Preparation method of p-type nitride ohmic electrode and power electronic device
The oxygen plasma oxidation method is used to form a uniform nickel oxide layer at a lower temperature, which solves the problems of poor uniformity of the nickel oxide layer and insufficient Au-based contact thermal stability in the preparation of p-type nitride ohmic electrodes, and achieves high-quality p-type ohmic electrodes. Preparation of nitride ohmic electrodes, suitable for large-area and industrial production.
Patent Information
- Application Number
- CN202410972683.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-10-11
AI Technical Summary
It is difficult to prepare high-quality p-type nitride ohmic electrodes with the existing technology, especially due to the poor uniformity of the nickel oxide layer and the insufficient thermal stability of the Au-based contact, resulting in high contact resistivity, making it difficult to meet the requirements for large-area preparation and industrialization at high temperatures. production requirements.
The oxygen plasma oxidation method is used to form a uniform nickel oxide layer at a lower temperature, and the physical vapor deposition method and electron beam evaporation and other technologies are combined to prepare a metallic nickel layer and a nickel oxide layer on the p-type nitride to form a high-quality p-type nitride. Type nitride ohmic electrode.
It achieves lower contact resistivity and better performance stability, is suitable for large-area preparation and industrial production, and avoids the increase in equipment complexity and cost caused by high-temperature annealing.
Smart Images

Figure CN118762987A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to the technical field of semiconductor device manufacturing, and in particular to a preparation method of a p-type nitride ohmic electrode and a power electronic device. Background Art
[0002] As one of the representatives of the third-generation semiconductor materials, III-V nitrides have the advantages of large bandwidth, high thermal conductivity, high electron mobility, high electron saturation velocity, and high breakdown electric field. In new application scenarios such as high temperature, high power, high frequency, and high radiation, they exhibit excellent performance far exceeding that of silicon-based and other similar devices. They have broad application prospects and an enormous market that cannot be estimated in the future.
[0003] Compared with the excellent performance of n-type devices, how to improve the performance of p-type devices has always been a hot topic of research. One of the important issues is how to form a good low-resistance ohmic contact of p-type nitride and prepare an ohmic electrode with excellent performance. The ohmic contact of n-type nitride is relatively easy to prepare. Usually, a combination of Ti / Al / Ti / Au is used, and the contact resistivity is generally 10 -5 ~ 10 -6 Ω·cm 2 The ohmic contact of p-type nitride is difficult to prepare. On the one hand, it is more difficult to prepare effectively heavily doped p-type nitride materials, and the effective hole concentration is always low. On the other hand, the work function of p-type nitride is very large. For example, the work function of p-GaN is about 7.5 eV. There is a lack of ohmic contact metal materials with matching work functions (the work function of metal materials is greater than 7.5 eV). The metal Pt with the largest work function is only 5.56 eV.
[0004] At present, the ohmic electrode of p-type nitride is prepared by using Ni / Au combination, and a lower contact resistivity is achieved. The main mechanism for reducing the contact resistivity is that the metal Ni is oxidized to nickel oxide and contacts with the p-type nitride to form an ohmic contact. However, the existing preparation methods all form a nickel oxide layer by rapid thermal annealing (RTA) in air or oxygen, which results in poor uniformity of the formed nickel oxide, thereby causing the formed ohmic contact to be unstable. At the same time, the thermal stability of Au-based contacts is usually poor, the thermal budget is low, and the contact quality will degrade at high temperatures. Therefore, the traditional rapid thermal annealing method does not meet the requirements for preparing high-quality p-type nitride ohmic electrodes, and the complex and high-cost annealing method is not suitable for preparation on large-area wafers and large-scale industrial production. Summary of the invention
[0005] In view of this, the present disclosure provides a method for preparing a p-type nitride ohmic electrode and a power electronic device, which are used to at least partially solve the above technical problems.
[0006] A first aspect of an embodiment of the present disclosure provides a method for preparing a p-type nitride ohmic electrode, comprising: preparing a p-type nitride on an epitaxial structure of a p-type device; preparing a metal nickel layer on the p-type nitride, and subjecting the metal nickel layer to oxygen plasma oxidation to react and form a nickel oxide layer; and preparing a metal layer on the nickel oxide layer to obtain a p-type nitride ohmic electrode.
[0007] According to an embodiment of the present disclosure, a p-type nitride is prepared on an epitaxial structure of a p-type device, including: depositing the p-type nitride on the epitaxial structure using a physical vapor deposition method, a chemical vapor deposition method, or a sputtering method; wherein the p-type nitride includes a p-type doped III-V group nitride.
[0008] According to an embodiment of the present disclosure, the p-type doped III-V group nitride includes p-type InN, p-type GaN, p-type AlN, p-type InGaN, p-type AlGaN, p-type InAlN or p-type AlGaInN.
[0009] According to an embodiment of the present disclosure, a metal nickel layer is prepared on a p-type nitride, including forming a photoresist on the p-type nitride, and photolithographically carving out an area to form an ohmic electrode based on the photoresist; depositing metal nickel by electron beam evaporation, sputtering or deposition, and stripping off the remaining photoresist and the metal nickel outside the area of the ohmic electrode to form a metal nickel layer.
[0010] According to an embodiment of the present disclosure, oxygen plasma oxidation is performed on the metal nickel layer, including: forming a photoresist on the metal nickel layer and the exposed p-type nitride; overlaying is performed on the area based on the photoresist and the ohmic electrode to expose the metal nickel layer; and oxygen plasma oxidation is performed on the metal nickel layer using pure oxygen plasma to remove the photoresist.
[0011] According to an embodiment of the present disclosure, a metal layer is prepared on a nickel oxide layer, including: forming a photoresist on the nickel oxide layer and the exposed p-type nitride; overlaying the photoresist and ohmic electrode areas to expose the nickel oxide layer; depositing metal on the nickel oxide layer by magnetron sputtering, physical vapor deposition or metal evaporation; and stripping off the remaining photoresist and the metal in the area outside the nickel oxide layer to form a metal layer.
[0012] According to an embodiment of the present disclosure, the preparation temperature of the p-type nitride ohmic electrode is 0-200° C. According to an embodiment of the present disclosure, the material of the metal layer includes at least one of Au, AuSn, Pt, and Al, and the metal layer is a single layer or a multilayer.
[0013] According to an embodiment of the present disclosure, the thickness of the metal nickel layer is 1 nm to 20 nm.
[0014] A second aspect of the embodiments of the present disclosure provides a power electronic device, including: an epitaxial structure; a p-type nitride ohmic electrode formed on the epitaxial structure, wherein the p-type nitride ohmic electrode is prepared by the above-mentioned preparation method.
[0015] The method for preparing the p-type nitride ohmic electrode and the power electronic device according to the embodiments of the present disclosure have at least the following beneficial effects:
[0016] Oxidation of the metal nickel layer by oxygen plasma oxidation can form a nickel oxide layer with better uniformity, making the contact resistivity of the p-type nitride ohmic electrode lower and the performance better. In addition, the properties of the oxide layer formed by oxygen plasma oxidation in different areas of the same wafer or between different wafers in the same batch are basically the same, which is suitable for simultaneous preparation on large-area wafers.
[0017] Compared with the traditional method of forming ohmic contact by rapid thermal annealing at high temperature for a period of time, the method of using oxygen plasma to oxidize Ni can complete the preparation of high-quality p-type nitride ohmic electrodes at a lower temperature below 200°C, avoiding large-area heating and cooling equipment, greatly reducing the complexity of the process, reducing production costs, and improving process stability, making it suitable for large-scale industrial production.
[0018] Oxygen plasma oxidation is used to oxidize the metal nickel layer, so that the entire preparation process can be carried out at a lower temperature, avoiding the problems of low thermal budget and poor thermal stability of Au-based contacts in the preparation of p-type nitride ohmic electrodes, and is more conducive to the formation of a good ohmic electrode. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] The above and other objects, features and advantages of the present disclosure will become more apparent through the following description of the embodiments of the present disclosure with reference to the accompanying drawings, in which:
[0020] Figure 1 A flow chart schematically shows a method for preparing a p-type nitride ohmic electrode according to an embodiment of the present disclosure;
[0021] Figure 2 The structure of a p-type nitride ohmic electrode according to an embodiment of the present disclosure is schematically shown;
[0022] Figure 3 The structural diagram corresponding to each step in the preparation method according to an embodiment of the present disclosure is schematically shown. DETAILED DESCRIPTION
[0023] Hereinafter, embodiments of the present disclosure will be described with reference to the accompanying drawings. However, it should be understood that these descriptions are exemplary only and are not intended to limit the scope of the present disclosure. In the following detailed description, for ease of explanation, many specific details are set forth to provide a comprehensive understanding of the embodiments of the present disclosure. However, it is apparent that one or more embodiments may also be implemented without these specific details. In addition, in the following description, descriptions of known structures and technologies are omitted to avoid unnecessary confusion of the concepts of the present disclosure.
[0024] The terms used herein are only for describing specific embodiments and are not intended to limit the present disclosure. The terms "comprise", "include", etc. used herein indicate the existence of the features, steps, operations and / or components, but do not exclude the existence or addition of one or more other features, steps, operations or components.
[0025] All terms (including technical and scientific terms) used herein have the meanings commonly understood by those skilled in the art unless otherwise defined. It should be noted that the terms used herein should be interpreted as having a meaning consistent with the context of this specification and should not be interpreted in an idealized or overly rigid manner.
[0026] When using expressions such as "at least one of A, B, and C, etc.", they should generally be interpreted according to the meaning of the expression commonly understood by those skilled in the art (for example, "a system having at least one of A, B, and C" should include but is not limited to a system having A alone, B alone, C alone, A and B, A and C, B and C, and / or A, B, C, etc.).
[0027] In view of the shortcomings of the prior art, the embodiments of the present disclosure provide a method for preparing a p-type nitride ohmic electrode, which uses oxygen plasma oxidation to prepare a nickel oxide layer, which can better improve the uniformity of nickel oxide, and the operation at a lower temperature also avoids the problem of low thermal budget. The following is a detailed description in conjunction with specific embodiments.
[0028] Figure 1 The flowchart of the method for preparing a p-type nitride ohmic electrode according to an embodiment of the present disclosure is schematically shown. Figure 2 The structure of a p-type nitride ohmic electrode according to an embodiment of the present disclosure is schematically shown.
[0029] like Figure 1 and Figure 2 As shown, the method for preparing a p-type nitride ohmic electrode may include operations S110 to S130.
[0030] In operation S110 , a p-type nitride is prepared on the epitaxial structure of the p-type device.
[0031] In operation S120, a metal nickel layer is formed on the p-type nitride, and the metal nickel layer is oxidized by oxygen plasma to react the metal nickel layer to form a nickel oxide layer.
[0032] In operation S130, a metal layer is formed on the nickel oxide layer to obtain a p-type nitride ohmic electrode.
[0033] That is, the p-type nitride ohmic electrode includes p-type nitride, a nickel oxide layer and a metal layer, and forms an ohmic contact with the epitaxial structure.
[0034] Based on the above embodiment, operation S110 may further include:
[0035] The p-type nitride is selectively deposited on an appropriate area of the epitaxial structure by using a physical vapor deposition method, a chemical vapor deposition method or a sputtering method, wherein the p-type nitride includes a p-type doped III-V group nitride.
[0036] For example, the p-type doped Group III-V nitride may include p-type InN, p-type GaN, p-type AlN, p-type InGaN, p-type AlGaN, p-type InAlN, p-type AlGaInN, or the like.
[0037] Based on the above embodiment, the step of preparing a metal nickel layer on the p-type nitride in operation S120 may further include:
[0038] A photoresist is formed on the p-type nitride, and a region where an ohmic electrode is to be formed is photolithographically formed based on the photoresist.
[0039] The metal nickel is deposited by electron beam evaporation, sputtering or deposition, and the metal nickel outside the area of the remaining photoresist and the ohmic electrode is stripped off to form a metal nickel layer.
[0040] Based on the above embodiment, the metal nickel layer is subjected to oxygen plasma oxidation in operation S120, including:
[0041] A photoresist is formed on the metallic nickel layer and the exposed p-type nitride.
[0042] Overlay is performed on the photoresist and ohmic electrode regions to expose the metal nickel layer.
[0043] The metal nickel layer is oxidized by pure oxygen plasma to remove the photoresist.
[0044] Furthermore, the thickness of the metal nickel layer can be 1 nm to 20 nm.
[0045] Based on the above embodiment, in operation S130, a metal layer is prepared on the nickel oxide layer, including:
[0046] A photoresist is formed on the nickel oxide layer and the exposed p-type nitride.
[0047] Overlay is performed on the photoresist and ohmic electrode regions to expose the nickel oxide layer.
[0048] The metal is deposited on the nickel oxide layer by magnetron sputtering, physical vapor deposition or metal evaporation.
[0049] The remaining photoresist and the metal in the area outside the nickel oxide layer are removed by stripping to form a metal layer.
[0050] Furthermore, the material of the metal layer includes at least one of Au, AuSn, Pt, and Al, and the metal layer is a single layer or multiple layers.
[0051] Based on the above embodiment, the preparation temperature range of the p-type nitride ohmic electrode can be 0-200°C.
[0052] It should be noted that Figure 2 The p-type nitride ohmic electrode structure shown is only used as an example to assist in introducing the preparation method of p-type nitride ohmic electrode by oxygen plasma oxidation of Ni, rather than limiting the application scenario of the present invention, and the introduction of the epitaxial structure under the p-type nitride ohmic electrode is omitted.
[0053] In order to more clearly describe the method for preparing the p-type nitride ohmic electrode provided by the embodiment of the present disclosure, a specific example is given below for illustration.
[0054] Figure 3 The structural diagram corresponding to each step in the preparation method according to an embodiment of the present disclosure is schematically shown.
[0055] like Figure 3 As shown, the preparation method is as follows:
[0056] In the first step, a p-type nitride layer is selectively grown in appropriate areas on the epitaxial structure by physical vapor deposition.
[0057] The second step is to photolithography the location of the ohmic electrode on the surface of the p-type nitride;
[0058] The third step is to plate Ni using electron beam evaporation;
[0059] The fourth step is to use appropriate conditions to perform stripping to remove the photoresist and metal Ni outside the ohmic electrode area. At this time, there is a metal Ni layer in the ohmic electrode area;
[0060] Step 5: Photolithography the position of the ohmic electrode again. The alignment should be accurate to ensure that it is absolutely overlaid with the previous ohmic electrode position. The purpose of this step is to protect the p-type nitride area outside the ohmic electrode area.
[0061] The sixth step is to perform oxygen plasma oxidation to react the metal Ni to form nickel oxide;
[0062] Step 7: Use appropriate conditions to wash the photoresist to remove the photoresist in the previous step. At this time, there is a nickel oxide layer in the ohmic electrode area.
[0063] Step 8: Photolithography the position of the ohmic electrode again. The alignment should be accurate to ensure that it is absolutely overlaid with the previous ohmic electrode position. The purpose of this step is to facilitate the subsequent stripping process.
[0064] Step 9: depositing an Au metal layer;
[0065] Finally, stripping is performed under appropriate conditions to remove the photoresist and Au metal outside the ohmic electrode area. At this time, the ohmic electrode area is, from bottom to top, p-type nitride, nickel oxide layer, and Au metal layer.
[0066] In this example, the photoresist and photolithography machine used in the photolithography process and the light source for exposure can be selected according to the required accuracy or existing equipment, and conditions such as the exposure time and exposure dose of the photolithography can be appropriately selected.
[0067] In this example, under high vacuum conditions, a thin layer of metal Ni is formed on the p-type nitride layer by electron beam evaporation of nickel; the thickness of the metal Ni layer is controlled by controlling the reaction time, and the thickness of the formed metal Ni layer is 1nm ~ 20nm.
[0068] In this example, pure oxygen is 99.9% or more pure oxygen.
[0069] In this example, the conditions for the stripping process are, in sequence, blue film adhesion, acetone soaking, ethanol soaking and deionized water soaking. The reaction time can also be controlled or other conditions can be selected for stripping according to the different photoresists used. The conditions for washing the glue are, in sequence, acetone soaking, ethanol soaking and film remover soaking. The reaction time can also be controlled or other conditions can be selected according to the different photoresists used and the thickness of the glue.
[0070] Based on the above-mentioned method for preparing the p-type nitride ohmic electrode, an embodiment of the present disclosure further provides a power electronic device, comprising:
[0071] epitaxial structure;
[0072] A p-type nitride ohmic electrode is formed on the epitaxial structure.
[0073] The p-type nitride ohmic electrode is prepared by the above-mentioned preparation method, which will not be described in detail here.
[0074] Power electronic devices can include a variety of power electronic devices such as p-type MOSFET, p-type HEMT, p-type HFET, IGBT and BJT.
[0075] According to the embodiments of the present disclosure, since the p-type nitride ohmic electrode prepared by the above method has lower contact resistivity and better performance, the performance of the power electronic device can be improved.
[0076] It will be appreciated by those skilled in the art that the features described in the various embodiments of the present disclosure may be combined and / or combined in a variety of ways, even if such combinations or combinations are not explicitly described in the present disclosure. In particular, without departing from the spirit and teachings of the present disclosure, the features described in the various embodiments of the present disclosure may be combined and / or combined in a variety of ways. All of these combinations and / or combinations fall within the scope of the present disclosure.
[0077] The embodiments of the present disclosure are described above. However, these embodiments are only for illustrative purposes and are not intended to limit the scope of the present disclosure. Although the embodiments are described above, this does not mean that the measures in the various embodiments cannot be used in combination to advantage. Without departing from the scope of the present disclosure, those skilled in the art may make a variety of substitutions and modifications, which should all fall within the scope of the present disclosure.
Claims
1. A method for preparing a p-type nitride ohmic electrode, characterized in that: include: preparing a p-type nitride on the epitaxial structure of a p-type device; Preparing a metal nickel layer on the p-type nitride, and subjecting the metal nickel layer to oxygen plasma oxidation to allow the metal nickel layer to react to form a nickel oxide layer; A metal layer is prepared on the nickel oxide layer to obtain a p-type nitride ohmic electrode.
2. The preparation method according to claim 1, characterized in that: The method of preparing a p-type nitride on the epitaxial structure of a p-type device comprises: The p-type nitride is deposited on the epitaxial structure by physical vapor deposition, chemical vapor deposition or sputtering; wherein the p-type nitride comprises a p-type doped III-V group nitride.
3. The preparation method according to claim 2, characterized in that: The p-type doped III-V group nitride includes p-type InN, p-type GaN, p-type AlN, p-type InGaN, p-type AlGaN, p-type InAlN or p-type AlGaInN.
4. The preparation method according to claim 1, characterized in that: The step of preparing a metal nickel layer on the p-type nitride comprises: forming a photoresist on the p-type nitride, and photolithographically forming a region for forming an ohmic electrode based on the photoresist; The metal nickel is deposited by electron beam evaporation, sputtering or deposition, and the metal nickel outside the region of the remaining photoresist and the ohmic electrode is stripped off to form the metal nickel layer.
5. The preparation method according to claim 4, characterized in that: The step of subjecting the metal nickel layer to oxygen plasma oxidation comprises: forming a photoresist on the metal nickel layer and the exposed p-type nitride; Overlaying is performed based on the photoresist and the ohmic electrode area to expose the metal nickel layer; The metal nickel layer is oxidized by pure oxygen plasma to remove the photoresist.
6. The preparation method according to claim 5, characterized in that: The step of preparing a metal layer on the nickel oxide layer comprises: forming a photoresist on the nickel oxide layer and the exposed p-type nitride; Overlaying is performed based on the photoresist and the ohmic electrode region to expose the nickel oxide layer; Depositing metal on the nickel oxide layer by magnetron sputtering, physical vapor deposition or metal evaporation; The remaining photoresist and the metal in the area outside the nickel oxide layer are removed by stripping to form the metal layer.
7. The preparation method according to claim 1, characterized in that: The preparation temperature of the p-type nitride ohmic electrode is 0-200°C.
8. The preparation method according to claim 1 or 6, characterized in that: The material of the metal layer includes at least one of Au, AuSn, Pt and Al, and the metal layer is a single layer or multiple layers.
9. The preparation method according to claim 1 or 4, characterized in that: The thickness of the metal nickel layer is 1 nm to 20 nm.
10. A power electronic device, characterized in that: include: epitaxial structure; A p-type nitride ohmic electrode is formed on the epitaxial structure, and the p-type nitride ohmic electrode is prepared by the preparation method according to any one of claims 1-9.