Composite material for producing gas-phase silicon and preparation method, device and method thereof

By using a composite material with a core-shell structure, the boron nitride shell is used to protect silicon particles at high temperatures to generate vapor-phase silicon, and the production of vapor-phase silicon is controlled by silicon saturation pressure and temperature, which solves the three major problems in obtaining vapor-phase silicon in the existing technology. , improving the purity of fumed silicon and the stability of products.

CN118771384AActive Publication Date: 2024-10-15ZHUHAI PRINT-RITE NEW MATERIALS CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410894414.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-04
Publication Date
2024-10-15
Estimated Expiration
2044-07-04

AI Technical Summary

Technical Problem

There are three major problems in the acquisition of fumed silicon in the existing technology: after the silicon reaction, there are holes left in the green body, which inhibits densification and sintering; the amount and rate of fumed silicon production cannot be controlled, causing the product to explode; the reaction between fumed silicon and substances lags behind, and it cannot be singled out. Obtain fumed silicon.

Method used

A composite material with a core-shell structure. The core is silicon particles and the outer shell is boron nitride. The boron nitride shell is formed by mixing and baking with boron nitride slurry. The boron nitride shell is heated to 1700~1800°C under vacuum. The rupture generates gas phase silicon, and the silicon saturation pressure and temperature are used to control the production rate of gas phase silicon.

Benefits of technology

It effectively avoids the oxidation of silicon particles, improves the purity of gas phase silicon, avoids cavities in the body and lagging reaction of gas phase silicon, achieves controllability of the amount and rate of gas phase silicon production, and prevents products from exploding.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118771384A_ABST
    Figure CN118771384A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of inorganic non-metallic material equipment, and discloses a composite material for producing gas-phase silicon and a preparation method, device and method thereof, the composite material for producing the gas-phase silicon is of a core-shell structure, the core of the core-shell structure is silicon particles, and the shell of the core-shell structure is a boron nitride shell. The method for producing the gas-phase silicon comprises the following process: heating the composite material for producing the gas-phase silicon to 1700-1800 DEG C in vacuum to generate the boron nitride shell and the gas-phase silicon. In the invention, after the boron nitride shell is broken, the silicon particles are directly gasified to generate the gas-phase silicon, so that the generation rate of the gas-phase silicon can be regulated and controlled by utilizing the positive correlation between the silicon saturation air pressure and the environment temperature, and the problems that the generation amount and the rate of the gas-phase silicon cannot be controlled and the product is exploded due to overlarge amount in the prior art are effectively avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of inorganic non-metallic material equipment, and in particular relates to a composite material for producing gas phase silicon and a preparation method, device and method thereof. Background Art

[0002] Silicon (Si) is an important raw material for synthesizing high-performance non-oxides such as silicon carbide, silicon nitride and sialon, as well as high-purity single crystal silicon and high-purity silicon oxide. It is widely used in photovoltaics, ceramics, glass, refractory materials, semiconductors and other fields. Silicon element has three physical phases: solid phase, liquid phase and gas phase. Compared with solid phase and liquid phase, gas phase silicon has atomic-level activity, lower reaction activation energy, and is easier to react with other substances to generate target products, such as high-purity single crystal silicon, nano-silicon carbide, silicon nitride, silicon carbide or silicon nitride whiskers. Therefore, obtaining gas phase silicon has become a focus of research in various fields.

[0003] At present, there is no effective means to obtain gas phase silicon, and most research focuses on the in-situ reaction of silicon or silicon oxide introduced into the green body with carbon at high temperature. This in-situ reaction method has common defects: (1) After the silicon reacts, cavities are left in the fired green body, inhibiting densification sintering; (2) The amount and rate of gas phase silicon production cannot be controlled, and excessive production will cause the product to explode; (3) Compared with the solid phase and liquid phase, the reaction of gas phase silicon with substances is delayed, and it is impossible to obtain the reaction of gas phase silicon alone. Summary of the invention

[0004] In view of the deficiencies in the above-mentioned prior art, the present invention provides a composite material for producing vapor-phase silicon and a preparation method, device and method thereof, which are used to solve the technical problems commonly existing in the existing in-situ reaction methods: (1) After the silicon reaction, cavities are left in the sintered blank, inhibiting densification sintering; (2) The amount and rate of vapor-phase silicon production cannot be controlled, and excessive production will cause the product to explode; (3) The reaction of vapor-phase silicon with substances is delayed, and it is impossible to obtain a single reaction of vapor-phase silicon.

[0005] The present invention adopts the following technical solutions:

[0006] A composite material for producing gas phase silicon, the composite material for producing gas phase silicon is a core-shell structure, wherein the core of the core-shell structure is silicon particles, and the shell of the core-shell structure is a boron nitride shell.

[0007] Preferably, the size requirement of the silicon particles is as follows: 1.0 mm ≤ D(50) ≤ 1.5 mm.

[0008] Preferably, the thickness d of the boron nitride shell satisfies: 0.05 mm≤d≤0.1 mm.

[0009] The method for preparing the composite material for producing gas phase silicon as described above in the present invention comprises the following steps:

[0010] Mixing silicon particles with boron nitride slurry so that the surface of the silicon particles is coated with a boron nitride slurry layer to obtain silicon particles W2;

[0011] The silicon particles W2 are baked to remove the free water in the boron nitride slurry and gel-bond the silicon particles to obtain the composite material for producing gas-phase silicon.

[0012] Preferably, the method for preparing the boron nitride slurry comprises:

[0013] A polyvinyl alcohol aqueous solution with a mass concentration of 30%-40% is mixed with boron nitride powder to obtain the boron nitride slurry. The mass ratio of the polyvinyl alcohol aqueous solution to the boron nitride powder is (4-6): (6-4).

[0014] Preferably, silicon particles are mixed with boron nitride slurry to coat the surface of the silicon particles with a silicon nitride slurry layer, and then the silicon particles are immersed in the boron nitride slurry for 5-10 minutes to obtain silicon particles W2, wherein the mass ratio of silicon particles to boron nitride slurry does not exceed 2:3.

[0015] Preferably, when the silicon particles W2 are baked, the silicon particles W2 are baked at 150-200° C. for 4-8 hours.

[0016] The present invention also provides a method for producing gas phase silicon, comprising the following process:

[0017] The composite material for producing gas phase silicon of the present invention as described above is heated to 1700-1800° C. under vacuum to produce a boron nitride shell and gas phase silicon.

[0018] Preferably, before the gas phase silicon is generated, the vacuum degree P satisfies: P≤100Pa;

[0019] During the process of producing vapor phase silicon, the positive correlation between silicon saturation pressure and temperature is used to regulate the production rate of vapor phase silicon.

[0020] The present invention also provides an apparatus for producing vapor-phase silicon, which is used to implement the method of the present invention as described above. The apparatus includes a supporting box, a silicon source box and a carrier box. The supporting box has an opening at the top, and a plurality of silicon source boxes are arranged in the inner cavity of the supporting box. The silicon source box has an opening at the top, and the inner cavity of the silicon source box is used to place the composite material for producing vapor-phase silicon as described above in the present invention. The carrier box is arranged at the opening of the supporting box, and a through hole is opened on the carrier box that penetrates the thickness thereof, and the through hole serves as a channel for the vapor-phase silicon to rise. The upper surface of the carrier box can reflect the product.

[0021] Compared with the prior art, the present invention has at least the following beneficial effects:

[0022] The composite material for producing gas-phase silicon of the present invention adopts a core-shell structure, wherein the core of the core-shell structure is silicon particles, and the shell of the core-shell structure adopts a boron nitride shell. When producing gas-phase silicon, the boron nitride shell begins to break after the target temperature, and the target temperature is higher than the gasification temperature of silicon. Therefore, before the boron nitride shell breaks, the silicon particles are well protected to prevent the silicon particles from being oxidized, so the obtained gas-phase silicon has a high purity. Therefore, the present invention avoids the problem of delayed reaction between gas-phase silicon and substances and inability to obtain a single reaction of gas-phase silicon in the prior art; and the present invention does not require in-situ reaction to generate gas-phase silicon, thereby avoiding the problem of leaving cavities in the sintered blank after the silicon reaction and inhibiting densification sintering in the prior art; in the present invention, since the silicon particles are directly gasified to generate gas-phase silicon after the boron nitride shell breaks, the positive correlation between the saturated gas pressure of silicon and the ambient temperature can be used to regulate the generation rate of gas-phase silicon, so the present invention effectively avoids the problem of uncontrollable generation amount and rate of gas-phase silicon in the prior art, and excessive generation will cause product explosion. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 A schematic diagram of the structure of a device for producing vapor phase silicon provided in an embodiment of the present invention;

[0024] Figure 2 This is a typical microstructure diagram of the composite material (i.e., boron nitride (BN) coated silicon particles) when reacted at 1700° C. in Example 1 of the present invention;

[0025] Figure 3 This is a typical microstructure diagram of the composite material (i.e., boron nitride (BN) coated silicon particles) when reacted at 1750° C. in Example 2 of the present invention;

[0026] Figure 4 This is a typical microstructure diagram of the composite material (i.e., boron nitride (BN) coated silicon particles) when reacting at 1800° C. in Example 3 of the present invention.

[0027] Among them, 1-support box; 2-silicon source box; 3-carrying box; 4-through hole; 5-silicon core; 6-boron nitride shell; 7-reaction product. DETAILED DESCRIPTION

[0028] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments.

[0029] like Figure 1As shown, the device for producing vapor-phase silicon of the present invention comprises a supporting box 1, a silicon source box 2 and a carrier box 3. The supporting box 1 is opened at the top, and the inner cavity of the supporting box 1 is provided with a plurality of the silicon source boxes 2. The silicon source box 2 is opened at the top, and the inner cavity of the silicon source box 2 is used to place the composite material for producing vapor-phase silicon of the present invention as described above. The carrier box 3 is arranged at the opening of the supporting box 1, and a through hole 4 penetrating the thickness thereof is opened on the carrier box 3, and the through hole 4 serves as a channel for the vapor-phase silicon to rise. The upper surface of the carrier box 3 can react with the product 7.

[0030] In the above solution of the present invention, the material of the support box 1 is graphite material, the carbon content w(C)>99%, the density 1.8≤ρ≤2.1g / cm 3 The material of the carrier box 3 and the silicon source box 2 is graphite, with a carbon content w(C) ≥ 99.5% and a density of 2.0 ≤ ρ ≤ 2.2 g / cm 3 The carrier box 3 is a plate-shaped through-hole structure, and a plurality of through holes 4 evenly distributed vertically may be provided on the carrier box 3, and the diameter d of the through holes 4 satisfies: 2mm≤d≤5mm.

[0031] The composite material used for producing gas phase silicon of the present invention is a core-shell structure, wherein the core of the core-shell structure is silicon particles, and the shell of the core-shell structure is a boron nitride shell. The particle size D(50) of the silicon core satisfies: 1.0mm≤D(50)≤1.5mm, the thickness d of the boron nitride shell satisfies: 0.05mm≤d≤0.1mm; the silicon content satisfies: w(Si)≥99.0%; and the boron nitride content satisfies: w(BN≥99.2%.

[0032] The method for preparing the composite material comprises the following steps:

[0033] S1, preparing polyvinyl alcohol with a concentration of 30%-40% and boron nitride powder in a mass ratio of (4-6): (6-4) to obtain boron nitride slurry W1;

[0034] S2, placing silicon particles with a size of 1.0 mm ≤ D (50) ≤ 1.5 mm in the boron nitride slurry W1, and soaking for 5-10 minutes; wherein the mass ratio of silicon particles to boron nitride slurry W1 does not exceed 2:3, and silicon particles W2 are obtained after soaking;

[0035] S3 and silicon particles W2 are placed in an oven and baked for 4 to 8 hours at a temperature set at 150 to 200° C. After baking, silicon particles W3 are obtained. Silicon particles W3 are the composite material for producing gas-phase silicon of the present invention.

[0036] The method for producing gas phase silicon using the above device and composite material comprises the following process:

[0037] Place silicon particles W3 in the silicon source box 2, place the silicon source box 2 into the support box 1 and assemble the cargo box 3;

[0038] The production device of vapor silicon is placed in a vacuum furnace, and after evacuating to less than 100Pa, the temperature is raised to the target temperature of 1700℃≤T≤1800℃, the boron nitride core-shell is broken, and vapor silicon is generated and diffused through the pore structure of the carrier to the surrounding of the product to react.

[0039] During the process of producing vapor phase silicon, the positive correlation between silicon saturation pressure and temperature is used to regulate the production rate of vapor phase silicon.

[0040] In the technical solution provided by the present invention, boron nitride is used as a carrier device for the silicon source, so that gas-phase silicon can be stably generated at high temperature, and the generation rate can be regulated by utilizing the positive correlation between the silicon saturation pressure and the ambient temperature; after the gas-phase silicon is generated, it stably diffuses into the carrier box, contacts and reacts with the product to be reacted, and avoids the hole structure after the silicon in-situ reaction and the delayed reaction of the gas-phase silicon, so as to meet the design requirements of the reaction product.

[0041] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. The components of the embodiments of the present invention described and shown in the drawings here can usually be arranged and designed in various different configurations. Therefore, the following detailed description of the embodiments of the present invention provided in the drawings is not intended to limit the scope of the claimed invention, but merely represents selected embodiments of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0042] Example 1

[0043] The method for producing gas phase silicon in this embodiment comprises the following steps:

[0044] S1, preparing polyvinyl alcohol with a concentration of 30% and boron nitride powder in a mass ratio of 4:6 to obtain boron nitride slurry W1;

[0045] S2, placing silicon particles with a size of D(50)=1.5 mm in the boron nitride slurry W1 and soaking for 10 minutes; wherein the mass ratio of silicon particles to boron nitride slurry W1 is 1:3, and silicon particles W2 are obtained after soaking;

[0046] S3, silicon particles W2 are placed in an oven and baked for 4 hours at a temperature set at 150°C. After baking, silicon particles W3 are obtained;

[0047] S4, placing silicon particles W3 in a silicon source cartridge, then placing the silicon source cartridge into a support cartridge and assembling a cargo cartridge to form a vapor phase silicon production device;

[0048] S5. Place the gas phase silicon production device in a vacuum furnace, evacuate to 90Pa and then heat to the target temperature of 1700°C. The boron nitride core-shell is broken, and gas phase silicon is generated and diffuses through the pore structure of the carrier to the surrounding of the product to react.

[0049] from Figure 2 It can be seen that when the composite material of this embodiment produces vapor-phase silicon, silicon undergoes a gasification reaction and leaves a hollow structure on the boron nitride shell.

[0050] Example 2

[0051] The method for producing gas phase silicon in this embodiment comprises the following steps:

[0052] S1, preparing polyvinyl alcohol with a concentration of 38% and boron nitride powder in a mass ratio of 5:5 to obtain boron nitride slurry W1;

[0053] S2, placing silicon particles with a size of D(50)=1.3 mm in the boron nitride slurry W1 and soaking for 10 minutes; wherein the mass ratio of silicon particles to boron nitride slurry W1 is 2:3, and silicon particles W2 are obtained after soaking;

[0054] S3, silicon particles W2 are placed in an oven and baked for 6 hours at a temperature set at 200°C. After baking, silicon particles W3 are obtained;

[0055] S4, placing silicon particles W3 in a silicon source cartridge, then placing the silicon source cartridge into a support cartridge and assembling a cargo cartridge to form a vapor phase silicon production device;

[0056] S5. Place the gas phase silicon production device in a vacuum furnace, evacuate to 90Pa and then heat to the target temperature of 1750°C. The boron nitride core-shell is broken, and gas phase silicon is generated and diffuses through the pore structure of the carrier to the surrounding of the product to react.

[0057] from Figure 3 It can be seen that when the composite material of this embodiment produces vapor-phase silicon, silicon undergoes a gasification reaction and leaves a hollow structure on the boron nitride shell.

[0058] Example 3

[0059] The method for producing gas phase silicon in this embodiment comprises the following steps:

[0060] S1, preparing polyvinyl alcohol with a concentration of 40% and boron nitride powder in a mass ratio of 6:4 to obtain boron nitride slurry W1;

[0061] S2, placing silicon particles with a size of D(50)=1.0 mm in the boron nitride slurry W1 and soaking them for 10 minutes; wherein the mass ratio of silicon particles to boron nitride slurry W1 is 1.5:3, and silicon particles W2 are obtained after soaking;

[0062] S3, silicon particles W2 are placed in an oven and baked for 8 hours at a temperature set at 160°C. After the baking is completed, silicon particles W3 are obtained;

[0063] S4, placing silicon particles W3 in a silicon source cartridge, then placing the silicon source cartridge into a support cartridge and assembling a cargo cartridge to form a vapor phase silicon production device;

[0064] S5. Place the gas phase silicon production device in a vacuum furnace, evacuate to 90Pa and then heat to the target temperature of 1800°C. The boron nitride core-shell is broken, and gas phase silicon is generated and diffuses through the pore structure of the carrier to the surrounding of the product to react.

[0065] from Figure 4 It can be seen that when the composite material of this embodiment produces vapor-phase silicon, silicon undergoes a gasification reaction and leaves a hollow structure on the boron nitride shell.

Claims

1. A composite material for producing fumed silicon, It is characterized in that The composite material for producing gas phase silicon is a core-shell structure, wherein the core of the core-shell structure is silicon particles, and the outer shell of the core-shell structure is a boron nitride outer shell.

2. The composite material for producing fumed silicon according to claim 1, It is characterized in that The size requirements of the silicon particles are as follows: 1.0 mm ≤ D(50) ≤ 1.5 mm.

3. The composite material for producing fumed silicon according to claim 1, It is characterized in that The thickness d of the boron nitride shell satisfies: 0.05mm≤d≤0.1mm.

4. The method for preparing a composite material for producing fumed silicon according to any one of claims 1 to 3, It is characterized in that The process includes the following: Mixing silicon particles with boron nitride slurry so that the surface of the silicon particles is coated with a boron nitride slurry layer to obtain silicon particles W2; The silicon particles W2 are baked to remove the free water in the boron nitride slurry and gel-bond the silicon particles to obtain the composite material for producing gas-phase silicon.

5. The method for preparing a composite material for producing fumed silicon according to claim 4, It is characterized in that The preparation method of the boron nitride slurry comprises: A polyvinyl alcohol aqueous solution with a mass concentration of 30%-40% is mixed with boron nitride powder to obtain the boron nitride slurry. The mass ratio of the polyvinyl alcohol aqueous solution to the boron nitride powder is (4-6): (6-4).

6. The method for preparing a composite material for producing fumed silicon according to claim 4, It is characterized in that The silicon particles are mixed with the boron nitride slurry to coat the surface of the silicon particles with the silicon nitride slurry layer, and then the silicon particles are immersed in the boron nitride slurry for 5-10 minutes to obtain silicon particles W2, wherein the mass ratio of the silicon particles to the boron nitride slurry does not exceed 2:

3.

7. The method for preparing a composite material for producing fumed silicon according to claim 5, It is characterized in that When the silicon particles W2 are baked, the silicon particles W2 are baked at 150 to 200° C. for 4 to 8 hours.

8. A method for producing gas phase silicon, It is characterized in that The process includes the following: The composite material for producing gas phase silicon according to any one of claims 1 to 3 is heated to 1700-1800° C. under vacuum to produce a boron nitride shell and gas phase silicon.

9. The method for producing vapor phase silicon according to claim 8, It is characterized in that Before the gas phase silicon is generated, the vacuum degree P satisfies: P≤100Pa; During the process of producing vapor phase silicon, the positive correlation between silicon saturation pressure and temperature is used to regulate the production rate of vapor phase silicon.

10. Apparatus for producing vapor phase silicon, It is characterized in that The device is used to implement the method described in claim 8 or 9, comprising a support box (1), a silicon source box (2) and a carrier box (3), wherein the support box (1) is open at the top, and a plurality of silicon source boxes (2) are arranged in the inner cavity of the support box (1), wherein the silicon source box (2) is open at the top, and the inner cavity of the silicon source box (2) is used to place the composite material for producing gas phase silicon described in any one of claims 1 to 3, and the carrier box (3) is arranged at the opening of the support box (1), and a through hole (4) penetrating the thickness of the carrier box (3) is opened, and the through hole (4) serves as a passage for the gas phase silicon to rise, and the upper surface of the carrier box (3) can react with the product (7).

Citation Information

Patent Citations

  • Fluidized-bed reactor for producing chlorosilanes

    CN107250039A

  • High volume fraction SiC / Cu particle reinforced Al-based metal composite material and preparation method thereof

    CN111172433A

  • Preparation method and application of boron nitride material with core-shell structure

    CN115093608A

  • BORON DOPED CARBON-SILICON OXIDE(C-SiOx) ANODE MATERIAL FOR LI-ION BATTERIES, AND METHOD FOR PREPARING THE SAME

    KR1020180092532A