Heavy oil hydrodemetallization catalyst and preparation method thereof
By using active metal-modified flaky pseudo-boehmite to adjust the pore structure of the catalyst, the problem of reduced activity and deactivation of heavy oil hydrodemetallization catalysts in the existing technology is solved, achieving high activity and sedimentation resistance, and simplifying preparation process.
Patent Information
- Application Number
- CN202310356750.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-06
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-04-06
AI Technical Summary
Existing heavy oil hydrodemetallization catalysts have problems with activity decline and deactivation in vacuum residue oil with high metal content, and the existing hole expansion methods are complex and have insufficient catalytic activity.
Active metal-modified flaky pseudo-boehmite is used as the carrier raw material, and the pore structure of the catalyst is adjusted through hydrothermal treatment to improve the active metal matching and pore activity of the catalyst. The active metal is loaded through the impregnation method to prepare a highly active catalyst. and catalysts that resist metal deposition.
The catalytic activity and utilization rate of the catalyst are improved, the operating cycle of the catalyst is extended, the preparation process is simple, and the catalyst has high resistance to metal deposition and stability.
Smart Images

Figure CN118767932A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of catalyst preparation, and specifically relates to a heavy oil hydrodemetallization catalyst and a preparation method thereof. Background Art
[0002] In recent years, with the heavy nature of crude oil resources, the growth of demand for fuel oil consumption and increasingly stringent environmental regulations, the use of hydrogenation technology to convert heavy oil including residual oil into high-quality fuel oil and chemical products is helpful to improve crude oil utilization, reduce environmental pollution, increase light oil yield and improve product quality. Hydrodemetallization catalysts used for heavy oil, especially vacuum residue with high metal content, are prone to rapid decline and deactivation of catalyst activity due to the deposition of metal impurities such as nickel and vanadium. Catalysts with larger pore volume and larger pore diameter have strong metal and carbon tolerance, which can slow down the deactivation of catalysts and extend the operation cycle of catalysts. The pore structure of the catalyst is determined by the carrier constituting the catalyst. Therefore, the preparation of a carrier with larger pore volume and larger pore diameter is the key to preparing residual oil, especially preparing a catalyst for hydrogenation and demetallization of vacuum residue with high metal content.
[0003] Alumina is a commonly used catalyst carrier, widely used in the fields of petroleum processing, chemical industry, environmental protection, etc. The pore diameter of alumina commonly used to prepare hydroprocessing catalysts and commercially available alumina is relatively small, which cannot meet the needs of preparing heavy oil, residual oil hydrodemetallization and / or heavy oil hydrodesulfurization catalysts. Therefore, it is necessary to use the method of "pore expansion" to increase its pore diameter during the carrier preparation process.
[0004] CN201510191156.7 discloses a heavy oil hydrogenation catalyst and a preparation method thereof. The catalyst comprises an alumina carrier composed of flaky polycrystalline γ-alumina and a hydrogenation active metal. The preparation method of the catalyst is as follows: adding a binder and an extrusion aid to a flaky γ-polycrystalline alumina raw powder, kneading, molding, drying and calcining to obtain an alumina carrier, and loading the active metal on the obtained alumina carrier by a conventional method. The preparation method of the flaky polycrystalline γ-alumina comprises the following steps: (1) mixing an inorganic aluminum salt, a low-carbon alcohol and / or water, and a low-carbon alkylene oxide uniformly to form a gel, and then aging the gel; (2) soaking the gel obtained in step (1) with a low-carbon alcohol, and then drying and calcining; (3) immersing the material obtained in step (2) in ammonia water for closed hydrothermal treatment, solid-liquid separation, and drying to obtain a flaky γ-polycrystalline alumina raw powder. This invention adjusts the pore structure of the carrier by adding flaky polycrystalline γ-alumina into the alumina carrier, but the preparation process of flaky polycrystalline γ-alumina is relatively complicated.
[0005] CN107913691A discloses an alumina carrier containing macropores and a preparation method thereof. The method firstly adds pseudo-boehmite powder and sesbania powder into a kneader and mixes them evenly, then prepares a styrene-butadiene rubber emulsion with a particle size of 10-500nm, and adds an organic acid or an inorganic acid thereto; then adds the acid solution containing the styrene-butadiene rubber emulsion into the pseudo-boehmite powder and sesbania powder and kneads them evenly, and then extrudes, forms, dries, and roasts to obtain an alumina carrier containing macropores. The pore size distribution of the alumina carrier obtained by the method is 60-400nm. However, the preparation process of the pore-enlarging agent styrene-butadiene rubber emulsion by the method is relatively complicated.
[0006] CN109718747A discloses a dual-pore alumina carrier, a demetallization catalyst and a preparation method thereof, wherein the dual-pore alumina carrier contains rod-shaped alumina clusters. The preparation method of the dual-pore alumina carrier comprises: calcining pseudo-boehmite A to obtain alumina; immersing the alumina in an aqueous solution of ammonium bicarbonate for sealed heat treatment, drying, and soaking in a polyethylene glycol solution, drying the material after soaking to obtain rod-shaped alumina clusters; then kneading pseudo-boehmite B with the rod-shaped alumina clusters obtained above into a molded product, drying and calcining the molded product to obtain a dual-pore alumina carrier. The invention adjusts the pore structure of the alumina carrier and the demetallization catalyst by using rod-shaped alumina clusters, but the catalytic activity of the catalyst prepared by this method at the macropores needs to be further improved. Summary of the invention
[0007] In view of the deficiencies in the prior art, the present invention provides a heavy oil hydrodemetallization catalyst and a preparation method thereof. The method uses flaky pseudo-boehmite modified with active metals as part of the raw materials, adjusts the pore structure of the catalyst, improves the matching degree between the pore structure of the catalyst and the active metal, and enhances the catalytic activity and utilization rate of the catalyst macropores. The preparation process is simple, and the prepared hydrodemetallization catalyst has high activity and resistance to metal deposition.
[0008] The heavy oil hydrodemetallization catalyst of the present invention comprises an active metal component and an alumina carrier, wherein the active metal component is a metal of Group VIB and Group VIII, and the alumina carrier comprises flaky alumina crystals and granular alumina crystals, wherein the mass ratio D of the content of the active metal component at the micro-region of the flaky particles to the active metal component at the micro-region of the spherical particles in terms of oxide is 1.1-1.85, and further preferably, the mass ratio D1 of the content of the Group VIB metal oxide at the micro-region of the flaky alumina crystals to the Group VIB metal oxide at the micro-region of the granular alumina crystals in terms of oxide is 1.25-1.50, and the mass ratio D2 of the Group VIII metal at the flaky alumina crystals to the Group VIII metal at the micro-region of the granular alumina crystals in terms of oxide is 1.20-1.55.
[0009] In the heavy oil hydrodemetallization catalyst of the present invention, the flaky alumina crystal has a size of 100-600nm and a thickness of 15-40nm, and the granular alumina crystal has a size of 20-100nm.
[0010] In the heavy oil hydrodemetallization catalyst of the present invention, based on the weight of the hydrodemetallization catalyst, the content of the active metal component in terms of oxide is 8%-20%, and the content of the alumina carrier is 80%-92%; preferably, the content of the VIB group metal in terms of metal oxide is 6.5wt%-12.5wt%, and the content of the VIII group metal in terms of metal oxide is 1.5wt%-4.5wt%; further preferably, the VIB group metal is selected from W and / or Mo, and the VIII group metal is selected from Co and / or Ni.
[0011] The heavy oil hydrodemetallization catalyst of the present invention has a specific surface area of 160-240m 2 / g, the pore volume is 0.65-1.1mL / g, the most probable pore diameters are 10-20nm and 50-100nm, the pores of 10-20nm account for 40%-60% of the total pore volume, and the pores of 50-100nm account for 10%-25% of the total pore volume.
[0012] The preparation method of the heavy oil hydrodemetallization catalyst of the present invention comprises the following contents: (1) roasting, crushing and screening aluminum nitrate, impregnating the screened material with an active component impregnation solution, drying and roasting the impregnated material to obtain a modified material; (2) immersing the modified material in a propylene oxide solution for closed heat treatment, and drying the treated material to obtain active metal-modified flaky pseudo-boehmite P1; (3) The active metal-modified flaky pseudo-boehmite P1 and the pseudo-boehmite P2 in step (2) are kneaded and formed into a carrier, and then loaded with active metal components to obtain a heavy oil hydrodemetallization catalyst.
[0013] In the method of the present invention, the calcination temperature of the aluminum nitrate in step (1) is 450-650° C., the calcination time is 4-8 hours, and the particle size of the material is greater than 100 mesh, preferably greater than 200 mesh.
[0014] In the method of the present invention, the active component impregnation solution in step (1) is a solution containing metals of Group VIB and Group VIII, preferably W and / or Mo of Group VIB, and Co and / or Ni of Group VIII. The preparation of the impregnation solution is well known to those skilled in the art, such as a phosphoric acid solution of W and / or Mo and Co and / or Ni, the concentration of WO3 and / or MoO3 in the solution is 1.5-4 g / 100 mL, and the concentration of CoO and / or NiO is 0.5-1.2 g / 100 mL. The amount of impregnation solution is such that the sieved material is completely immersed, and the impregnation time is 0.5-2 hours. The drying temperature is 80-140°C, the drying time is 4-10 hours, and the calcination temperature is 400-550°C, and the calcination time is 4-10 hours.
[0015] In the method of the present invention, the concentration of the propylene oxide solution in step (2) is 2.5wt%-12wt%, preferably 4wt%-8wt%, and the mass ratio of the propylene oxide solution to the modified material is 3:1-10:1, preferably 4:1-8:1.
[0016] In the method of the present invention, the closed heat treatment in step (2) is generally carried out in a closed container, preferably an autoclave, the closed heat treatment temperature is 110-180°C, preferably 120-160°C, the closed heat treatment time is 4-8 hours, and the pressure in the sealed container during the closed heat treatment is autogenous pressure. The drying temperature is 100-160°C, and the drying time is 2-8 hours.
[0017] In the method of the present invention, the pseudo-boehmite P2 described in step (3) can be a granular pseudo-boehmite prepared by an existing method, such as an acid precipitation method, an alkali precipitation method, an alcohol aluminum hydrolysis method, etc., preferably a spherical particle, further preferably a pseudo-boehmite with a pore size of 10-20 nm, and more preferably a pseudo-boehmite with a pore volume of 10-20 nm accounting for more than 50% of the total pore volume.
[0018] In the method of the present invention, the mass ratio of the active metal modified pseudo-boehmite P1 to the pseudo-boehmite P2 in step (3) is 1:4-1:1.
[0019] In the method of the present invention, the kneading molding described in step (3) is carried out by conventional methods in the art. During the molding process, conventional molding aids such as peptizers, extrusion aids, etc. may be added as needed. The peptizer is one or more of hydrochloric acid, nitric acid, sulfuric acid, acetic acid, oxalic acid, etc., and the mass percentage concentration of the peptizer is 0.5%-2%. The amount of the peptizer depends on the molding effect; the extrusion aid is sesbania powder, and the amount added is 1%-3% of the final weight of the alumina carrier.
[0020] In the method of the present invention, the carrier preparation process described in step (3) generally also includes drying and calcining the formed material. The general drying temperature is 100-160°C, the drying time is 6-10 hours, and the calcination temperature is 450-750°C, preferably 500-600°C, and the calcination time is 4-6 hours.
[0021] In the method of the present invention, the loading process described in step (3) is carried out by impregnation, and the alumina carrier is impregnated with an active metal component impregnation liquid. The impregnated carrier is dried and calcined to obtain a hydrodemetallization catalyst; the active metal component impregnation liquid is a solution containing a metal of Group VIB and a metal of Group VIII. The metal of Group VIB is Mo and / or W, preferably Mo, the metal of Group VIII is Ni and / or Co, preferably Ni, the content of the metal of Group VIB is 6-16 g / 100 mL in terms of oxide, and the content of the metal of Group VIII is 0.5-4.5 g / 100 mL in terms of oxide. The active component impregnation liquid can be an ammonia solution, an aqueous solution or a phosphoric acid solution of the metal of Group VIB and the metal of Group VIII, preferably a phosphoric acid solution containing the metal of Group VIB and the metal of Group VIII; the drying and calcination conditions are well known to those skilled in the art, and are generally: a drying temperature of 100-160°C, a drying time of 6-10 hours; a calcination temperature of 450-550°C, and a calcination time of 4-6 hours.
[0022] Compared with the prior art, the present invention has the following advantages: (1) The method of the present invention first prepares active metal modified pseudo-boehmite P1, the pseudo-boehmite grains are flaky in structure, the grain size is relatively large, and the flaky grains are interwoven and stacked to form a large number of macroporous channels; when the carrier is extruded, the flaky particles support each other, so that the formed macroporous channels are relatively intact, ensuring the macroporous content of the final carrier and catalyst, which is beneficial to the diffusion of macromolecular reactants in the reaction raw materials.
[0023] (2) The present invention uses active metal-modified flaky pseudo-boehmite as part of the raw material to prepare a hydrodemetallization catalyst. The macropores formed by the accumulation of flaky particles in the catalyst have a high content of active metal, which improves the catalytic activity of the macropores in the catalyst. In addition, the high activity sites of the catalyst are well matched with the pores, and the high activity sites have a strong ability to resist metal deposition, thereby ensuring high activity of the catalyst while having high activity stability.
[0024] (3) The active metal-modified flaky pseudo-boehmite used in the present invention is obtained by hydrothermal treatment of an aluminum compound containing an active metal in a propylene oxide solution. During the hydrothermal treatment, the active metal component grows secondary along with the aluminum compound, which can improve the strong interaction between the active metal and the final alumina carrier and enhance the catalyst activity. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] FIG1 is a SEM image of the sample prepared in Example 1.
[0026] FIG. 2 is a SEM image of the sample prepared in Comparative Example 1.
[0027] FIG3 is a SEM image of the sample prepared in Comparative Example 4. Implementation
[0028] The technical scheme and technical effect of the present invention are further described below in conjunction with the embodiments, but are not limited to the following embodiments. In the present invention, wt% represents mass fraction.
[0029] BET method: N2 physical adsorption-desorption was used to characterize the pore structure of the carriers of the embodiment and the comparative example. The specific operation was as follows: The pore structure of the sample was characterized by using an ASAP-2420 N2 physical adsorption-desorption instrument. A small amount of sample was vacuum treated at 300°C for 3-4 hours, and finally the product was placed under liquid nitrogen low temperature (-200°C) for nitrogen adsorption-desorption test. The specific surface area was obtained according to the BET equation, and the pore volume and the distribution rate of pore diameters below 30nm were obtained according to the BJH model.
[0030] Mercury intrusion method: A mercury intrusion instrument was used to characterize the pore diameter distribution of the carriers of the embodiment and the comparative example. The specific operation is as follows: The pore distribution of the sample was characterized using the American Micromeritics AutoPore 9500 fully automatic mercury intrusion instrument. After the sample was dried, it was weighed and loaded into the dilatometer, and degassed for 30 minutes under the vacuum conditions given by the instrument, and then loaded with mercury. The dilatometer was then placed in an autoclave and vented. Then, a pressure increase and pressure reduction test was performed. The mercury contact angle was 130°, and the mercury interfacial tension was 0.485N.cm -1 The distribution rate of pores with a diameter of more than 100 nm is measured by mercury intrusion porosimetry.
[0031] Scanning electron microscopy was used to characterize the microstructure of the sample. The specific operation was as follows: JSM-7500F scanning electron microscope was used to characterize the microstructure of the carrier, with an accelerating voltage of 5 kV, an accelerating current of 20 µA, and a working distance of 8 mm.
[0032] The micro-region composition of the sample was characterized by scanning electron microscope-energy spectrometer. The specific operation was as follows: a JSM-7500F scanning electron microscope equipped with an EDAX energy spectrometer was used, with an accelerating voltage of 30 kV, a probe current of 11µA, and a working distance of 8mm. In the experiment, 20 micro-regions of flaky particles and spherical particles were selected as the measurement areas, and the contents of metal oxides of Group VIB and Group VIII in the corresponding areas were measured and the average values were taken to calculate the D1 and D2 values.
[0033] The molybdenum and nickel content of the catalyst bulk phase was determined according to the method described in the literature ICP-AES determination of the content of metal elements in molybdenum-nickel series hydrogenation catalysts, Guangzhou Chemical Industry, 2021, 49, (17): 129-130.
[0034] The cobalt content in the catalyst bulk phase is determined according to the standard SHT0345-1992-Determination of cobalt content in hydrotreating catalysts.
[0035] The tungsten content in the bulk phase of the catalyst was determined according to the method described in the literature, Determination of tungsten content in hydrogenation catalyst by thiocyanate photometry, Physical and Chemical Testing - Chemical Section, 2003, 39 (1): 51-53.
[0036] The GB / T 34099-2017 standard method was used to determine the Ni and V contents in oil products.
[0037] V+Ni removal rate % = (metal V+Ni content of crude oil - metal V+Ni content of product) / metal V+Ni content of crude oil × 100%.
[0038] Relative demetallization rate: Determine the demetallization rate of a certain catalyst, define its relative demetallization rate as 100%, and the impurity removal rate of other catalysts / defined catalyst impurity removal rate × 100% is the relative deimpurity removal rate.
[0039] Preparation of active metal modified flaky pseudo-boehmite: Example 1
[0040] (1) Weigh an appropriate amount of aluminum nitrate and place it in a crucible and calcine it at 550℃ for 5 hours. Crush and sieve out particles larger than 200 mesh; (2) Weigh an appropriate amount of the above material powder, and supersaturate the powder with Mo-Ni-P impregnation solution with a molybdenum oxide concentration of 3 g / 100 mL and a nickel oxide concentration of 0.8 g / 100 mL for 1 hour. The impregnated material is filtered, dried at 120°C for 6 hours, and calcined at 450°C for 6 hours; (3) Weigh 100 g of the calcined material from step (2) and add propylene oxide at a mass concentration of 5.4% 670 g of aqueous solution was stirred magnetically for 30 minutes, and then the mixture was transferred into an autoclave and sealed and heated at 135°C for 6.5 hours. After cooling, the solid material was filtered, washed, and dried at 120°C for 4 hours to obtain active component modified pseudo-boehmite P1-1. The microstructure of the sample was flaky grain accumulation, the flaky grain size was 150-550nm, and the thickness was 15-30nm. The scanning electron microscope image of the sample is shown in Figure 1 and Figure 2 . Example 2
[0041] The same as Example 1, except that the calcination temperature of aluminum nitrate in step (1) is 500°C and the calcination time is 6 hours. In step (2), the concentration of molybdenum oxide in the active component impregnation solution is 3.5 g / 100 mL, and the concentration of nickel oxide is 0.9 g / 100 mL; the concentration of propylene oxide is 6.5%, the amount of solution is 550 g, the hydrothermal treatment temperature is 145°C, and the treatment time is 5.5 hours, to obtain active component modified pseudo-boehmite P1-2, the microstructure of the sample is flaky grain accumulation, the flaky grain size is 120-540 nm, and the thickness is 15-35 nm. Example 3
[0042] The same as Example 1, except that the calcination temperature of aluminum nitrate in step (1) is 600°C and the calcination time is 4 hours. In step (2), the molybdenum oxide in the active component impregnation solution is replaced by tungsten oxide with a concentration of 2.5 g / 100 mL, and the nickel oxide is replaced by cobalt oxide with a concentration of 0.6 g / 100 mL; the concentration of propylene oxide is 7.5%, the amount of solution is 430 grams, the hydrothermal treatment temperature is 155°C, and the treatment time is 4.5 hours, to obtain active component modified pseudo-boehmite P1-3, the microstructure of the sample is flaky grain accumulation, the flaky grain size is 150-560 nm, and the thickness is 15-35 nm. Example 4
[0043] The same as Example 1, except that the calcination temperature of aluminum nitrate in step (1) is 450°C and the calcination time is 7 hours. In step (2), the concentration of molybdenum oxide in the active component impregnation solution is 1.8 g / 100 mL, and the concentration of nickel oxide is 0.5 g / 100 mL; the concentration of propylene oxide is 4.4%, the amount of solution is 760 g, the hydrothermal treatment temperature is 125°C, and the treatment time is 7.5 hours, to obtain active component modified pseudo-boehmite P1-4, the microstructure of the sample is flaky grain accumulation, the flaky grain size is 120-500 nm, and the thickness is 15-30 nm.
[0044] Comparative Example 1 The same as Example 1, except that the propylene oxide in step (3) was replaced by the same amount of ethylene oxide, no lamellar grains were observed in the microstructure of the material P1-5 after the hydrothermal treatment.
[0045] Comparative Example 2 The same as Example 1, except that the aluminum nitrate in step (1) is replaced by aluminum sulfate, and the solid material particles are dissolved after hydrothermal treatment, and the product is not separated.
[0046] Comparative Example 3 The same as Example 1, except that the aluminum nitrate in step (1) is replaced by aluminum chloride. After the hydrothermal treatment, no lamellar grains are observed in the microstructure of the material P1-6. The scanning electron microscope image of the sample is shown in FIG. Figure 2 .
[0047] Comparative Example 4 The same as Example 1, except that the material powder in step (2) was changed to γ-alumina powder of the same mesh size. The material P1-7 after hydrothermal treatment, the sample scanning electron microscope image is shown in Figure 3 .
[0048] Comparative Example 5 The same as Example 1, except that the hydrothermal treatment time in step (3) was 1.5 hours, and no lamellar grains were observed in the microstructure of the material P1-8 after the hydrothermal treatment.
[0049] Preparation of Hydrodemetallization Catalyst Example 5
[0050] (1) Weigh 100 g of the active metal modified pseudo-boehmite P1-1 prepared in Example 1, 230 g of pseudo-boehmite P2 (produced by Wenzhou Jingjing Alumina Co., Ltd., with pore volume of 10-20 nm accounting for 58% of the total pore volume), and 0.5 g of sesbania powder, mix the above materials evenly, add an appropriate amount of 1% acetic acid aqueous solution for kneading, extrude into strips, dry the shaped material at 140° C. for 6 hours, and calcine the dried material at 550° C. in air for 5 hours to obtain an alumina carrier. A scanning electron microscope equipped with an energy dispersive spectrometer was used to determine the micro-region composition of the flaky grains in the carrier, and the MoO3 content of the micro-region was 3.2%, and the NiO content was 0.9%.
[0051] (2) Weigh 50 g of the above-mentioned alumina carrier and impregnate the alumina carrier with a Mo-Ni-P active component impregnation solution having a molybdenum oxide concentration of 7.2 g / 100 mL and a nickel oxide concentration of 2.1 g / 100 mL by saturated impregnation. The impregnated material is dried at 120° C. for 6 hours and the dried material is calcined in air at 500° C. for 5 hours to obtain a hydrodemetallization catalyst Cat-1. The catalyst properties are shown in Table 1. Example 6
[0052] The same as Example (5), except that the active metal modified pseudo-boehmite P1-1 was replaced by P1-2, and the amount of pseudo-boehmite P2 added was 166 g, to obtain an alumina carrier, in which the MoO3 content in the micro-region of the flaky grains in the alumina carrier was 3.4%, and the NiO content was 1.1%. The hydrodemetallization catalyst Cat-2 was obtained, and the catalyst properties are shown in Table 1. Example 7
[0053] The same as Example (5), except that the active metal modified pseudo-boehmite P1-1 was replaced by P1-3, the amount of pseudo-boehmite P2 added was 125 g, and an alumina carrier was obtained. The WO3 content in the micro-region of the flaky grains in the alumina carrier was 2.6%, and the CoO content was 0.6%. The hydrodemetallization catalyst Cat-3 was obtained, and the catalyst properties are shown in Table 1. Example 8
[0054] The same as Example (5), except that the active metal modified pseudo-boehmite P1-1 was replaced by P1-4, the amount of pseudo-boehmite P2 added was 340 g, and an alumina carrier was obtained. The MoO3 content in the micro-region of the flaky grains in the alumina carrier was 1.9%, and the NiO content was 0.5%. The hydrodemetallization catalyst Cat-4 was obtained, and the catalyst properties are shown in Table 1.
[0055] Comparative Example 4 The same as Example (5), except that the active metal modified pseudo-boehmite P1-1 was replaced by P1-5, and no plate-like crystal micro-regions were found in the carrier, and a comparative hydrodemetallization catalyst Cat-5 was prepared. The catalyst properties are shown in Table 1.
[0056] Comparative Example 5 The same as Example (5), except that the active metal modified pseudo-boehmite P1-1 was replaced by P1-6, and no plate-like crystal micro-regions were found in the carrier, and a comparative hydrodemetallization catalyst Cat-6 was prepared. The catalyst properties are shown in Table 1.
[0057] Comparative Example 6 The same method as in Example (5) was used, except that the active metal-modified pseudo-boehmite P1-1 was replaced with P1-7 to prepare a comparative hydrodemetallization catalyst Cat-7. The catalyst properties are shown in Table 1.
[0058] Comparative Example 7 The same as Example (5), except that the active metal modified pseudo-boehmite P1-1 was replaced by P1-8, and no plate-like crystal micro-regions were found in the carrier, a comparative hydrodemetallization catalyst Cat-6 was prepared, and the catalyst properties are shown in Table 1.
[0059] Table 1 Catalyst properties Example 5 Example 6 Example 7 Example 8 Comparative Example 4 Comparative Example 5 Comparative Example 6 Comparative Example 7 catalyst Cat-1 Cat-2 Cat-3 Cat-4 Cat-5 Cat-6 Cat-7 Cat-8 <![CDATA[Specific surface area, m 2 / g]]> 206 187 165 220 173 158 191 183 Pore volume, mL / g 0.93 0.91 0.88 0.95 0.81 0.79 0.86 0.83 10-20nm pore content, % 53.7 51.4 49.6 56.3 60.4 58.7 50.3 59.7 50-100nm pore content, % 15.6 18.3 22.1 11.7 3.3 4.1 7.3 6.2 D1 1.47 1.49 1.32 1.27 — — 1.46 — D2 1.45 1.54 1.31 1.26 — — 1.44 — <![CDATA[MoO3 content, wt%]]> 8.3 8.6 7.3 7.7 8.4 8.3 8.3 8.4 <![CDATA[WO3 content, wt%]]> — — 1.2 — — — — — NiO content, wt% 2.4 2.6 2.3 2.3 2.5 2.4 2.5 2.4 Co content, wt% — — 0.3 — — — — —
[0060] The catalytic performance of the hydrodemetallization catalysts (Cat-1-Cat-6) prepared in the above examples and comparative examples was evaluated by the following method: Using a certain residual oil as raw material, the metal (Ni+V) content in the raw oil is 179μg / g. The catalytic performance of the hydrodemetallization catalyst Cat-1-Cat-6 was evaluated on a 200mL small evaluation device. The reaction conditions are as follows: reaction temperature 380℃, pressure 14.0MPa, liquid hourly volume space velocity 0.6h -1 The volume ratio of hydrogen to oil was 800. The contents of various impurities in the generated oil were determined after 500 hours and 2000 hours of reaction, and the impurity removal rate was calculated. The evaluation results are shown in Table 2.
[0061] Table 2 Comparison of catalyst hydrogenation performance Catalyst No. Cat-1 Cat-2 Cat-3 Cat-4 Cat-5 Cat-6 Cat-7 Cat-8 500 hours relative demetallization (V+Ni) rate, % 134 137 141 129 100 98 118 112 3000 hours relative demetallization (V+Ni) rate, % 131 138 146 132 100 81 120 119 It can be seen from the data in Table 2 that when the reaction time is 500 hours, the hydrodemetallization catalyst of the present invention has higher activity than the comparative catalyst; when the reaction time is 3000 hours, the hydrodemetallization catalyst prepared by the method of the present invention still has higher activity than the comparative catalyst. This indicates that the catalyst prepared by the method of the present invention has higher hydrodemetallization activity and activity stability.
Claims
1. A heavy oil hydrodemetallization catalyst, characterized in that: It comprises an active metal component and an alumina carrier, wherein the active metal component is a metal of Group VIB and Group VIII, and the alumina carrier comprises flaky alumina grains and granular alumina grains, wherein the mass ratio D of the content of the active metal component at the micro-region of the flaky particles to the active metal component at the micro-region of the spherical particles in terms of oxide is 1.1-1.85, and it is further preferred that the mass ratio D1 of the content of the Group VIB metal oxide at the micro-region of the flaky alumina grains to the Group VIB metal oxide at the micro-region of the granular alumina grains in terms of oxide is 1.25-1.50, and the mass ratio D2 of the Group VIII metal at the flaky alumina grains to the Group VIII metal at the micro-region of the granular alumina grains in terms of oxide is 1.20-1.
55.
2. The heavy oil hydrodemetallization catalyst according to claim 1, characterized in that: The flaky aluminum oxide has a grain size of 100-600 nm and a thickness of 15-40 nm; the granular aluminum oxide has a grain size of 20-100 nm.
3. The heavy oil hydrodemetallization catalyst according to claim 1, characterized in that: Based on the weight of the catalyst, the content of the active metal component in terms of oxide is 8%-20%, and the content of the alumina carrier is 80%-92%; preferably, the content of the VIB group metal in terms of metal oxide is 6.5wt%-12.5wt%, and the content of the VIII group metal in terms of metal oxide is 1.5wt%-4.5wt%; further preferably, the VIB group metal is selected from W and / or Mo, and the VIII group metal is selected from Co and / or Ni.
4. The heavy oil hydrodemetallization catalyst according to claim 1, characterized in that: The specific surface area of the catalyst is 160-240m 2 / g, the pore volume is 0.65-1.1mL / g, and the most probable pore diameters are 10-20nm and 50-100nm, of which pores of 10-20nm account for 40%-60% of the total pore volume, and pores of 50-100nm account for 10%-25% of the total pore volume.
5. A method for preparing the heavy oil hydrodemetallization catalyst according to any one of claims 1 to 4, characterized in that The method comprises the following contents: (1) roasting, crushing and screening aluminum nitrate, impregnating the screened material with an active component impregnation solution, drying and roasting the impregnated material to obtain a modified material; (2) immersing the modified material in a propylene oxide solution for closed heat treatment, drying the treated material to obtain an active metal modified flaky pseudo-boehmite P1; (3) kneading the active metal modified flaky pseudo-boehmite P1 and the pseudo-boehmite P2 in step (2) into a carrier, and then loading the active metal component to obtain a heavy oil hydrogenation demetallization catalyst.
6. The method according to claim 5, characterized in that: The calcination temperature of the aluminum nitrate in step (1) is 450-650° C., the calcination time is 4-8 hours, and the particle size of the material is greater than 100 mesh, preferably greater than 200 mesh.
7. The method according to claim 5, characterized in that: The active component impregnation liquid in step (1) is a solution containing metals of Group VIB and Group VIII, the amount of impregnation liquid is such that the screened material is completely immersed, and the impregnation time is 0.5-2 hours; the drying temperature is 80-140°C, the drying time is 4-10 hours, the calcination temperature is 400-550°C, and the calcination time is 4-10 hours.
8. The method according to claim 5, characterized in that: The concentration of the propylene oxide solution in step (2) is 2.5wt%-12wt%, preferably 4wt%-8wt%, and the mass ratio of the propylene oxide solution to the modified material is 3:1-10:1, preferably 4:1-8:
1.
9. The method according to claim 5, characterized in that: The temperature of the sealed heat treatment in step (2) is 110-180°C, preferably 120-160°C, and the sealed heat treatment time is 4-8 hours. During the sealed heat treatment, the pressure in the sealed container is the autogenous pressure.
10. The method according to claim 5, characterized in that: The pseudo-boehmite P2 in step (3) is a spherical particle, which may be a pseudo-boehmite with a pore size of 10-20 nm, preferably a pseudo-boehmite with a pore volume of 10-20 nm accounting for more than 50% of the total pore volume.
11. The method according to claim 5, characterized in that: The mass ratio of the active metal modified pseudo-boehmite P1 to the pseudo-boehmite P2 in step (3) is 1:4-1:
1.
12. Use of the heavy oil hydrodemetallization catalyst according to any one of claims 1 to 4 in the field of heavy oil hydrogenation.
Citation Information
Patent Citations
Heavy oil hydrogenation catalyst and preparation method thereof
CN106140180A
Preparation method of hydrodemetallization catalyst
CN111774065A
Highly-dispersed particulate catalyst for use in hydrogen peroxide synthesis, preparation method therefor and application thereof
WO2017128946A1
Method for preparing hydrotreating catalyst by impregnation method
WO2018161952A1