Chemical polishing solution and polishing process for 2-series aluminum alloy

By adjusting the proportion of acid and adding dichromate, emulsifier and other ingredients in the aluminum alloy chemical polishing solution, the problem of Cu element dust in the polishing of 2 series aluminum alloys is solved, achieving efficient polishing effect and reducing the risk of corrosion. Applicable to a variety of aluminum alloy series.

CN118756142APending Publication Date: 2024-10-11SICHUAN FANHUA AVIATION INSTR & ELECTRICAL CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202410837541.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing aluminum alloy chemical polishing solutions cannot effectively treat 2-series aluminum alloys, resulting in poor polishing results and possible local corrosion. This is mainly because the Cu element produces dust during the polishing process to prevent the reaction.

Method used

Use a chemical polishing solution including sulfuric acid, phosphoric acid, nitric acid, dichromate, corrosion inhibitor, fog suppressor and emulsifier, by adjusting the proportion of acid and adding ingredients such as dichromate and sodium lauryl sulfate. , reduce the decomposition of nitric acid and the evolution of N0x gas, improve the reaction efficiency, and reduce the viscosity and surface tension through the emulsifier, promote the reaction between dichromate and CuO, and remove hanging ash.

Benefits of technology

It achieves smokeless polishing, improves the glossiness of the surface of 2 series aluminum alloys, reduces the generation of corrosion pits, and is suitable for a variety of aluminum alloy series, significantly improving the polishing effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004913586540000031
    Figure BDA0004913586540000031
Patent Text Reader

Abstract

The invention discloses a chemical polishing solution and a polishing process for a 2-series aluminum alloy. The chemical polishing solution comprises sulfuric acid, phosphoric acid, nitric acid, 3-5g / L of dichromate, 5-10g / L of a corrosion inhibitor, 8-15g / L of a fog inhibitor and 1-3g / L of an emulsifier. The mass ratio of the sulfuric acid to the phosphoric acid to the nitric acid is 3: 7: (1-1.2). Or the chemical polishing solution comprises 5g / L-10g / L of sulfuric acid, phosphoric acid and potassium permanganate, 0.3 g / L-0. 8g / L of nickel sulfate, 0.1 g / L-0. 5g / L of copper sulfate, 0.1 g / L-0. 5g / L of thiourea, 2g / L-5g / L of triethanolamine, 3g / L-5g / L of dichromate, 5g / L-10 g / L of corrosion inhibitor, 8g / L-15g / L of fog inhibitor and 1g / L-3 g / L of emulsifier; the mass ratio of the sulfuric acid to the phosphoric acid is (3-4): 7. According to the invention, by adding the dichromate with a relatively high proportion into the bright dipping liquid, Cu-containing hanging dust generated after the reaction of series 2 aluminum can be completely removed, so that the bright surface is completely exposed on the surface of a workpiece, and the bright dipping liquid has relatively good practicability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of aluminum alloy surface treatment, and in particular relates to a chemical polishing liquid and a polishing process for a 2-series aluminum alloy. Background Art

[0002] Aluminum and aluminum alloys are widely used in the manufacturing industry. In order to enhance their appearance brightness, they are usually chemically polished before anodizing to make their surfaces mirror-bright. The purity of aluminum and aluminum alloys has a great influence on the quality of chemical polishing. Usually, pure aluminum has the highest polishing quality. Aluminum alloys of different purities have different polishing effects according to the elements they contain. Among them, 2 series aluminum (including Cu) is the most difficult to chemically polish.

[0003] Existing chemical polishing liquids are mainly applicable to chemical polishing of other series of aluminum alloys except 2 series aluminum. For example, Chinese patent CN 108950565B discloses an aluminum alloy chemical polishing agent and an aluminum alloy surface polishing method, wherein the aluminum alloy chemical polishing agent is composed of 100g-1500g potassium hydroxide (KOH), 100g-800g polyol and 100L-200L water. The patent clearly indicates that it is applicable to chemical polishing of 7 series aluminum alloy workpieces.

[0004] Chinese patent CN 103361646A discloses a chemical polishing liquid for aluminum and aluminum alloys, which is composed of 450-500 mL / L of phosphoric acid, 100-200 mL / L of sulfuric acid, 1-3 g / L of tartaric acid, 30-60 g / L of brightener, 0.5-1 mL / L of fatty alcohol polyoxyethylene ether, 3-4 g / L of ammonium sulfate, 1-3 g / L of ammonium carbonate, 3-4 g / L of sodium molybdate or ammonium molybdate, and the remainder of water. The patent is applied to chemical polishing of some 6 series and 7 series aluminum alloys.

[0005] Among the aluminum alloy chemical polishing technologies that have been published, there is no effective chemical polishing solution for 2 series aluminum alloys. This is because 2 series aluminum alloys contain Cu elements. During chemical polishing, a layer of ash will be generated on the surface of the aluminum alloy, thereby preventing the polishing solution from contacting the aluminum alloy substrate, causing the reaction to stop and the polishing effect to be poor. In severe cases, it will also cause local corrosion on the aluminum alloy surface. Summary of the invention

[0006] The object of the present invention is to provide a chemical polishing solution and a polishing process for 2 series aluminum alloys, aiming to solve the above-mentioned problems.

[0007] The present invention is mainly achieved through the following technical solutions:

[0008] A chemical polishing liquid for 2 series aluminum alloy comprises sulfuric acid, phosphoric acid, nitric acid, 3-5 g / L of dichromate, 5-10 g / L of corrosion inhibitor, 8-15 g / L of fog suppressant and 1-3 g / L of emulsifier; the mass ratio of sulfuric acid, phosphoric acid and nitric acid is 3:7:1-1.2.

[0009] In order to better realize the present invention, further, the dichromate is potassium dichromate and / or sodium dichromate.

[0010] In order to better realize the present invention, further, the corrosion inhibitor is boric acid, the fog suppressant is ammonium sulfate, and the emulsifier is sodium dodecyl sulfate.

[0011] In order to better realize the present invention, further, it includes 210mL sulfuric acid, 100mL nitric acid, 483mL phosphoric acid, 207mL pure water, 4g dichromate, 8g boric acid, 12g ammonium sulfate, and 2g sodium dodecyl sulfate; the concentrations of the sulfuric acid, phosphoric acid and nitric acid are 98wt%, 85wt% and 68wt%, respectively.

[0012] The present invention is mainly achieved through the following technical solutions:

[0013] A chemical polishing liquid for 2 series aluminum alloys comprises sulfuric acid, phosphoric acid, 5g / L-10g / L potassium permanganate, 0.3g / L-0.8g / L nickel sulfate, 0.1g / L-0.5g / L copper sulfate, 0.1g / L-0.5g / L thiourea, 2g / L-5g / L triethanolamine, 3g / L-5g / L dichromate, 5-10g / L corrosion inhibitor, 8-15g / L fog suppressant and 1-3g / L emulsifier; the mass ratio of sulfuric acid to phosphoric acid is 3-4:7.

[0014] In order to better realize the present invention, it further includes sulfuric acid, phosphoric acid, 10 g / L potassium permanganate, 0.7 g / L nickel sulfate, 0.3 g / L copper sulfate, 0.3 g / L thiourea, 3 g / L triethanolamine and 3 g / L dichromate, 5 g / L corrosion inhibitor, 8 g / L fog suppressant and 1 g / L emulsifier; the mass ratio of sulfuric acid to phosphoric acid is 1:2.

[0015] In order to better realize the present invention, further, the dichromate is potassium dichromate and / or sodium dichromate.

[0016] In order to better realize the present invention, further, the corrosion inhibitor is boric acid, the fog suppressant is ammonium sulfate, and the emulsifier is sodium dodecyl sulfate.

[0017] The present invention is mainly achieved through the following technical solutions:

[0018] A polishing process for a 2-series aluminum alloy, using the above-mentioned chemical polishing solution, comprises the following steps:

[0019] Step S1: preparing a chemical polishing solution: dissolving a corrosion inhibitor, dichromate, a mist suppressant and an emulsifier in hot water, and then sequentially adding nitric acid, sulfuric acid and phosphoric acid, and mixing them evenly;

[0020] Step S2: preparing a polishing liquid, wherein the polishing liquid comprises sulfuric acid and dichromate, wherein the sulfuric acid is 500ml-600ml / L and the dichromate is 10-20g / L;

[0021] Step S3: performing degreasing and oil removal treatment or surface mechanical shot peening treatment on the aluminum alloy workpiece to remove grease on the surface of the aluminum alloy workpiece; then, washing with cold water;

[0022] Step S4: heating the chemical polishing liquid to 100-120° C., and then using the heated chemical polishing liquid to chemically polish the aluminum alloy workpiece for 30-60 seconds; then, washing with cold water;

[0023] Step S5: at room temperature, the aluminum alloy workpiece is polished with a polishing liquid for 30-60 seconds; then, washed with cold water;

[0024] Step S6: Blow dry or dry the surface moisture of the workpiece for later use.

[0025] The beneficial effects of the present invention are as follows:

[0026] (1) The present invention provides a polishing liquid of a tri-acid system, wherein the amount of nitric acid used is reduced, thereby effectively alleviating the generation of yellow smoke; and the present invention can reduce the decomposition of nitric acid and the generation of NO during chemical polishing by adding a mist suppressant to the chemical polishing liquid. x The release of gas can achieve the effect of suppressing acid mist.

[0027] (2) The present invention adds a trace amount of dichromate and sodium dodecyl sulfate to the chemical polishing liquid. In the pickling system, the dichromate can react with the copper in the aluminum alloy. The use of the emulsifier reduces the viscosity of the polishing liquid and increases the efficiency of the polishing reaction. Most of the Cu-containing dust generated during the 2-series aluminum reaction can be removed during chemical polishing. When there is less dust attached to the workpiece, the chemical polishing reaction can continue. The present invention adds a relatively high proportion of dichromate to the polishing liquid, which can completely remove the Cu-containing dust generated after the 2-series aluminum reaction, so that the surface of the workpiece is completely exposed to a bright surface.

[0028] (3) The present invention also provides a smokeless polishing liquid, which removes the nitric acid component and eliminates the generation of yellow smoke. In order to ensure the normal progress of the polishing reaction, potassium permanganate, a strong oxidant, is added, and studies have found that copper ions and nickel ions synergistically promote polishing and improve glossiness; at the same time, copper is preferentially deposited on convex points, while nickel is deposited on concave points, and the coverage area ratio of copper and nickel heavy metals on the surface of the aluminum alloy is increased, thereby greatly reducing the speed at which the polishing liquid dissolves aluminum and effectively reducing the amount of aluminum dissolved in the polishing liquid. Secondly, the present invention also effectively improves the glossiness of polishing by compounding thiourea and triethanolamine.

[0029] (4) Series 2 aluminum contains 4.3-4.8% Cu. During chemical polishing, the ash produced by the reaction, namely CuO, will adhere to the aluminum surface to prevent the reaction from continuing. Since the polishing system contains a large amount of phosphoric acid, a viscous layer is formed on the surface of the workpiece, resulting in the dichromate that can react with CuO being unable to pass through the viscous layer and contact CuO in time. At this time, the surface tension of the viscous layer is reduced by adding an emulsifier, so that the dichromate can pass through the viscous layer and directly react with CuO, converting the precipitated CuO into ionic CuO. 2+ , to achieve the effect of removing dust. The main reaction formula is:

[0030]

[0031] (5) The present invention releases a large amount of heat during chemical polishing, which causes the temperature to rise, accelerating the corrosion rate of the acid solution on the aluminum alloy. In severe cases, corrosion pits will be generated on the surface of the aluminum alloy. At this time, by adding a corrosion inhibitor to the chemical polishing solution, when the temperature rises, the corrosion rate of the acid on the aluminum alloy can be slowed down, reducing the generation of corrosion pits. The present invention can also be applied to the chemical polishing of 1 series, 3 series, 5 series, 6 series, and 7 series aluminum alloys, and has good practicality. DETAILED DESCRIPTION

[0032] Embodiment 1:

[0033] A polishing process for a 2-series aluminum alloy comprises the following steps:

[0034] a. Solution configuration

[0035] (1) Prepare 1L of chemical polishing solution and weigh the components according to the following proportions:

[0036] 231 mL of sulfuric acid, 100 mL of nitric acid, 532 mL of phosphoric acid, 140 mL of purified water, 3 g of dichromate, 5 g of boric acid, 8 g of ammonium sulfate, and 1 g of sodium dodecyl sulfate.

[0037] First, introduce 140 mL of pure water into the stainless steel trough, add 5 g of boric acid into the trough after heating, stir until completely dissolved, then add 3 g of dichromate, 8 g of ammonium sulfate, and 1 g of sodium dodecyl sulfate in turn, stir to dissolve, mix evenly, then add 100 mL of nitric acid, 228 mL of sulfuric acid, and 532 mL of phosphoric acid to the solution in turn and mix evenly.

[0038] (2) Prepare 1L of light emitting liquid and weigh the components according to the following proportions:

[0039] 500mL of sulfuric acid, 500mL of purified water, and 10g of dichromate.

[0040] First, introduce 500 mL of pure water into the plastic tank, add 10 g of dichromate into the tank, stir to dissolve, mix evenly, and then add 500 mL of sulfuric acid into the solution and mix evenly.

[0041] b. Polishing steps

[0042] (1) Prepare polishing liquid and glazing liquid according to the above ratio;

[0043] (2) heating the polishing liquid to 100° C.

[0044] (3) Degreasing and deoiling of 2 series aluminum alloy specimens measuring 100×50×2 mm;

[0045] (4) Wash the 2 series aluminum alloy test piece with water to ensure that there is no grease on the surface of the workpiece;

[0046] (5) Immerse the 2 series aluminum alloy test piece completely in the polishing liquid and take it out after treating for 30 seconds;

[0047] (6) Washing the 2 series aluminum alloy test piece with water;

[0048] (7) Immerse the 2 series aluminum alloy test piece in the above-mentioned polishing liquid and take it out after treating it for 30 seconds;

[0049] (8) Washing the 2 series aluminum alloy test piece with water;

[0050] (9) Blow dry or bake the surface moisture of the test piece.

[0051] As shown in Table 1, the surface glossiness of the obtained 2-series aluminum alloy test piece is 630 Gs, the area of ​​corrosion pits on the surface of the test piece is ≤0.5%, and the weight loss rate is 0.0103.

[0052] Example 2

[0053] A polishing process for a 2-series aluminum alloy comprises the following steps:

[0054] a. Solution configuration

[0055] (1) Prepare 1L of chemical polishing solution and weigh the components according to the following proportions:

[0056] Sulfuric acid 210mL, nitric acid 100mL, phosphoric acid 483mL, purified water 207mL, dichromate 4g, boric acid 8g, ammonium sulfate 12g, sodium dodecyl sulfate 2g.

[0057] First, introduce 207 mL of pure water into the stainless steel trough, add 8 g of boric acid into the trough after heating, stir until completely dissolved, then add 4 g of dichromate, 12 g of ammonium sulfate, and 2 g of sodium dodecyl sulfate in sequence, stir to dissolve, mix evenly, then add 100 mL of nitric acid, 210 mL of sulfuric acid, and 483 mL of phosphoric acid to the solution in sequence and mix evenly.

[0058] (2) Prepare 1L of light emitting liquid and weigh the components according to the following proportions:

[0059] 500mL of sulfuric acid, 500mL of purified water, and 15g of dichromate.

[0060] First, introduce 500 mL of pure water into the plastic tank, add 15 g of dichromate into the tank, stir to dissolve, mix evenly, and then add 500 mL of sulfuric acid into the solution and mix evenly.

[0061] b. Polishing steps

[0062] (1) Prepare polishing liquid and glazing liquid according to the above ratio;

[0063] (2) heating the polishing liquid to 110° C.

[0064] (3) Degreasing and deoiling of 2 series aluminum alloy specimens measuring 100×50×2 mm;

[0065] (4) Wash the 2 series aluminum alloy test piece with water to ensure that there is no grease on the surface of the workpiece;

[0066] (5) Immerse the 2 series aluminum alloy test piece completely in the polishing liquid and take it out after 45 seconds;

[0067] (6) Washing the 2 series aluminum alloy test piece with water;

[0068] (7) Immerse the 2 series aluminum alloy test piece in the above-mentioned polishing liquid and take it out after treating it for 45 seconds;

[0069] (8) Washing the 2 series aluminum alloy test piece with water;

[0070] (9) Blow dry or bake the surface moisture of the test piece.

[0071] As shown in Table 1, the surface glossiness of the obtained 2-series aluminum alloy test piece is 666Gs, the area of ​​corrosion pits on the surface of the test piece is ≤0.3%, and the weight loss rate is 0.0162.

[0072] Example 3

[0073] A polishing process for a 2-series aluminum alloy comprises the following steps:

[0074] a. Solution configuration

[0075] (1) Prepare 1L of chemical polishing solution and weigh the components according to the following proportions:

[0076] 193 mL of sulfuric acid, 100 mL of nitric acid, 443 mL of phosphoric acid, 264 mL of purified water, 5 g of dichromate, 10 g of boric acid, 15 g of ammonium sulfate, and 3 g of sodium dodecyl sulfate.

[0077] First, introduce 264 mL of pure water into the stainless steel trough, add 10 g of boric acid into the trough after heating, stir until completely dissolved, then add 5 g of dichromate, 15 g of ammonium sulfate, and 3 g of sodium dodecyl sulfate in sequence, stir to dissolve, mix evenly, then add 100 mL of nitric acid, 193 mL of sulfuric acid, and 443 mL of phosphoric acid to the solution in sequence and mix evenly.

[0078] (2) Prepare 1L of light emitting liquid and weigh the components according to the following proportions:

[0079] 500mL of sulfuric acid, 500mL of purified water, 20g of dichromate.

[0080] First, introduce 500 mL of pure water into the plastic tank, add 20 g of dichromate into the tank, stir to dissolve, mix evenly, and then add 500 mL of sulfuric acid into the solution and mix evenly.

[0081] b. Polishing steps

[0082] (1) Prepare polishing liquid and glazing liquid according to the above ratio;

[0083] (2) heating the polishing liquid to 120°C;

[0084] (3) Degreasing and deoiling of 2 series aluminum alloy specimens measuring 100×50×2 mm;

[0085] (4) Wash the 2 series aluminum alloy test piece with water to ensure that there is no grease on the surface of the workpiece;

[0086] (5) Immerse the 2 series aluminum alloy test piece completely in the polishing liquid and take it out after treating for 60 seconds;

[0087] (6) Washing the 2 series aluminum alloy test piece with water;

[0088] (7) Immerse the 2 series aluminum alloy test piece in the above-mentioned polishing liquid and take it out after treating it for 60 seconds;

[0089] (8) Washing the 2 series aluminum alloy test piece with water;

[0090] (9) Blow dry or bake the surface moisture of the test piece.

[0091] As shown in Table 1, the surface glossiness of the obtained 2-series aluminum alloy test piece is 647Gs, the area of ​​corrosion pits on the test piece surface is ≤0.8%, and the weight loss rate is 0.0147.

[0092] Embodiment 4:

[0093] A polishing process for a 2-series aluminum alloy comprises the following steps:

[0094] a. Solution configuration

[0095] (1) Prepare 1L of chemical polishing solution and weigh the components according to the following proportions:

[0096] 266mL of sulfuric acid, 534mL of nitric acid, 443mL of phosphoric acid, 200mL of purified water, 10g of potassium permanganate, 0.7g of nickel sulfate, 0.3g of copper sulfate, 0.3g of thiourea, 3g of triethanolamine, 4g of dichromate, 8g of boric acid, 12g of ammonium sulfate, and 2g of sodium dodecyl sulfate.

[0097] First, introduce 264 mL of pure water into the stainless steel trough. After heating, add 10 g of boric acid, 10 g of potassium permanganate, 0.7 g of nickel sulfate, 0.3 g of copper sulfate, 0.3 g of thiourea, and 3 g of triethanolamine into the trough, and stir until completely dissolved. Then, add 5 g of dichromate, 15 g of ammonium sulfate, and 3 g of sodium dodecyl sulfate in turn, stir to dissolve, and after mixing evenly, add 100 mL of nitric acid, 193 mL of sulfuric acid, and 443 mL of phosphoric acid to the solution in turn and mix evenly.

[0098] (2) Prepare 1L of light emitting liquid and weigh the components according to the following proportions:

[0099] 500mL of sulfuric acid, 500mL of purified water, 20g of dichromate.

[0100] First, introduce 500 mL of pure water into the plastic tank, add 20 g of dichromate into the tank, stir to dissolve, mix evenly, and then add 500 mL of sulfuric acid into the solution and mix evenly.

[0101] b. Polishing steps

[0102] (1) Prepare polishing liquid and glazing liquid according to the above ratio;

[0103] (2) heating the polishing liquid to 120° C.

[0104] (3) Degreasing and deoiling of 2 series aluminum alloy specimens measuring 100×50×2 mm;

[0105] (4) Wash the 2 series aluminum alloy test piece with water to ensure that there is no grease on the surface of the workpiece;

[0106] (5) Immerse the 2 series aluminum alloy test piece completely in the polishing liquid and take it out after treating for 60 seconds;

[0107] (6) Washing the 2 series aluminum alloy test piece with water;

[0108] (7) Immerse the 2 series aluminum alloy test piece in the above-mentioned polishing liquid and take it out after treating it for 60 seconds;

[0109] (8) Washing the 2 series aluminum alloy test piece with water;

[0110] (9) Blow dry or bake the surface moisture of the test piece.

[0111] As shown in Table 1, the surface glossiness of the obtained 2-series aluminum alloy test piece is 712Gs, the area of ​​corrosion pits on the test piece surface is ≤0.1%, and the weight loss rate is 0.0135.

[0112] During the polishing process, attention should also be paid to the placement of the workpiece. It is best to place it vertically to facilitate the discharge of bubbles. After polishing, the surface of the 2 series aluminum alloy workpiece can reach mirror finish. If the tank is not used for a long time after polishing, it should be covered to prevent the tank from absorbing water and affecting the polishing effect.

[0113] The present invention effectively solves the technical difficulty that dust on the surface of 2 series aluminum alloy chemical polishing cannot be removed by adding dichromate and emulsifier. The glossiness of the polished test piece reaches above 630Gs, and can reach 735Gs at the highest. The surface corrosion pit area can be controlled below 8 / 1000, and can reach below 1 / 1000 at the highest. The present invention has good practicality.

[0114] Table 2

[0115] Example Glossiness Gs Corrosion pit area Weight loss rate Example 1 630 ≤0.5% 0.0103 Example 2 666 ≤0.3% 0.0162 Example 3 647 ≤0.8% 0.0147 Example 4 712 ≤0.1% 0.0135

[0116] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Any simple modification or equivalent change made to the above embodiment based on the technical essence of the present invention shall fall within the protection scope of the present invention.

Claims

1. A chemical polishing solution for 2 series aluminum alloy, characterized in that: It includes sulfuric acid, phosphoric acid, nitric acid, 3-5 g / L of dichromate, 5-10 g / L of corrosion inhibitor, 8-15 g / L of fog suppressant and 1-3 g / L of emulsifier; the mass ratio of sulfuric acid, phosphoric acid and nitric acid is 3:7:1-1.

2.

2. The chemical polishing liquid for series 2 aluminum alloy according to claim 1, characterized in that: The dichromate is potassium dichromate and / or sodium dichromate.

3. The chemical polishing liquid for 2-series aluminum alloy according to claim 1, characterized in that: The corrosion inhibitor is boric acid, the fog suppressant is ammonium sulfate, and the emulsifier is sodium dodecyl sulfate.

4. A chemical polishing solution for 2-series aluminum alloy according to any one of claims 1 to 3, characterized in that: The invention comprises 210 mL of sulfuric acid, 100 mL of nitric acid, 483 mL of phosphoric acid, 207 mL of purified water, 4 g of dichromate, 8 g of boric acid, 12 g of ammonium sulfate and 2 g of sodium dodecyl sulfate; the concentrations of the sulfuric acid, phosphoric acid and nitric acid are 98 wt%, 85 wt% and 68 wt% respectively.

5. A chemical polishing solution for 2 series aluminum alloy, characterized in that: It includes sulfuric acid, phosphoric acid, potassium permanganate 5g / L-10g / L, nickel sulfate 0.3g / L-0.8g / L, copper sulfate 0.1g / L-0.5g / L, thiourea 0.1g / L-0.5 g / L, triethanolamine 2g / L-5g / L, dichromate 3g / L-5g / L, corrosion inhibitor 5-10g / L, fog suppressant 8-15 g / L and emulsifier 1-3 g / L; the mass ratio of sulfuric acid to phosphoric acid is 3-4:

7.

6. The chemical polishing liquid for 2-series aluminum alloy according to claim 5, characterized in that: It includes sulfuric acid, phosphoric acid, 10 g / L potassium permanganate, 0.7 g / L nickel sulfate, 0.3 g / L copper sulfate, 0.3 g / L thiourea, 3 g / L triethanolamine, 3 g / L dichromate, 5 g / L corrosion inhibitor, 8 g / L fog suppressant and 1 g / L emulsifier; the mass ratio of sulfuric acid to phosphoric acid is 1:

2.

7. The chemical polishing liquid for series 2 aluminum alloy according to claim 5, characterized in that: The dichromate is potassium dichromate and / or sodium dichromate.

8. The chemical polishing liquid for series 2 aluminum alloy according to claim 5, characterized in that: The corrosion inhibitor is boric acid, the fog suppressant is ammonium sulfate, and the emulsifier is sodium dodecyl sulfate.

9. A polishing process for a 2-series aluminum alloy, using the chemical polishing solution according to any one of claims 1 to 8, characterized in that: The following steps are involved: Step S1: preparing a chemical polishing solution: dissolving a corrosion inhibitor, dichromate, a mist suppressant and an emulsifier in hot water, and then sequentially adding nitric acid, sulfuric acid and phosphoric acid, and mixing them evenly; Step S2: preparing a polishing liquid, wherein the polishing liquid comprises sulfuric acid and dichromate, wherein the sulfuric acid is 500ml-600ml / L and the dichromate is 10-20g / L; Step S3: performing degreasing and oil removal treatment or surface mechanical shot peening treatment on the aluminum alloy workpiece to remove grease on the surface of the aluminum alloy workpiece; then, washing with cold water; Step S4: heating the chemical polishing liquid to 100-120° C., and then using the heated chemical polishing liquid to chemically polish the aluminum alloy workpiece for 30-60 seconds; then, washing with cold water; Step S5: at room temperature, the aluminum alloy workpiece is polished with a polishing liquid for 30-60 seconds; then, washed with cold water; Step S6: Blow dry or dry the surface moisture of the workpiece for later use.

Citation Information

Patent Citations

  • Chemical polishing solution for aluminum and aluminum alloy

    CN103361646A

  • Chemical polishing agents for aluminum alloys and methods for polishing aluminum alloy surfaces

    CN108950565B

  • Aluminum alloy polishing process

    CN103668212A

  • Aluminum product chemical polishing solution and preparing method thereof

    CN108505044A

  • Environment-friendly aluminum alloy chemical polishing solution as well as preparation method and polishing method thereof

    CN111996533A