Dry-process electrode sheet based on spraying enhancement, and processing method and equipment thereof

Through the spray-strengthening dry electrode sheet processing method, the lateral tensile strength of the electrode sheet is improved, and the problem of loss and cracking of the electrode sheet during the calendering and winding process is solved, achieving higher production yield and process efficiency .

CN118763183BActive Publication Date: 2024-11-15GAC AION NEW ENERGY AUTOMOBILE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411205713.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-15
Estimated Expiration
2044-08-30

AI Technical Summary

Technical Problem

The tensile strength of the dry electrode sheet in the transverse direction is low, resulting in easy cracking during calendering or winding.

Method used

The dry electrode sheet processing method of spray-strengthening is adopted. By uniformly dispersing and fibrosis of the material, an intermediate film body is formed, and spraying is carried out in the transverse direction to form a cured layer to enhance the tensile strength of the intermediate film body. The specific steps include mixing and dispersing the materials evenly, performing fibrosis treatment, forming an intermediate film body, spraying along the width direction of the intermediate film body, curing to form a cured layer, and finally pressing it with the current collector to form a dry electrode sheet. The spray width and speed of the spray treatment are between 2mm and 5mm, between 0.1m/s and 0.3m/s. The resin system oligomer, diluent, solid electrolyte and initiator are used, and cured by ultraviolet light or heating.

Benefits of technology

The tensile strength of the dry electrode sheet in the lateral direction is effectively improved, the cracking problem during the calendering and winding process is avoided, the production yield is improved, and the process time is optimized.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118763183B_ABST
    Figure CN118763183B_ABST
Patent Text Reader

Abstract

The present application discloses a dry electrode plate based on spraying enhancement, and a processing method and equipment thereof. The processing method comprises the following steps: mixing and uniformly dispersing the materials; subjecting the uniformly dispersed materials to fiberization; placing the fiberized materials into a film-forming device to form an intermediate film body; subjecting the intermediate film body to spraying treatment to form a plurality of spraying stripes, and the direction of the spraying treatment is to extend along the width direction of the intermediate film body; curing the spraying stripes to form a solidified layer; continuing to process the intermediate film body with the solidified layer in the film-forming device to form a self-supporting film; and pressing the self-supporting film with the current collector to obtain a dry electrode plate. By forming a plurality of spraying stripes on the surface of the intermediate film body and curing them, it can effectively improve the tensile strength of the self-supporting film in the lateral direction.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of lithium-ion battery manufacturing, and in particular to a dry-process electrode plate based on spraying enhancement, and a processing method and equipment thereof. Background Art

[0002] Lithium-ion batteries have the advantages of high energy density and long cycle life, and are widely used in new energy power and energy storage equipment.

[0003] At present, dry electrodes are a new technical direction for the development of lithium-ion batteries. The characteristic of dry electrodes is that the active material, binder and conductive agent are evenly mixed through a drying process under solvent-free conditions, and then pressed into electrodes of the desired shape. Dry electrodes have the advantages of low cost, uniform distribution of electrode components, and easy control of electrode thickness. Dry electrode pole pieces generally include a current collector and a self-supporting film disposed on the current collector. Since the self-supporting film is generally made by uniaxial stretching, the prepared self-supporting film has a good tensile strength in the longitudinal direction, that is, the machine direction (Machine Direction, MD), and a low tensile strength in the transverse direction (Transverse Direction, TD), which makes the self-supporting film prone to damage and cracking during calendering or winding. Summary of the invention

[0004] The main purpose of the present application is to provide a dry electrode plate based on spraying reinforcement, and its processing method and equipment, so as to solve the problem of low tensile strength of dry electrode plates in the lateral direction in the prior art.

[0005] One embodiment of the present application provides a dry electrode plate processing method based on spraying enhancement, comprising the following steps:

[0006] Mix the materials and disperse them evenly;

[0007] The uniformly dispersed material is subjected to fiberization treatment;

[0008] Putting the fiberized material into a film forming device to form an intermediate film body, wherein the intermediate film body has a first direction and a second direction, wherein the first direction extends along the length direction of the intermediate film body, and the second direction extends along the width direction of the intermediate film body;

[0009] Performing a spraying treatment on the intermediate film body to form a plurality of spraying stripes, wherein the spraying treatment direction extends along the second direction of the intermediate film body;

[0010] Curing the sprayed stripes to form a cured layer;

[0011] The intermediate film body having the solidified layer is further processed in the film forming device to form a self-supporting film;

[0012] The self-supporting film is pressed together with the current collector to obtain a dry electrode plate.

[0013] In one of the embodiments, the spraying width of the spraying process ranges from 2 mm to 5 mm, and the spraying speed of the spraying process ranges from 0.1 m / s to 0.3 m / s.

[0014] In one embodiment, during the spraying process, the spraying material includes a resin system oligomer, a diluent, a solid electrolyte and an initiator, and the contents thereof in the spraying material are calculated by mass percentage as follows:

[0015] Resin system oligomer, content is 62%-65%;

[0016] Diluent, content is 18%-20%;

[0017] Solid electrolyte, content of 13.5%-14.5%;

[0018] Initiator, content is 2.5%.

[0019] In one embodiment, the resin system oligomer includes polyurethane acrylate, epoxy acrylate or polyester acrylate, the diluent includes acrylic multifunctional monomer, the initiator includes acylphosphine oxide, and the solid electrolyte includes lithium lanthanum zirconium oxide, lithium titanium aluminum phosphate or aluminum oxide.

[0020] In one of the embodiments, during the process of curing the sprayed stripes, ultraviolet light is used to cure the sprayed material to form the cured layer.

[0021] In one embodiment, during the spraying process, the spraying material includes a resin, a curing agent and a solid electrolyte, and the contents thereof in the spraying material are respectively as follows, calculated by mass percentage:

[0022] Resin, content is 44%-46%;

[0023] Curing agent, content is 44%-46%;

[0024] Solid electrolyte, content is 10%.

[0025] In one embodiment, the resin includes phenolic resin, epoxy resin, acrylic resin or polyester resin, the curing agent includes amine curing agent and acid anhydride curing agent, and the solid electrolyte includes lithium lanthanum zirconium oxide, lithium aluminum titanium phosphate or aluminum oxide.

[0026] In one embodiment, during the process of mixing and evenly dispersing the material, the spray material used for the spraying process is added to the material and mixed and evenly dispersed together, and the mass percentage content of the spray material is 0.5%-1%; during the curing process, the spray material added to the material is cured together with the spray stripes.

[0027] Another embodiment of the present application provides a dry electrode plate processing device based on spraying enhancement, comprising:

[0028] Mixing equipment, used to mix and evenly disperse materials;

[0029] Material fiberizing equipment, used for fiberizing the uniformly dispersed material;

[0030] A pre-filming device, used for filming the fiberized material to form an intermediate film body, wherein the intermediate film body has a first direction and a second direction, wherein the first direction extends along the length direction of the intermediate film body, and the second direction extends along the width direction of the intermediate film body;

[0031] A spraying device, used for spraying the intermediate film body to form a plurality of spraying stripes, wherein the spraying direction is extending along the second direction of the intermediate film body;

[0032] A curing device for curing the sprayed stripes to form a cured layer;

[0033] A film forming device, used for processing the intermediate film body having the solidified layer to form a self-supporting film;

[0034] The composite processing equipment is used to press the self-supporting film and the current collector to obtain a dry electrode plate.

[0035] Another embodiment of the present application provides a dry electrode plate based on spraying enhancement, and the dry electrode plate is manufactured by the dry electrode plate processing method as described in any of the above embodiments.

[0036] In one embodiment, the dry electrode plate comprises:

[0037] a current collector; and

[0038] A self-supporting film is arranged on the surface of the current collector, and a solidified layer is arranged on the surface of the self-supporting film, and the solidified layer includes a plurality of spray-cured stripes, and the spray-cured stripes extend in the lateral direction of the self-supporting film;

[0039] The width of the spray-cured stripes ranges from 2 mm to 5 mm;

[0040] The thickness of the spray-cured stripes ranges from 10 μm to 1 mm.

[0041] The dry electrode sheet processing method, equipment and dry electrode sheet based on spraying enhancement of the present application have the following advantages and beneficial effects:

[0042] 1. In the dry electrode plate processing method provided in the present application, the intermediate film body is sprayed to form a plurality of spray stripes, and the direction of the spraying treatment is to extend along the second direction of the intermediate film body. In the subsequent processing, the spray stripes can be cured to form a solidified layer. At this time, the solidified layer extending laterally along the intermediate film body can play a role in improving the tensile strength of the intermediate film body in the second direction, thereby further improving the tensile strength of the subsequently manufactured dry electrode plate in the second direction. The above spraying and curing treatment methods can effectively avoid the problem of damage and cracking of the dry electrode plate during the calendering and winding process, and improve the production yield of the dry electrode plate.

[0043] 2. In one embodiment, the spraying width range of the spraying treatment is set to between 2 mm and 5 mm, and the spraying speed range of the spraying treatment is set to between 0.1 m / s and 0.3 m / s, which can effectively ensure that the formed solidified layer can improve the tensile strength of the second direction of the intermediate film body. In fact, the faster the speed of the spraying treatment, the less the spraying material attached to the intermediate film body, and the worse the effect of improving the tensile strength of the intermediate film body in the second direction after the spraying material is cured; the slower the speed of the spraying treatment, the more the spraying material attached to the intermediate film body, and the better the effect of improving the tensile strength of the intermediate film body in the second direction after the spraying material is cured. However, the slower the spraying speed, the longer the process time. Under comprehensive consideration, the spraying speed range is generally set to between 0.1 m / s and 0.3 m / s. In this way, the tensile strength of the second direction of the prepared dry electrode pole piece can be improved without having too much impact on the process time. The narrower the spraying width, the less the spraying material adheres to the intermediate film body, and after the spraying material is solidified, the worse the effect of improving the tensile strength of the intermediate film body in the second direction is; the wider the spraying width, the more the spraying material adheres to the intermediate film body, and after the spraying material is solidified, the better the effect of improving the tensile strength of the intermediate film body in the second direction is. Therefore, the spraying width is selected to be more than 2 mm as much as possible to achieve the effect of improving the tensile strength of the intermediate film body in the second direction.

[0044] 3. In one embodiment, the spraying material includes a resin system oligomer, a diluent, a solid electrolyte and an initiator, and the contents of each component in the spraying material are calculated by mass percentage as follows: resin system oligomer, content is 62%-65%; diluent, content is 18%-20%; solid electrolyte, content is 13.5%-14.5%; initiator, content is 2.5%. By setting the above spraying material, in the subsequent curing process, the spraying material can be cured by ultraviolet light curing. Specifically, the initiator in the spraying material decomposes into free radicals after being irradiated with ultraviolet light, thereby initiating polymer cross-linking and curing, thereby forming a cured layer on the intermediate film body. The cured layer extending laterally along the intermediate film body can play a role in improving the tensile strength of the intermediate film body in the second direction, thereby improving the tensile strength of the subsequently manufactured dry electrode pole piece in the second direction. Specifically, in one embodiment, the initiator includes acylphosphine oxide, which is excited after absorbing ultraviolet light to generate high-energy reaction intermediates, such as alkyl free radicals, oxide free radicals, etc., thereby initiating a photo-initiated reaction. The photo-initiated reaction can crosslink and cure the polymer, thereby forming a cured layer on the intermediate film body.

[0045] 4. In one embodiment, the spraying material includes a resin, a curing agent and a solid electrolyte, and the contents thereof in the spraying material are calculated by mass percentage as follows: resin, the content is 44%-46%; curing agent, the content is 44%; solid electrolyte, the content is 10%. By setting the above spraying material, in the subsequent curing process, the spraying material can be cured by heating and curing. Specifically, when the spraying material is heated, the curing agent therein will produce active free radicals or ions by thermal decomposition, and these active substances can react with the double bonds in the resin molecules to recombine the chemical bonds between the molecules to form a cross-linked structure. These cross-linked structures have high strength and rigidity, so that the cured spraying material has excellent mechanical properties. Therefore, after the heating and curing treatment, the curing layer extending laterally along the intermediate film body can play a role in improving the tensile strength of the second direction of the intermediate film body, thereby improving the tensile strength of the subsequent dry electrode plate in the second direction. Specifically, in one embodiment, the curing agent includes an amine curing agent or an acid anhydride curing agent. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] The drawings described herein are used to provide a further understanding of the present application and constitute a part of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:

[0047] Figure 1A schematic diagram of the steps of a dry electrode sheet processing method disclosed in one embodiment of the present application;

[0048] Figure 2 for Figure 1 A schematic diagram of the structure of the film forming equipment;

[0049] Figure 3 for Figure 2 Schematic diagram of the structure of the intermediate film after spraying treatment;

[0050] Figure 4 for Figure 3 A schematic top view of the intermediate membrane body;

[0051] Figure 5 for Figure 3 Scanning electron microscope image of the intermediate film after curing;

[0052] Figure 6 for Figure 5 Scanning electron microscope image of the cross section of the middle membrane;

[0053] Figure 7 The dry electrode sheets of Sample 1, Sample 2 and Sample 3 given in the embodiments of the present application are respectively fabricated into lithium-ion batteries, and their 400-cycle capacity retention rate test data;

[0054] Figure 8 A schematic structural diagram of a dry electrode sheet processing device provided in yet another embodiment of the present application;

[0055] Fig. 9 This is a schematic structural diagram of a dry electrode plate according to another embodiment of the present application. DETAILED DESCRIPTION

[0056] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present application will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.

[0057] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit the exemplary embodiments according to the present application. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprise" and / or "include" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.

[0058] Unless otherwise specifically stated, the relative arrangement, numerical expressions and numerical values ​​of the parts and steps set forth in these embodiments do not limit the scope of the application. Meanwhile, it should be understood that, for ease of description, the sizes of the various parts shown in the accompanying drawings are not drawn according to actual proportional relationships. The technology, methods and equipment known to those of ordinary skill in the relevant art may not be discussed in detail, but in appropriate cases, the technology, methods and equipment should be considered as a part of the specification. In all examples shown and discussed here, any specific value should be interpreted as being merely exemplary, rather than as a limitation. Therefore, other examples of exemplary embodiments may have different values. It should be noted that similar reference numerals and letters represent similar items in the following drawings, and therefore, once a certain item is defined in an accompanying drawing, it does not need to be further discussed in subsequent drawings.

[0059] See also Figures 1 to 4 One embodiment of the present application provides a dry electrode plate processing method based on spraying enhancement. The dry electrode plate processing method based on spraying enhancement includes the following steps:

[0060] The materials are mixed and dispersed uniformly. In the present embodiment, the materials include: an electrode main material, an adhesive and a conductive agent. Specifically, the electrode main material, the adhesive and the conductive agent are mechanically mixed to form a uniform dry powder mixture. The equipment used for mechanical mixing can be a high-speed high-power mixer or a ball mill. In the present embodiment, the electrode main material includes a nickel-cobalt-manganese ternary material or a lithium iron phosphate material. The adhesive includes a polytetrafluoroethylene material. The conductive agent includes conductive carbon black or carbon nanotubes. Calculated by mass percentage, the mass percentage contents of the electrode main material, the adhesive, and the conductive agent are respectively:

[0061] The electrode main material: 92.5%-97.50%; the adhesive: 0.5%-5%; the conductive agent: 1.5%-5%.

[0062] The uniformly dispersed material is subjected to a fiberization treatment. In this embodiment, the fiberization process is to process the adhesive into a form with a fibrous structure, so that it is easier to combine with the electrode main material, the conductive agent and other components during the dry mixing process. This step is also called the fibrillation step (Fibrillation). The adhesive is processed into a form with a fibrous structure, mainly to enable the adhesive to fully exert its bonding effect in a dry state, thereby enhancing the adhesion and mechanical strength of the mixture. Through the fiberization step, the adhesive can firmly combine the electrode main material and the conductive agent and other components. In one embodiment, the fiberization process is mainly to apply a high shear force to the mixed material, so that the adhesive is fiberized and then bonded to the electrode main material and the conductive agent and other materials to form a fiberized material.

[0063] The fiberized material is placed in a film-forming device to form an intermediate film body 10, and the intermediate film body 10 has a first direction and a second direction, wherein the first direction extends along the length direction of the intermediate film body 10, and the second direction extends along the width direction of the intermediate film body 10. In this embodiment, the film-forming device is a multi-stage rolling device. As needed, the fiberized material can be granulated before being placed in the multi-stage rolling device. The granulation process can make the fiberized material into granules through a mechanical granulation process. After the granulation process, the granules have good fluidity and handling characteristics, so that they are suitable for the subsequent film-forming steps.

[0064] The intermediate film body 10 is sprayed to form a plurality of spray stripes 11 , and the spraying direction is extended along the second direction of the intermediate film body.

[0065] The sprayed stripes 11 are cured to form a cured layer.

[0066] The intermediate film body having the solidified layer is further processed in the film forming device to form a self-supporting film.

[0067] The self-supporting film is pressed with a current collector to obtain a dry electrode plate. In this embodiment, the current collector may be a copper foil or an aluminum foil. In the process of combining the self-supporting film with the current collector, a hot press or a rolling press device may be used to firmly combine the self-supporting film with the current collector. As needed, before the self-supporting film is combined with the current collector, the current collector may be surface treated to enhance the adhesion of the current collector, so that the self-supporting film and the current collector can be more firmly combined to obtain the dry electrode plate.

[0068] In the dry electrode sheet processing method provided in the above embodiment, the intermediate film body 10 is sprayed to form a plurality of spray stripes 11, and the direction of the spraying treatment is to extend along the second direction of the intermediate film body 10. In the subsequent processing, the spray stripes 11 can be cured to form a solidified layer. At this time, the solidified layer extending laterally along the intermediate film body 10 can play a role in improving the tensile strength of the intermediate film body 10 in the second direction, thereby further improving the tensile strength of the subsequently manufactured dry electrode sheet in the second direction. The above spraying and curing treatment methods can effectively avoid the problem of damage and cracking of the dry electrode sheet during the calendering and winding process, and improve the production yield of the dry electrode sheet.

[0069] In practice, in the conventional production process of dry electrode plates, the self-supporting film is generally made by uniaxial stretching. Therefore, the prepared self-supporting film has good tensile strength in the first direction and low tensile strength in the second direction, so that the self-supporting film is easy to break in the second direction. In the dry electrode plate processing method provided in this embodiment, the intermediate film body 10 is sprayed to form a plurality of spray stripes 11, and the spray stripes 11 are cured in a subsequent process to form a solidified layer. Since the solidified layer has relatively excellent mechanical properties, it extends along the lateral direction of the intermediate film body 10, which can effectively improve the tensile strength of the intermediate film body 10 in the second direction, thereby improving the tensile strength of the subsequently manufactured dry electrode plate in the second direction.

[0070] In one of the embodiments, the spraying width of the spraying process ranges from 2 mm to 5 mm, and the spraying speed of the spraying process ranges from 0.1 m / s to 0.3 m / s.

[0071] In the above embodiment, the spraying width range of the spraying treatment is set to between 2mm and 5mm, and the spraying speed range of the spraying treatment is set to between 0.1m / s and 0.3m / s, which can effectively ensure that the formed solidified layer can improve the tensile strength of the second direction of the intermediate film body. In fact, the faster the speed of the spraying treatment, the less the spraying material attached to the intermediate film body, and the worse the effect of improving the tensile strength of the intermediate film body in the second direction after the spraying material is cured; the slower the speed of the spraying treatment, the more the spraying material attached to the intermediate film body, and the better the effect of improving the tensile strength of the intermediate film body in the second direction after the spraying material is cured. However, the slower the spraying speed, the longer the process time. Under comprehensive consideration, the spraying speed range is generally set to between 0.1m / s and 0.3m / s. In this way, the tensile strength of the second direction of the prepared dry electrode pole piece can be improved without having too much impact on the process time. The narrower the spraying width, the less the spraying material adheres to the intermediate film body, and after the spraying material is solidified, the worse the effect of improving the tensile strength of the intermediate film body in the second direction is; the wider the spraying width, the more the spraying material adheres to the intermediate film body, and after the spraying material is solidified, the better the effect of improving the tensile strength of the intermediate film body in the second direction is. Therefore, the spraying width is selected to be more than 2 mm as much as possible to achieve the effect of improving the tensile strength of the intermediate film body in the second direction.

[0072] In this embodiment, the transverse length of the spray stripe 11 is set according to the width of the intermediate film body 10, and is slightly shorter than the width of the intermediate film body 10. For example, assuming that the width of the intermediate film body 10 is 300 mm, the transverse length of the spray stripe 11 can be set to 250-300 mm.

[0073] In one embodiment, during the spraying process, the spraying material includes a resin system oligomer, a diluent, a solid electrolyte and an initiator, and the contents thereof in the spraying material are calculated by mass percentage as follows:

[0074] Resin system oligomer, content is 62%-65%;

[0075] Diluent, content is 18%-20%;

[0076] Solid electrolyte, content of 13.5%-14.5%;

[0077] Initiator, content is 2.5%.

[0078] In the above embodiments, since the spraying material includes a resin system oligomer, a diluent, a solid electrolyte and an initiator, in the subsequent curing process, the spraying material can be cured by ultraviolet curing. Specifically, the initiator in the spraying material decomposes into free radicals after being irradiated with ultraviolet light, thereby initiating polymer cross-linking and curing, thereby forming a cured layer on the intermediate film body. The cured layer extending laterally along the intermediate film body can play a role in improving the tensile strength of the intermediate film body in the second direction, thereby improving the tensile strength of the subsequent dry electrode plate in the second direction. In one embodiment, the resin system oligomer includes polyurethane acrylate, epoxy acrylate or polyester acrylate, the diluent includes acrylic acid multifunctional monomer, the initiator includes acylphosphine oxide, and the solid electrolyte includes lithium lanthanum zirconium oxide, lithium titanium aluminum phosphate or aluminum oxide. When the initiator is an acylphosphine oxide, the acylphosphine oxide will be excited after absorbing ultraviolet light, thereby generating high-energy reaction intermediates, such as alkyl radicals, oxide radicals, etc., thereby initiating a photoinitiated reaction. The photoinitiated reaction can cause the polymer to crosslink and cure, thereby forming a cured layer on the intermediate film body.

[0079] Therefore, when the spraying material includes a resin system oligomer, a diluent, a solid electrolyte and an initiator, in the process of curing the spraying stripes, ultraviolet light is used to cure the spraying material to form the cured layer.

[0080] In one embodiment, during the spraying process, the spraying material includes a resin, a curing agent and a solid electrolyte, and the contents thereof in the spraying material are respectively as follows, calculated by mass percentage:

[0081] Resin, content is 44%-46%;

[0082] Curing agent, content is 44%-46%;

[0083] Solid electrolyte, content is 10%.

[0084] In the above embodiments, the spray material includes a resin, a curing agent and a solid electrolyte. In the subsequent curing process, the spray material can be cured by heating. Specifically, when the spray material is heated, the curing agent therein will produce active free radicals or ions through thermal decomposition. These active substances can react with the double bonds in the resin molecules to recombine the chemical bonds between the molecules to form a cross-linked structure. These cross-linked structures have high strength and rigidity, so that the cured spray material has excellent mechanical properties. Therefore, after the heating and curing treatment, the cured layer extending laterally along the intermediate film body can play a role in improving the tensile strength of the intermediate film body in the second direction, thereby improving the tensile strength of the subsequently manufactured dry electrode pole piece in the second direction.

[0085] In one embodiment, the resin includes phenolic resin, epoxy resin, acrylic resin or polyester resin, the curing agent includes amine curing agent and acid anhydride curing agent, and the solid electrolyte includes lithium lanthanum zirconium oxide, lithium aluminum titanium phosphate or aluminum oxide.

[0086] In this embodiment, by providing an amine curing agent or an acid anhydride curing agent, in the subsequent process of curing the spray material, the amine curing agent or the acid anhydride curing agent has a better thermal curing effect on the resin.

[0087] Table 1 shows the effect of different spraying speeds and spraying widths on the tensile strength of dry electrode sheets.

[0088]

[0089] It can be seen from Table 1 that the faster the speed of the spraying treatment, the less the spraying material attached to the intermediate film body, and the worse the effect of improving the tensile strength of the intermediate film body in the second direction after the spraying material is cured. The slower the speed of the spraying treatment, the more the spraying material attached to the intermediate film body, and the better the effect of improving the tensile strength of the intermediate film body in the second direction after the spraying material is cured. However, the slower the spraying speed, the longer the process time. Under comprehensive consideration, the spraying speed range is generally set between 0.1m / s and 0.3m / s. In this way, the tensile strength of the prepared dry electrode sheet in the second direction can be improved without having too much impact on the process time. The narrower the spraying width, the less the spraying material attached to the intermediate film body, and the worse the effect of improving the tensile strength of the intermediate film body in the second direction after the spraying material is cured; the wider the spraying width, the more the spraying material attached to the intermediate film body, and the better the effect of improving the tensile strength of the intermediate film body in the second direction after the spraying material is cured. Therefore, the spraying width is selected to be greater than 2 mm as much as possible to achieve the effect of improving the tensile strength of the intermediate film body in the second direction.

[0090] Using UV light-curing paint, the spraying speed is 0.3m / s, the spraying width is 1mm, the tensile strength of the dry electrode pole piece is 0.08MPa, and cracks appear in the first direction of the dry electrode pole piece during the winding process, which means that the tensile strength in the second direction is relatively low. Using UV light-curing paint, the spraying speed is 0.1m / s, the spraying width is 2mm, the tensile strength of the dry electrode pole piece is 0.20MPa, and the dry pole piece does not show any damage or cracking. Using UV light-curing paint, the spraying speed is 0.3m / s, the spraying width is 5mm, the tensile strength of the dry electrode pole piece is 0.48MPa, and the dry pole piece does not show any damage or cracking in the first direction. Using UV light-curing paint, the spraying speed is 0.1m / s, the spraying width is 5mm, the tensile strength of the dry electrode pole piece is 0.65MPa, and the dry pole piece does not show any damage or cracking in the first direction. The above data show that by adjusting the spraying speed and spraying width of UV curing spraying, the strength of the dry electrode in the second direction can be improved, and the dry electrode can be effectively prevented from being damaged along the first direction.

[0091] Using thermosetting paint, the spraying speed is 0.3m / s, the spraying width is 1mm, the tensile strength of the dry electrode plate is 0.06MPa, and cracks appear in the first direction of the dry electrode plate during the winding process, which means that the tensile strength in the second direction is relatively low. Using thermosetting paint, the spraying speed is 0.3m / s, the spraying width is 2mm, the tensile strength of the dry electrode plate is 0.19MPa, and no damage or cracking occurs in the first direction of the dry electrode plate. Using thermosetting paint, the spraying speed is 0.3m / s, the spraying width is 5mm, the tensile strength of the dry electrode plate is 0.42MPa, and no damage or cracking occurs in the first direction of the dry electrode plate. Using thermosetting paint, the spraying speed is 0.1m / s, the spraying width is 5mm, the tensile strength of the dry electrode plate is 0.58MPa, and no damage or cracking occurs in the first direction of the dry electrode plate. The above data show that by adjusting the spraying speed and spraying width of the powder thermal curing spray, the strength of the dry electrode in the second direction can be improved, and the dry electrode can be effectively prevented from being damaged along the first direction.

[0092] Please also see Figures 2 to 4 In one embodiment, the film forming device is a multi-stage rolling device. The multi-stage rolling device includes a first pressing roller 110, a second pressing roller 120, a third pressing roller 130 and a fourth pressing roller 140. A first roller gap 111 is formed between the first pressing roller 110 and the second pressing roller 120. A second roller gap 121 is formed between the second pressing roller 120 and the third pressing roller 130. A third roller gap 131 is formed between the third pressing roller 130 and the fourth pressing roller 140. The fiberized material passes through the first roller gap 111 and the second roller gap 112 to form the intermediate film body 10.

[0093] In this embodiment, the fiberized material passes through the first roller gap 111 and the second roller gap 121 to form the intermediate film body 10. After the rolling process of the first roller gap 111 and the second roller gap 121, the intermediate film body 10 can be roughly formed, which is convenient for subsequent spraying and curing operations.

[0094] In one embodiment, the first pressing roller 110, the second pressing roller 120, the third pressing roller 130 and the fourth pressing roller 140 are arranged along the first direction, that is, the length direction of the intermediate film body 10. In this embodiment, the first direction is the MD direction of the dry electrode sheet, or the movement direction of the dry electrode sheet. The rotation axis direction of the first pressing roller 110, the second pressing roller 120, the third pressing roller 130 and the fourth pressing roller 140 is the second direction perpendicular to the first direction, that is, the width direction of the intermediate film body 10. In this embodiment, the second direction is the TD direction of the dry electrode sheet, or the lateral direction of the dry electrode sheet. The spraying device 20 is arranged close to the third pressing roller 130 to spray the intermediate film body 10 formed after passing through the first roller gap 111 and the second roller gap 121. The spraying direction of the spraying device 20 is parallel to the second direction.

[0095] In this embodiment, the spraying device 20 is arranged close to the third pressing roller 130 to spray the intermediate film body 10 formed after passing through the first roller gap 111 and the second roller gap 121. On the one hand, after the rolling process of the first roller gap 111 and the second roller gap 121, the intermediate film body 10 can be roughly formed, which is convenient for the subsequent spraying process.

[0096] In this embodiment, the curing device 21 is used to cure the sprayed stripes to form a cured layer. In this embodiment, the curing device 21 can be arranged between the third pressing roller 130 and the fourth pressing roller 140, or can be arranged close to the fourth pressing roller 140, or can be arranged after the fourth pressing roller 140, as long as it can achieve the curing of the sprayed stripes formed on the surface of the intermediate film body 10. In one embodiment, an independent chamber can also be arranged in the multi-stage rolling device, and the independent chamber is arranged after the third pressing roller 130. The curing device 21 is arranged in the independent chamber to cure the sprayed stripes.

[0097] In this embodiment, the intermediate film body 10 after spraying and curing is subjected to differential thinning in the third roller gap 131 to form the self-supporting film. As needed, the multi-stage rolling equipment can further increase the number of rollers to adjust the thickness and compaction density of the dry electrode sheet.

[0098] Figure 5 The surface SEM (scanning electron microscope) photos of the dry electrode sheets made after spraying and curing are given. Figure 6 The cross-sectional SEM (scanning electron microscope) photo of the dry electrode sheet made by spraying and curing is given. It can be seen from the figure that Figure 5 and Figure 6 The thick and long fiber bundles in the electrode are fiber structures formed by UV-cured resin, which are cross-linked with the slender PTFE fiber structures to form a network structure, providing stronger cohesion and higher tensile strength for the electrode structure.

[0099] Table 2 shows the K value test data of the dry electrode plate made by spray curing treatment after being made into a lithium-ion battery. Table 3 shows the K value test data of the dry electrode plate made without spray curing treatment after being made into a lithium-ion battery. The K value is an important indicator to measure the self-discharge degree of lithium-ion batteries. It refers to the voltage drop of lithium-ion batteries per unit time. K=△OCT / △t, OCV refers to the open circuit voltage, t is the storage time. The unit of K value is mV / d, which is related to the performance of the battery itself, the test conditions, the positive and negative electrode materials, and the length of storage time.

[0100]

[0101]

[0102] As can be seen from Table 2 and Table 3, in terms of the K value test results, the dry electrode sheet made without laser treatment has an average K value of 0.0393 and an average yield of 98.05% after being made into a lithium-ion battery; while the dry electrode sheet made with laser treatment has an average K value of 0.0225 and an average yield of 99.12% after being made into a lithium-ion battery. That is, compared with the dry electrode sheet made without spray curing treatment, the dry electrode sheet made with spray curing treatment has an improved K value and yield after being made into a lithium-ion battery.

[0103] In one of the embodiments, part of the spraying material may be first mixed into the material, and after mixing, fiberization, pre-filming and spraying, during the curing of the spray stripes, since the intermediate film body also has the spraying material, this part of the material will also be cured during the curing process, thereby increasing the tensile strength of the intermediate film body. The specific process is as follows: in the process of mixing and evenly dispersing the materials, the spraying material used for the spraying treatment is added to the materials and mixed and evenly dispersed, and the mass percentage content of the spraying material is 0.5%-1%; in the curing process, the spraying material added to the material is cured together with the spraying stripes. At this time, the material includes: an electrode main material, an adhesive, a conductive agent and a spraying material. Calculated by mass percentage, the mass percentage contents of the electrode main material, the adhesive, the conductive agent and the spraying material are respectively:

[0104] The electrode main material: 92.5%-97.50%; the adhesive: 0.5%-4%; the conductive agent: 1.5%-5%; the spraying material: 0.5%-1%.

[0105]

[0106] Table 4 gives the tensile strength data of samples without spray curing, spray curing, and doping + spray curing. It can be seen from Table 4 that for sample 1, spray material was used for doping, the content was 0.5% (wt), and the binder content was 1.5% (wt). The tensile strength of the dry electrode sheet was 0.65MPa. The dry electrode sheet did not show any damage in the first direction. For sample 2, the binder content was 2%, and no spray material was used for doping, but spraying and curing were used in the manufacturing process. The tensile strength of the dry electrode sheet was 0.58MPa, and the dry electrode sheet did not show any damage in the first direction. For sample 3, the binder content was 2%, no spray material was used for doping, and no spraying and curing were performed. The tensile strength of the dry electrode sheet was 0.1MPa, and the dry electrode sheet was prone to damage in the first direction.

[0107] In this embodiment, the composition of the spraying material is Formula 1. The ingredients of Formula 1 are: the spraying material includes a resin system oligomer, a diluent, a solid electrolyte and an initiator, and the contents thereof in the spraying material are respectively as follows, calculated by mass percentage:

[0108] Resin system oligomer, content is 62%-65%;

[0109] Diluent, content is 18%-20%;

[0110] Solid electrolyte, content of 13.5%-14.5%;

[0111] Initiator, content is 2.5%.

[0112] The above embodiments illustrate that the doping+spray curing treatment can effectively improve the tensile strength of the dry electrode sheet in the second direction, thereby effectively preventing the dry electrode sheet from cracking along the first direction.

[0113] Figure 7 The 400-week capacity retention test data of the dry electrode plates in Sample 1, Sample 2, and Sample 3 after they were made into lithium-ion batteries are given. The 400-week capacity retention rate refers to the ability of the battery to maintain its capacity after 400 cycles. The test data of Sample 1 is represented by the blue line. The test data of Sample 2 is represented by the red line. The test data of Sample 3 is represented by the green line. Figure 7 It can be seen that the 400-week capacity retention rate of sample 1 is 90.96%, the 400-week capacity retention rate of sample 2 is 88.78%, and the 400-week capacity retention rate of sample 3 is 20%.

[0114] The above data show that the normal temperature cycle performance of lithium-ion batteries made of dry electrode sheets that are doped + sprayed and cured is better than that of lithium-ion batteries made of dry electrode sheets that are not sprayed and cured. Among them, the normal temperature cycle performance of lithium-ion batteries made of dry electrode sheets that are doped + sprayed and cured is the best.

[0115] Table 5 shows the rate discharge performance of the dry electrode sheets in Sample 1, Sample 2 and Sample 3 after being made into lithium-ion batteries. Table 6 shows the rate charge performance of the dry electrode sheets in Sample 1, Sample 2 and Sample 3 after being made into lithium-ion batteries.

[0116]

[0117]

[0118] It can be seen from Tables 5 and 6 that the high-rate charge and discharge performance of the lithium-ion battery made of the dry electrode sheet of Sample 1 is not as good as that of the lithium-ion battery made of the dry electrode sheet of Sample 2. However, the high-rate charge and discharge performance of the lithium-ion battery made of the dry electrode sheet of Sample 2 is better than that of the lithium-ion battery made of the dry electrode sheet of Sample 3. The above data show that the high-rate charge and discharge performance of the lithium-ion battery is affected to a certain extent by doping the spray material, but considering its excellent performance in room temperature cycling, it can be used in application scenarios with long cycle requirements. However, the high-rate charge and discharge performance of the spray-cured sample 2 is better than the high-rate charge and discharge performance of the unspray-cured sample 3.

[0119] See also Figure 8 Another embodiment of the present application provides a dry electrode sheet processing device 200 based on spraying enhancement, comprising:

[0120] The mixing device 210 is used to mix and evenly disperse the materials.

[0121] The material fiberizing device 220 is used to perform fiberizing treatment on the uniformly dispersed material.

[0122] The pre-filming device 230 is used to process the fiberized material into a film to form an intermediate film body. The intermediate film body has a first direction and a second direction, wherein the first direction extends along the length direction of the intermediate film body and the second direction extends along the width direction of the intermediate film body.

[0123] The spraying device 20 is used to spray the intermediate film body to form a plurality of spraying stripes. The spraying direction is along the second direction of the intermediate film body.

[0124] The curing device 21 cures the sprayed stripes to form a cured layer.

[0125] The film forming device 260 is used to process the intermediate film body having the solidified layer to form a self-supporting film.

[0126] The composite processing equipment 270 is used to press the self-supporting film and the current collector to obtain a dry electrode plate.

[0127] In this embodiment, the pre-film forming device 230 and the film forming device 260 are different parts of the same set of equipment. Specifically, the pre-film forming device 230 is the front section of the multi-stage rolling device, and the film forming device 260 is the back section of the multi-stage rolling device.

[0128] Yet another embodiment of the present application provides a dry electrode plate, which is manufactured by the dry electrode plate processing method as described in any one of the above embodiments.

[0129] See also Fig. 9 Another embodiment of the present application provides a dry electrode plate 300 based on spraying enhancement, comprising:

[0130] a current collector 310; and

[0131] The self-supporting film 320 is disposed on the surface of the current collector 310. A solidification layer 330 is disposed on the surface of the self-supporting film 320. The solidification layer 330 includes a plurality of spray-cured stripes 331. The spray-cured stripes 331 extend in the lateral direction of the self-supporting film 320.

[0132] The width of the spray curing stripe 331 ranges from 2 mm to 5 mm;

[0133] The thickness of the spray-cured stripes 331 is in the range of 10 μm to 1 mm.

[0134] In this embodiment, a plurality of spray-cured stripes 331 are provided on the surface of the self-supporting film 320, and the spray-cured stripes 331 are provided along the lateral extension of the self-supporting film 320. Since the spray-cured stripes 331 have relatively excellent mechanical properties, and their width ranges from 2 mm to 5 mm, and their thickness ranges from 10 μm to 1 mm, the spray-cured stripes 331 can enhance the tensile strength of the self-supporting film 320 in the second direction.

[0135] For ease of description, spatially relative terms such as "above", "above", "on the upper surface of", "above", etc. may be used herein to describe the spatial positional relationship between a device or feature and other devices or features as shown in the figure. It should be understood that spatially relative terms are intended to include different orientations of the device in use or operation in addition to the orientation described in the figure. For example, if the device in the accompanying drawings is inverted, the device described as "above other devices or structures" or "above other devices or structures" will be positioned as "below other devices or structures" or "below other devices or structures". Thus, the exemplary term "above" may include both "above" and "below". The device may also be positioned in other different ways (rotated 90 degrees or in other orientations), and the spatially relative descriptions used herein are interpreted accordingly.

[0136] In addition, it should be noted that the use of terms such as "first" and "second" to limit components is only for the convenience of distinguishing the corresponding components. Unless otherwise stated, the above terms have no special meaning and therefore cannot be understood as limiting the scope of protection of this application.

[0137] The above are only preferred embodiments of the present application and are not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.

Claims

1. A dry electrode plate processing method based on spraying enhancement, It is characterized in that The following steps are involved: Mixing and evenly dispersing materials, the materials including: electrode main material, adhesive and conductive agent; The uniformly dispersed material is subjected to fiberization treatment; Putting the fiberized material into a film forming device to form an intermediate film body, wherein the intermediate film body has a first direction and a second direction, wherein the first direction extends along the length direction of the intermediate film body, and the second direction extends along the width direction of the intermediate film body; Performing a spraying treatment on the intermediate film body to form a plurality of spraying stripes, wherein the spraying treatment direction extends along the second direction of the intermediate film body; Curing the sprayed stripes to form a cured layer; The intermediate film body having the solidified layer is further processed in the film forming device to form a self-supporting film; Pressing the self-supporting film and the current collector to obtain a dry electrode plate; The spraying width of the spraying process is in the range of 2 mm to 5 mm, and the spraying speed of the spraying process is in the range of 0.1 m / s to 0.3 m / s. During the spraying process, the spraying material includes resin system oligomers, diluents, solid electrolytes and initiators. Calculated by mass percentage, their contents in the spraying material are: resin system oligomers, content of 62%-65%; diluents, content of 18%-21%; solid electrolytes, content of 13.5%-14.5%; initiators, content of 2.5%; or, during the spraying process, the spraying material includes resin, curing agent and solid electrolytes. Calculated by mass percentage, their contents in the spraying material are: resin, content of 44%-46%; curing agent, content of 44%-46%; solid electrolyte, content of 10%.

2. According to claim 1, the dry electrode plate processing method based on spraying enhancement, It is characterized in that The resin system oligomer includes polyurethane acrylate, epoxy acrylate or polyester acrylate, the diluent includes acrylic multifunctional monomer, the initiator includes acylphosphine oxide, and the solid electrolyte includes lithium lanthanum zirconium oxide, lithium titanium aluminum phosphate or aluminum oxide.

3. The dry electrode plate processing method based on spraying enhancement according to claim 1, It is characterized in that The resin includes phenolic resin, epoxy resin, acrylic resin or polyester resin, the curing agent includes amine curing agent and acid anhydride curing agent, and the solid electrolyte includes lithium lanthanum zirconium oxide, lithium aluminum titanium phosphate or aluminum oxide.

4. The dry electrode sheet processing method based on spraying enhancement according to any one of claims 1 to 3, It is characterized in that In the process of mixing and uniformly dispersing the materials, the spraying material used in the spraying treatment is added to the materials, mixed and uniformly dispersed, and the mass percentage content of the spraying material is 0.5%-1%; During the curing process, the spray material added to the material is cured together with the spray stripes.

5. A dry electrode plate processing device based on spraying enhancement, used to perform the dry electrode plate processing method based on spraying enhancement as claimed in any one of claims 1 to 4, It is characterized in that include: Mixing equipment, used to mix and evenly disperse materials; Material fiberizing equipment, used for fiberizing the uniformly dispersed material; A pre-filming device, used for filming the fiberized material to form an intermediate film body, wherein the intermediate film body has a first direction and a second direction, wherein the first direction extends along the length direction of the intermediate film body, and the second direction extends along the width direction of the intermediate film body; A spraying device, used for spraying the intermediate film body to form a plurality of spraying stripes, wherein the spraying direction is extending along the second direction of the intermediate film body; A curing device for curing the sprayed stripes to form a cured layer; A film forming device, used for processing the intermediate film body having the solidified layer to form a self-supporting film; The composite processing equipment is used to press the self-supporting film and the current collector to obtain a dry electrode plate.

6. A dry electrode sheet based on spraying enhancement, It is characterized in that The dry electrode plate is manufactured by the dry electrode plate processing method based on spraying enhancement as described in any one of claims 1 to 4.

7. The dry electrode sheet based on spraying enhancement according to claim 6, It is characterized in that include: current collector; as well as A self-supporting film is arranged on the surface of the current collector, and a solidified layer is arranged on the surface of the self-supporting film, and the solidified layer includes a plurality of spray-cured stripes, and the spray-cured stripes extend in the lateral direction of the self-supporting film; The width of the spray-cured stripes ranges from 2 mm to 5 mm; The thickness of the spray-cured stripes ranges from 10 μm to 1 mm.