101 aluminum alloy material without any rare earth modification in this comparative example has a tensile strength of 202 MPa and a conductivity of 57.34% IACS. Comparison of this comparative example 2 with Examples 1-5 and Comparative Example 1 shows that adding an appropriate amount of rare earth elements Sm or La to the 6101 aluminum alloy can increase the number density of the iron-rich phase in the alloy, and the morphology is transformed into a spherical or nearly spherical shape, and the size is significantly refined, so that the mechanical and conductive properties of the material can be improved at the same time.
[0204] The implementation results show that the present invention creatively improves the mechanical properties and electrical conductivity of the alloy by adding rare earth elements Sm and La extracted and recovered from waste samarium cobalt and lanthanum iron silicon magnets to the 6101 aluminum alloy, and the alloy melt is refined and purified before adding rare earth elements, which weakens or avoids the adverse effects of various slag inclusions / inclusions in the alloy melt on rare earths. It not only provides a way to recycle and reuse secondary rare earth metal resources in waste samarium cobalt and lanthanum iron silicon magnets, gives full play to the role of secondary rare earth metals in aluminum alloys, but also provides a method for the production of low-cost, high-quality rare earth aluminum alloy materials. The high-conductivity 6101 aluminum alloy material modified by recycled rare earth of the present invention has higher strength and better electrical conductivity, and its tensile strength is ≥210 MPa and its electrical conductivity is ≥58%IACS.
Claims
1. A high-conductivity 6101 aluminum alloy material modified by recycled rare earth, characterized in that: The aluminum alloy composition includes components by mass percentage: recycled rare earth element Sm or La 0.03-0.3%, iron Fe 0.05-0.1%, and the balance is 6101 aluminum alloy; The added recycled rare earth element Sm or La is respectively derived from the Mg-Sm master alloy or Mg-La master alloy formed by extracting the rare earth element Sm or La from the rare earth magnetic waste using Mg as a collector, and the rare earth magnetic waste is a samarium-cobalt permanent magnet alloy or a lanthanum-iron-silicon alloy; The method of extracting rare earth elements Sm or La from rare earth magnetic waste by using Mg element to prepare Mg-Sm or Mg-La master alloy respectively comprises the following steps: The first step is to sequentially clean, dry and crush the rare earth magnetic waste to obtain rare earth magnetic waste particles with an effective diameter of no more than 5 mm; The second step is to place the rare earth magnetic waste particles in a magnesium melt at a temperature of 750-1050°C under argon protection, keep the temperature and stir for 10-45 minutes, and then let the melt stand for 20-60 minutes; The third step is to pour the upper layer of magnesium melt containing rare earth elements into a mold to cool and solidify to form a Mg-Sm master alloy or a Mg-La master alloy.
2. A method for preparing the recycled rare earth modified high-conductivity 6101 aluminum alloy material according to claim 1, characterized in that: The method comprises the following steps: (1) Prepare alloy raw materials according to the national standard composition requirements of 6101 aluminum alloy; (2) Place the aluminum ingot into a smelting furnace for melting and adjust the melt temperature to 740°C~770°C; (3) adding silicon and iron elements to the melt in the form of Al-Si master alloy and Al-Fe master alloy, and stirring the alloy melt to obtain a 6101 aluminum alloy melt; (4) The alloy melt temperature is lowered to 690°C~720°C, and part of the magnesium content in the 6101 aluminum alloy is added in the form of Al-Mg master alloy; (5) The melt temperature is heated to 740°C to 770°C, and a refining agent and argon gas are introduced into the melt for purification; (6) The temperature of the aluminum alloy melt is adjusted to 690°C to 720°C, rare earth elements Sm or La and the remaining Mg in the 6101 aluminum alloy are added in the form of Mg-Sm master alloy or Mg-La master alloy, and the alloy melt is stirred and kept at a constant temperature to obtain an alloy melt with uniform composition; (7) pouring the alloy melt into a mold, cooling it, and obtaining an aluminum alloy ingot after solidification; (8) heating the aluminum alloy ingot to 460°C~490°C and keeping it at this temperature for 8~16 h for homogenization treatment; (9) heating the homogenized ingot to 510°C to 540°C and keeping it at that temperature for 1 to 6 hours to perform solution quenching; (10) performing rolling deformation treatment on the ingot after solution quenching treatment; (11) The deformed alloy profile is heated to 175°C~210°C and kept at this temperature for 4~18 hours for aging treatment to obtain a recycled rare earth modified high conductive 6101 aluminum alloy material.
3. The method for preparing the recycled rare earth modified high-conductivity 6101 aluminum alloy material according to claim 2, characterized in that: In step (5), the refining agent composition is, by mass percentage, 40% sodium cryolite, 46% salt slag prepared by fluoride salt reaction to prepare Al5Ti1B master alloy, 10% aluminum fluoride, 2% calcium fluoride, and 2% potassium feldspar.
4. The method for preparing the high-conductivity 6101 aluminum alloy material modified by recycled rare earth according to claim 2, characterized in that: In step (6), the rare earth element Sm or La in the rare earth magnetic waste is extracted with the Mg element to prepare the Mg-Sm or Mg-La master alloy respectively, comprising the following steps: The first step is to sequentially clean, dry and crush the rare earth magnetic waste to obtain rare earth magnetic waste particles with an effective diameter of no more than 5 mm; The second step is to place the rare earth magnetic waste particles in a magnesium melt at a temperature of 750-1050°C under argon protection, keep the temperature and stir for 10-45 minutes, and then let the melt stand for 20-60 minutes; The third step is to pour the upper layer of magnesium melt containing rare earth elements into a mold to cool and solidify to form a Mg-Sm master alloy or a Mg-La master alloy.
5. The method for preparing the high-conductivity 6101 aluminum alloy material modified by recycled rare earth according to claim 4, characterized in that: In the first step, the crushing process needs to be carried out in an inert gas protection environment, and the diameter of the rare earth magnetic waste particles is 1~3 mm.
6. The method for preparing the high-conductivity 6101 aluminum alloy material modified by recycled rare earth according to claim 4, characterized in that: In the second step, the mass ratio of magnesium to rare earth magnetic waste is 0.2~0.
8.
7. The method for preparing the high-conductivity 6101 aluminum alloy material modified by recycled rare earth according to claim 4, characterized in that: In the second step, the magnesium melt temperature and the insulation stirring time in the preparation process of the Mg-Sm master alloy or the Mg-La master alloy are 850° C. and 35 min or 950° C. and 25 min, respectively.
8. The method for preparing the high-conductivity 6101 aluminum alloy material modified by recycled rare earth according to claim 4, characterized in that: In the third step, the upper layer of magnesium melt containing rare earth elements is poured into a water-cooled iron mold or copper mold and rapidly cooled to obtain a magnesium-rare earth intermediate alloy with uniform microstructure distribution.
9. The method for preparing the high-conductivity 6101 aluminum alloy material modified by recycled rare earth according to claim 4, characterized in that: In the third step, the content of Sm or La in the prepared Mg-Sm master alloy or Mg-La master alloy is 10% to 40% by mass, and the total content of impurity elements Co and Fe is less than 0.1%.
Citation Information
Patent Citations
A low-cost 63%iacs high-conductivity duralumin wire and its manufacturing method
CN105950893B
Production method of high-conductivity 6101 aluminum alloy board
CN108546850A
A 6101-T63 temper aluminum alloy coil for battery conductors and its preparation method
CN110093536B
Aluminium alloy material applied for new energy automobile fuse and preparation method thereof
CN111850350A
Production process of high-quality 6101 aluminum alloy coiled strip for new energy automobile power supply