Recycled cement-based composite material added with waste concrete and preparation method of recycled cement-based composite material
Waste concrete is processed through thermal activation and alkali excitation technology to prepare efficient recycled cement-based composite materials, which solves the problems of high energy consumption and insufficient mechanical properties in the existing technology, and realizes the effective application of high-content recycled cement and the improvement of material properties. .
Patent Information
- Application Number
- CN202410845393.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-15
AI Technical Summary
In the existing technology, the preparation process of recycled cement from waste concrete consumes high energy and has insufficient mechanical properties, making it difficult to effectively replace ordinary cement.
Thermal activation treatment and alkali excitation technology are used to prepare regenerated cement-based composite materials. By heating the waste concrete powder to 750°C for thermal activation, combined with nano-silica treatment, an efficient cement gel system is formed to improve the mechanical properties of the material.
It simplifies the preparation process of recycled cement, reduces energy consumption, improves the compressive flexural strength and setting time of the material, ensures the comprehensive performance of the material, and realizes the application of high-content recycled cement.
Smart Images

Figure CN118771797A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of recycled building material processing, and in particular to a recycled cement-based composite material added with waste concrete and a preparation method thereof. Background Art
[0002] Concrete production is one of the important sources of environmental problems because it may involve large-scale extraction of raw materials, consumption of non-renewable energy and excessive emission of greenhouse gases. At present, construction waste accounts for about half of the entire industrial waste. Reusing waste concrete can effectively reduce the demand for raw materials and reduce energy consumption. In addition, ordinary Portland cement accounts for 80-90% of CO2 emissions in concrete production and more than 5% of annual CO2 production. Among them, nearly 83.1% of emissions are due to the sintering process and about 60% are due to the decarbonization of limestone. Therefore, recycling waste concrete also helps to reduce the consumption of construction waste and natural resources, reduce carbon emissions and achieve sustainable development.
[0003] At present, the recycling of waste concrete is mainly used as recycled coarse aggregate (admixture), but the use of it as an admixture is limited and still cannot fundamentally solve the problem. Recycled cement is a solution with great potential for the recycling of waste concrete. For example, the patent application document with application publication number CN113754324A discloses a method for preparing recycled cement based on high temperature and carbonization coupling. The technology includes grinding, high temperature carbonization coupling treatment and drying treatment, and has a good carbon fixation effect. However, its preparation process is relatively complicated. After grinding, it is necessary to perform ball milling under an environment of 400℃~600℃ to achieve mortar separation, and then cool to below 100℃ for fan screening. After screening, it is necessary to perform grinding treatment and high temperature carbonization coupling treatment again. The conditions for high temperature carbonization coupling treatment are: in the presence of water and carbon dioxide, high temperature carbonization coupling treatment is performed in the form of powder raising, and the high temperature temperature is 400℃~650℃. After high temperature carbonization coupling treatment, the high temperature temperature must be maintained continuously for drying. After drying, it is cooled to below 100℃ and then ground again. In terms of energy consumption, this technology requires two heating and cooling operations and three grinding times, which consumes a lot of energy and it is difficult to form an advantage in regeneration costs. Further improvement is needed. Summary of the invention
[0004] The invention prepares a recycled cement-based composite material with waste concrete added by a specific method to solve the technical problem of high energy consumption in the prior art.
[0005] The technical solution adopted by the present invention is as follows:
[0006] A recycled cement-based composite material with waste concrete added, comprising a cement gel system, water, a water reducing agent and aggregates, wherein the cement gel system is composed of 70% by mass of cement and 30% by mass of heat-activated cement powder, and the preparation process of the recycled cement-based composite material is as follows:
[0007] (1) preparing waste concrete into waste concrete powder;
[0008] (2) subjecting the waste concrete powder to thermal activation treatment, wherein the thermal activation treatment process is as follows: subjecting the waste concrete powder to thermal activation treatment, wherein the thermal activation treatment process is as follows: heating the waste concrete powder to 750° C., maintaining the heating for 3 hours, and finally cooling the waste concrete powder to room temperature to obtain thermally activated cement powder for standby use;
[0009] (3) mixing cement, heat-activated cement powder, water, a water reducing agent and aggregate to obtain a recycled cement-based mixture;
[0010] (4) Alkali activation: adding 2-8% of water glass by weight of the cement gel system to the recycled cement-based mixture, and mixing and stirring to obtain an alkali-activated system;
[0011] (5) Add 1-5% of the mass of the cement gel system of nano-silicon dioxide into the alkali-activated system and stir evenly to obtain a recycled cement-based composite material.
[0012] Preferably, the aggregate is sand, and the weight proportions of cement gel system, water, water reducer and aggregate are respectively: 100 parts of cement gel system, 66 parts of water, 0.1 parts of water reducer and 300 parts of sand.
[0013] Preferably, the water reducer is a polycarboxylate water reducer.
[0014] Preferably, the process of preparing waste concrete into waste concrete powder is as follows: first, the waste concrete is crushed by a jaw crusher to obtain primary crushed powder with a particle size not greater than 8 mm; then, the waste concrete is further ground by a roller crusher to a grinding powder with a particle size less than 2 mm; finally, a disc crusher is used for secondary grinding to obtain waste concrete powder with a particle size less than 75 μm.
[0015] Preferably, the modulus of the water glass is 1.5.
[0016] The method for preparing the recycled cement-based composite material by adding waste concrete comprises the following steps:
[0017] (1) preparing waste concrete into waste concrete powder;
[0018] (2) subjecting the waste concrete powder to thermal activation treatment, wherein the thermal activation treatment process is as follows: subjecting the waste concrete powder to thermal activation treatment, wherein the thermal activation treatment process is as follows: heating the waste concrete powder to 750° C., maintaining the heating for 3 hours, and finally cooling the waste concrete powder to room temperature to obtain thermally activated cement powder for standby use;
[0019] (3) mixing cement, heat-activated cement powder, water, a water reducing agent and aggregate to obtain a recycled cement-based mixture;
[0020] (4) Alkali activation: adding water glass to the recycled cement-based mixture in terms of Na2O equivalent, and mixing and stirring to obtain an alkali activation system;
[0021] (5) Add nano-silicon dioxide to the alkali-activated system and stir evenly to obtain a recycled cement-based composite material. In summary, compared with the prior art, the present invention has the following advantages and beneficial effects:
[0022] 1. The recycled cement-based composite material provided by the present invention, wherein the regeneration process of the recycled cement includes micro-powder preparation, thermal activation, alkali excitation and nano-silica treatment process, which promotes the formation of ettringite and hydrated calcium silicate in the recycled cement and improves the mechanical properties of the material, thereby making it possible to add a high content of recycled cement to the cementitious material. Compared with the cement regeneration process in the prior art, the crushing process and the heating process are each concentrated, the process is simpler and the energy consumption is lower;
[0023] 2. The present invention comprehensively considers the compressive and flexural strength, setting time and density of the material, and controls the replacement rate of recycled cement in the gel material to more than 30%, so that the recycled cement-based composite material not only has good mechanical properties, but also has good working performance, ensuring the comprehensive performance of the material;
[0024] 3. The present invention uses recycled cement as a cementitious material to replace part of the cement, which not only reduces the amount of cement used and saves cement resources, but also provides a new application path for the reuse of waste concrete, and adds alkali activators, nano-silicon dioxide and other materials to improve the material performance;
[0025] 4. The present invention strictly controls various parameters of recycled cement so that the prepared recycled cement-based composite material has good mechanical properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 The compressive strength and flexural strength diagrams of recycled cement-based composite material specimens prepared at different recycled cement replacement rates in Comparative Example 1 and Examples 1-3;
[0027] Figure 2 It is a hardening density diagram of recycled cement-based composite material specimens prepared at different recycled cement replacement rates in Comparative Example 1 and Examples 1-3;
[0028] Figure 3 The compressive strength and flexural strength diagrams of recycled cement-based composite material specimens prepared from recycled cement at different thermal activation temperatures in Comparative Example 2 and Examples 4-7;
[0029] Figure 4 It is the setting time influence diagram of the recycled cement-based composite material specimens prepared by recycled cement with different thermal activation temperatures in Comparative Examples 1-2 and Examples 4-7;
[0030] Figure 5 The influence diagram of the standard consistency water consumption of the recycled cement-based composite material specimens prepared by recycled cement with different thermal activation temperatures in Comparative Example 2 and Examples 4-7;
[0031] Figure 6 The compressive strength and flexural strength diagrams of the alkali-activated thermally activated regenerated cement-based composite material specimens under different Na2O equivalents in Comparative Example 3 and Examples 8-11;
[0032] Figure 7 Graphs showing the compressive strength and flexural strength of nano-modified alkali-activated thermally activated regenerated cement-based composite material specimens at different nano-silica contents in Comparative Example 4 and Examples 12-15. DETAILED DESCRIPTION
[0033] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with various embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention, that is, the embodiments described are only part of the embodiments of the present invention, rather than all of the embodiments.
[0034] The word "embodiment" used here as an "exemplary" does not necessarily mean that any embodiment described is superior to or better than other embodiments. Unless otherwise specified, the performance index tests in the embodiments of this method adopt conventional test methods in the art. The terms described in the present invention are only for describing specific implementation methods and are not intended to limit the content disclosed in the present invention.
[0035] Unless otherwise specified, the technical and scientific terms used herein have the same meanings as commonly understood by ordinary technicians in the technical field to which the invention belongs; other raw materials, reagents, experimental methods and technical means not specifically specified in the present invention refer to the raw materials and reagents commonly used by ordinary technicians in the field, as well as the commonly used experimental methods and technical means.
[0036] The various materials involved in the various embodiments of the present invention are as follows:
[0037] Cement is ordinary Portland cement PO42.5;
[0038] The sand is natural river sand;
[0039] The water reducing agent is polycarboxylate water reducing agent, and the water reduction rate of mortar is 45%;
[0040] The alkaline activator is water glass with a modulus of 1.5, and its dosage is calculated based on the Na2O equivalent;
[0041] Nano-silicon dioxide;
[0042] The water is tap water;
[0043] Waste concrete is provided by Zhengzhou Dingsheng Enterprise Group Co., Ltd.
[0044] The waste concrete was crushed by jaw crusher to a particle size of d≤8mm. Then, it was further ground in roller crusher to a particle size of d<2mm. Then, it was ground again by disc crusher for about 3h. The fine powder with a particle size of d<75μm was obtained, which was waste concrete fine powder. Its chemical composition is shown in Table 1.
[0045] Before use, the waste concrete powder is heat treated in a muffle furnace heating device, with the target temperature set at 750°C and the heating rate at 10°C / min to the target temperature. The temperature is kept for 3 hours and then naturally cooled to room temperature in the kiln.
[0046] Table 1
[0047] Element CaO <![CDATA[SiO2]]> <![CDATA[Al2O3]]> <![CDATA[Fe2O3]]> MgO <![CDATA[SO3]]> <![CDATA[K2O]]> <![CDATA[TiO2]]> <![CDATA[Na2O]]> <![CDATA[P2O5]]> content / % 56.992 21.495 6.985 3.278 8.137 0.737 1.195 0.378 0.444 0.079
[0048] The preparation method of the recycled cement-based composite material of the present invention comprises the following steps:
[0049] (1) preparing waste concrete into waste concrete powder;
[0050] (2) subjecting the waste concrete powder to thermal activation treatment, wherein the thermal activation treatment process is as follows: subjecting the waste concrete powder to thermal activation treatment, wherein the thermal activation treatment process is as follows: heating the waste concrete powder to 750° C., maintaining the heating for 3 hours, and finally cooling the waste concrete powder to room temperature to obtain thermally activated cement powder for standby use;
[0051] (3) mixing cement, heat-activated cement powder, water, a water reducing agent and aggregate to obtain a recycled cement-based mixture;
[0052] (4) Alkali activation: adding 2-8% of water glass by weight of the cement gel system to the recycled cement-based mixture, calculated as Na2O equivalent, and mixing and stirring to obtain an alkali-activated system;
[0053] (5) Add 1-5% of the mass of the cement gel system of nano-silicon dioxide into the alkali-activated system and stir evenly to obtain a recycled cement-based composite material.
[0054] The present invention relates to a composite material physical and mechanical properties test method comprising:
[0055] (1) Compressive strength and flexural strength test: According to GB / T 17671-2021, the 40×40×160 mm prism specimens of cement mortar standard specimens were compacted. The compressive and flexural strengths were measured at 1d, 3d, 7d, and 28d, respectively.
[0056] (2) Determination of water consumption and setting time for standard consistency: The water consumption and setting time of cement are tested in accordance with the national standard GB / T1346-2011.
[0057] (3) Hardening density test: The hardening density test of cement shall comply with GB / T 208-2014 “Determination and method of cement density”.
[0058] 1. Experiment on the influence of thermally activated recycled cement replacement rate on the mechanical properties and hardened density of cementitious materials (Comparative Example 1 and Examples 1-3)
[0059] The recycled cement-based composite material prepared in this experiment is composed of the following raw materials in parts by weight:
[0060] Cement binder: 100 parts;
[0061] Water reducing agent: 0.1 part;
[0062] Sand: 300 parts;
[0063] Water: 66 parts.
[0064] The composition of cementitious materials is shown in Table 2.
[0065] Table 2
[0066]
[0067] like Figure 1 , Figure 2 As shown in the figure, the effect of recycled cement replacement rate in cementitious materials on the performance of cement-based cementitious materials:
[0068] (1) Compressive strength and flexural strength: Figure 1From the comparison between comparative example 1 and examples 1-3, it can be seen that as the replacement rate of recycled cement gradually increases, the mechanical strength decreases. The compressive strength of the recycled cement with an incorporation rate of 10%, 30% and 50% in examples 1-3 was 40.7%, 39.31% and 70.88% lower than that of the ordinary cement in the control group comparative example 1 at 28 days. This is because after the addition of recycled cement, the overall gelling property of the cementitious material is reduced, resulting in a decrease in the compressive strength of the cement-based material test block. It was also found that the recycled cement with a replacement rate of 30% in example 2 had the slowest decrease in compressive strength at the later 28 days, and the compressive strength was greater than that of the recycled cement with a replacement rate of 10% in example 1. This shows that recycled cement has a potential contribution to filler and nucleation effects.
[0069] (2) Hardening density: Figure 2 From the comparison between Comparative Example 1 and Examples 1-3, it can be seen that different substitution rates also have a certain influence on the hardened density of recycled cement, and its density shows an overall downward trend, but the influence of recycled cement with different substitution rates on the hardened density after thermal activation is relatively small, among which the ratios of the hardened density of Examples 1-3 to that of Comparative Example 1 are 98.47%, 96.96% and 96.25%, that is, the change is no more than 10%.
[0070] 2. Experiment on the influence of heat-activated cement powder at different activation temperatures on the physical and mechanical properties of cement-based materials (Comparative Example 2 and Examples 4-7)
[0071] The recycled cement-based composite material prepared in this experiment is composed of the following raw materials in parts by weight:
[0072] Cement binder: 100 parts, of which 70 parts are cement and 30 parts are heat-activated cement powder;
[0073] Water reducing agent: 0.1 part;
[0074] Sand: 300 parts;
[0075] Water: 66 parts.
[0076] The thermal activation temperatures of Comparative Example 2 and Examples 4-7 during the preparation of recycled cement are shown in Table 3.
[0077] Table 3
[0078] sample Activation temperature(℃) Comparative Example 2 25 Example 4 120 Example 5 450 Example 6 750 Example 7 1000
[0079] like Figures 3 to 5 The following are the results of the effects of different thermal activation temperatures on the physical and mechanical properties of recycled cement-based composites:
[0080] (1) Compressive strength and flexural strength: Figure 3As shown, compared with the ordinary Portland cement in Comparative Example 1, the mechanical properties of the recycled cement are significantly reduced. And with the increase of thermal activation temperature, the flexural strength and compressive strength first increase and then decrease. Among them, the best compressive strength performance appears in the recycled cement mortar with a thermal activation temperature of 750°C in Example 6, indicating that the temperature at 750°C enhances the rehydration ability of the recycled cement, and the compressive strength at 3d and 28d reaches 11.52MPa and 19.45MPa respectively. The compressive strength of the recycled cement in Example 6 at 28d is equivalent to 60.69% of the compressive strength of the ordinary Portland cement in Comparative Example 1. The flexural strength also shows the same trend, and it is found that the flexural strength of the recycled cement at 750°C in Example 6 is equivalent to that of the ordinary Portland cement in Comparative Example 1 at the later 28d.
[0081] In addition, from the data comparison of Example 4, Example 5, and Example 7, it is found that the compressive strength of Examples 4, 5, and 7, which use temperatures of 120, 450, and 1000° C., respectively, is increased by 36.28%, 39.85%, and 50.42% compared to the unheated Comparative Example 2.
[0082] (2) Coagulation time: from Figure 4 It can be seen from Comparative Examples 1-2 and Examples 4-7 that with the increase of thermal activation temperature, the setting time of recycled cement first decreases and then increases. When the thermal activation temperature of Example 6 reaches 750°C, the setting time at this temperature is the shortest, indicating that the early hydration rate at this temperature is faster, which corresponds to the compressive strength results.
[0083] However, the initial setting time and final setting time in Example 7 are approximately 3.7 times and 1.42 times those in Example 6. In contrast, the setting time of the unheated comparative example 2 is longer, indicating that the hydration rate of the unheated recycled cement is slower. The setting time of Examples 4-5 increases with increasing temperature.
[0084] (3) Standard consistency water consumption: Figure 5 It can be seen from Comparative Examples 1-2 and Examples 4-7 that as the temperature increases, the amount of water required to reach the standard consistency of cement paste increases. Among them, the standard consistency water required for Example 7 is 2.25 times that of ordinary cement in Example 1. Examples 4-7 are 16.67%, 33.33%, 100%, and 140% higher than the standard consistency water used in Comparative Example 2, respectively. The rheological characteristics of cement paste can be regulated by the use of high-efficiency water reducers. Compared with ordinary cement, recycled cement requires more than twice the water to achieve the same consistency.
[0085] 3. Experiment on the influence of alkali-activated thermally activated recycled cement-based composite materials on mechanical properties under different Na2O equivalents (Comparative Example 3 and Examples 8-11).
[0086] The recycled cement-based composite material prepared in this experiment is composed of the following raw materials in parts by weight:
[0087] Cementitious material: 100 parts, of which 70 parts are cement and 30 parts are heat-activated cement powder (activation temperature 750°C);
[0088] Water reducing agent: 0.1 part;
[0089] Water glass: The modulus is 1.5, and the proportion range is 2-8% of the cementitious material calculated as Na2O equivalent; wherein the preparation method of water glass with a modulus of 1.5 mainly includes: sodium hydroxide, sodium silicate and water are prepared in a certain proportion. The sodium hydroxide is analytically pure, and industrial pure water glass (3.29M) is selected, and its solid content is 34.15% (Na2O=8.15%, SiO2=26%). Add analytically pure sodium hydroxide to the sodium silicate solution, and stir continuously during the addition process until the solid sodium hydroxide is dissolved. Place the prepared sodium silicate solution with the required modulus of 1.5 in a beaker and cool for 24 hours for use.
[0090] Sand: 300 parts;
[0091] Water: 66 parts;
[0092] The different Na2O equivalents in Comparative Example 3 (equivalent to Example 6) and Examples 8-11 when preparing recycled cement-based composite materials are shown in Table 4.
[0093] Table 4
[0094] <![CDATA[Na2O equivalent (%)]]> Comparative Example 3 0 Example 8 2 Example 9 4 Example 10 6 Embodiment 11 8
[0095] like Figure 6 As shown, the mechanical properties of alkali-activated thermally activated recycled cement-based composites under different Na2O equivalents are affected:
[0096] from Figure 6 It can be seen from Comparative Example 3 and Examples 8-11 that as the curing age increases, the compressive strength and flexural strength also gradually increase, which indicates that the alkali-induced thermal activation of the regenerated cement hydration reaction continues. For example, the compressive strength of Examples 8-11 at 28d increased by 36.92%, 25.51%, 40.45%, and 3.02% respectively compared with 1d. For specimens under the same water glass modulus, the compressive strength and flexural strength at each age showed a trend of first increasing and then decreasing with the increase of Na2O content. Among them, when the Na2O content in Example 10 is 6%, the optimal strength value can be obtained. And Example 10 can reach the compressive strength of Example 8 at 28d at 1d, indicating that it has the characteristics of high early strength. At 28d, the compressive strength reaches 25.48MPa, and the strength develops rapidly. Compared with Comparative Example 3, the compressive strength of Example 10 is increased by 23.64%.
[0097] The compressive strength of Example 8 is only 0.61 times that of Example 10. The reason is that when the Na2O content is low, it is not enough to provide a high-strength alkaline environment, the hydration reaction of the recycled cement is slow, and its compressive strength and flexural strength are low. On the contrary, the compressive strength and flexural strength of Example 11 at 28 days showed a downward trend. This is because when the Na2O content is too high, the hydration reaction of the recycled cement will be accelerated, and a protective film of hydration products will be formed on the surface of the recycled cement particles, which will hinder the continued hydration of the recycled cement and affect the strength development. And the flexural and compressive strengths at 28 days are lower than those of Comparative Example 3.
[0098] 4. Experimental study on mechanical properties of alkali-activated thermally activated regenerated cement-based composite materials at different nano-silicon dioxide contents (Comparative Example 4 and Examples 12-15)
[0099] The recycled cement-based composite material prepared in this experiment is composed of the following raw materials in parts by weight:
[0100] Cementitious material: 100 parts, of which 70 parts are cement and 30 parts are heat-activated cement powder (activation temperature 750°C);
[0101] Water reducing agent: 0.1 part;
[0102] Water glass: The modulus is 1.5, calculated as Na2O equivalent, and the proportion range is 6% of the cementitious material.
[0103] Nano-silicon dioxide: The mass ratio of nano-silicon dioxide to gel material particles is 1-5%. When used, it is prepared into a nano-silicon dioxide suspension, and mixed with other raw materials in the form of a nano-silicon dioxide dispersion. The preparation process of the nano-silicon dioxide suspension is: pour the weighed nano-silicon dioxide solution into a container, and disperse it for 45 minutes using an ultrasonic disperser to obtain a uniform nano-silicon dioxide suspension.
[0104] Sand: 300 parts;
[0105] Water: 66 parts;
[0106] The different nano-silicon dioxide contents in Comparative Example 4 (equivalent to Example 10) and Examples 12-15 when preparing recycled cement-based composite materials are shown in Table 5.
[0107] Table 5
[0108] Nano-silicon dioxide content (%) Comparative Example 4 0 Example 12 1 Embodiment 13 2 Embodiment 14 3 Embodiment 15 5
[0109] like Figure 7 As shown, the mechanical properties of alkali-activated thermally activated recycled cement-based composites under different nano-silica contents are affected:
[0110] from Figure 7It can be seen from Comparative Example 4 and Examples 12-15 that as the curing age increases, the compressive strength and flexural strength also gradually increase, which indicates that the nano-modified alkali excites the heat-activated regenerated cement hydration reaction and continues. For example, the compressive strength of Examples 12-15 at 28d increased by 52.07%, 54.94%, 50.77% and 60.43% respectively relative to 1d. Under the condition of the same water glass content, the flexural strength and compressive strength of each age increase first and then decrease with the increase of nano-silicon dioxide content, and when the nano-silicon dioxide content in Example 13 is 2%, the best strength value can be obtained. The compressive strength and flexural strength of Example 13 are increased by 9.06% and 11.47% respectively compared with those of Example 12. Compared with Comparative Example 4, the 28d compressive strength of Example 13 is increased by 31.50%, with good mechanical properties, which can reach the strength of ordinary silicate PO32.5, and the 28-day strength can reach more than 37MPa. This indicates that nano-silicon dioxide accelerates the hydration process of recycled cement, which is beneficial to improving the mechanical properties of recycled cement-based composite materials. However, excessive nano-silicon dioxide causes the strength of recycled cement to decline. The flexural strength and compressive strength of Example 15 are reduced by 1.62 MPa and 6.69 MPa, respectively, compared with those of Example 13.
[0111] The above-mentioned embodiments only express the specific implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the protection scope of the present application. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the technical solution concept of the present application, and these all belong to the protection scope of the present application.
Claims
1. A recycled cement-based composite material with waste concrete, characterized in that: The invention comprises a cement gel system, water, a water reducing agent and aggregates, wherein the cement gel system is composed of 70% by mass of cement and 30% by mass of heat-activated cement powder. The preparation process of the recycled cement-based composite material is as follows: (1) preparing waste concrete into waste concrete powder; (2) subjecting the waste concrete powder to thermal activation treatment, wherein the thermal activation treatment process is as follows: heating the waste concrete powder to 750° C., maintaining the heating for 3 hours, and finally cooling to room temperature to obtain thermally activated cement powder for standby use; (3) mixing cement, heat-activated cement powder, water, a water reducing agent and aggregate to obtain a recycled cement-based mixture; (4) Alkali activation: adding 2-8% of water glass by mass of the cement gel system to the recycled cement-based mixture, and mixing and stirring to obtain an alkali-activated system; (5) Add 1-5% of the mass of the cement gel system of nano-silicon dioxide into the alkali-activated system and stir evenly to obtain a recycled cement-based composite material.
2. The recycled cement-based composite material with waste concrete added as claimed in claim 1, characterized in that: The aggregate is sand, and the weight proportions of the cement gel system, water, water reducing agent and aggregate are respectively: 100 parts of the cement gel system, 66 parts of water, 0.1 parts of the water reducing agent and 300 parts of sand.
3. The recycled cement-based composite material with waste concrete added as claimed in claim 1, characterized in that: The water reducer is a polycarboxylate water reducer.
4. The recycled cement-based composite material with waste concrete added as claimed in claim 1, characterized in that: The process of preparing waste concrete into waste concrete powder is as follows: first, the waste concrete is crushed by a jaw crusher to obtain primary crushed powder with a particle size not greater than 8 mm; then, it is further ground by a roller crusher to a grinding powder with a particle size less than 2 mm; finally, a disc crusher is used for secondary grinding to obtain waste concrete powder with a particle size less than 75 μm.
5. The recycled cement-based composite material with waste concrete added as claimed in claim 1, characterized in that: The modulus of the water glass is 1.
5.
6. The method for preparing a recycled cement-based composite material with waste concrete as claimed in any one of claims 1 to 5, characterized in that: The steps include: (1) preparing waste concrete into waste concrete powder; (2) subjecting the waste concrete powder to thermal activation treatment, wherein the thermal activation treatment process is as follows: subjecting the waste concrete powder to thermal activation treatment, wherein the thermal activation treatment process is as follows: heating the waste concrete powder to 750° C., maintaining the heating for 3 hours, and finally cooling the waste concrete powder to room temperature to obtain thermally activated cement powder for standby use; (3) mixing cement, heat-activated cement powder, water, a water reducing agent and aggregate to obtain a recycled cement-based mixture; (4) Alkali activation: adding water glass to the recycled cement-based mixture in terms of Na2O equivalent, and mixing and stirring to obtain an alkali activation system; Claims (5) Add nano-silica to the alkali-activated system and stir evenly to obtain a recycled cement-based composite material.
Citation Information
Cited By
Concrete plant wastewater recycling system
CN121225785A