Self-film-forming core-shell structure photonic crystal microsphere and preparation method thereof

The hard-core soft-shell structure photonic crystal microspheres were prepared by seed emulsion polymerization, which solved the problem of traditional photonic crystal microspheres being prone to cracks and achieved a crack-free and stretchable photonic crystal microsphere film with good softness and high performance. Saturation structural color, suitable for structural color fields.

CN118772448AActive Publication Date: 2024-10-15JIANGNAN UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411008652.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-10-15
Estimated Expiration
2044-07-26

AI Technical Summary

Technical Problem

Traditional photonic crystal microspheres are prone to cracks or film rupture when drying or being affected by external forces, and the polymer film-forming materials affect their self-assembly process, resulting in uneven structural colors.

Method used

The seed emulsion polymerization method is used to prepare core-shell structure photonic crystal microspheres with hard cores and soft shells. The hard cores include hard microspheres with high glass transition temperatures such as PS, PMMA, PAN, and SiO2, and the soft shells are made of low-temperature microspheres such as EA, BA, and MMA. It is composed of a block copolymer with a glass transition temperature that forms a shell with a glass transition temperature lower than room temperature, ensuring that the film automatically adheres and becomes elastic after moisture is removed.

Benefits of technology

A crack-free, flat and stretchable photonic crystal microsphere film with good flexibility and high saturation structural color is achieved, which is suitable for the field of structural color generation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118772448A_ABST
    Figure CN118772448A_ABST
Patent Text Reader

Abstract

The invention discloses a self-film-forming core-shell structure photonic crystal microsphere and a preparation method thereof, and belongs to the technical field of material engineering. The core-shell structure composite photonic crystal microspheres with hard cores and soft shells are prepared by adopting a seed emulsion polymerization method, the hard cores comprise hard microspheres with high glass transition temperatures such as PS (polystyrene), PMMA (polymethyl methacrylate), PAN (polyacrylonitrile) and SiO2 (silicon dioxide), and the soft shells mainly comprise block copolymers with low glass transition temperatures, which are specifically composed of one or two of EA (ethylene acrylate), BA (butyl acrylate), MMA (methyl methacrylate) and the like. The shell of the prepared hard-core and soft-shell photonic crystal microsphere has a glass-transition temperature lower than room temperature, can be automatically adhered between hard microspheres after moisture is removed to form a crack-free and flat film, has certain elasticity, and can realize elastic recovery of the film after stretching; meanwhile, when the particle size of the core-shell structure photonic crystal microsphere is 200-300nm, the formed film has a structural color.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of material engineering, and in particular relates to a photonic crystal microsphere with a core-shell structure capable of self-forming a film and a preparation method thereof. Background Art

[0002] Photonic crystal (PC) is a crystalline material formed by periodically arranging materials with different refractive indices in space. The main feature of photonic crystals is that they have photonic bandgap, which can prohibit the propagation of light within a specific frequency range. When the photonic bandgap of photonic crystals is in the visible light band, the visible light within the bandgap is prohibited from propagating and is selectively reflected, thereby forming coherent diffraction on the periodically arranged photonic crystal surface. The reflected light of constructive interference stimulates the human eye, resulting in a structural color effect. Unlike general dyes that produce colors based on the absorption of light, the color of photonic crystals is produced by adjusting the effects of light diffraction and scattering to produce structural colors derived from physical structures. It is more environmentally friendly and has great application potential in coloring coatings.

[0003] Traditional photonic crystals such as polystyrene and silicon dioxide often crack during the drying process due to weak inter-particle forces. Chinese patent document CN115558145A discloses a method for preparing photonic crystal structure color-forming materials by spraying, in which the photonic crystal microspheres used have cracks after drying on the substrate surface. As a result, a method for preparing structural color films by compounding photonic crystal microspheres with polymer film-forming materials has emerged. For example, Chinese patent document CN116622215A provides a method for preparing SiO2-phenolic resin-polyurethane composite photonic crystal deformation color-changing film, in which SiO2 microspheres are compounded with resin materials to prepare structural color films. This method is affected by the need to add additional film-forming materials, which affects the process of self-assembly of photonic crystals to form structural color films. In places where the polymer is not filled evenly, cracking still occurs.

[0004] In view of the fact that existing single photonic crystal microspheres are prone to cracking when forming thin films, and in order to further realize that photonic crystal structure color films have good film-forming stability under the influence of external conditions such as stretching and compression, it is urgent to develop and prepare a photonic crystal microsphere that can directly form a crack-free, stretchable and recoverable thin film. Summary of the invention

[0005] Technical issues:

[0006] Traditional photonic crystal microspheres such as PS, PMMA, PAN, SiO2, etc. are prone to cracks when directly dried to form films, or the film is prone to rupture when affected by external forces. When adding polymer materials to assist in film formation, the polymer film-forming materials will affect the self-assembly process of the photonic crystal microspheres, causing the structural color produced by the microspheres to be uneven.

[0007] Technical solution:

[0008] In order to solve the above problems, the present invention adopts a seed emulsion polymerization method to prepare a hard-core-soft-shell composite photonic crystal microsphere, wherein the hard core includes hard microspheres with high glass transition temperatures such as PS, PMMA, PAN, and SiO2, and the soft shell mainly includes one or two specific composition block copolymers with low glass transition temperatures such as EA, BA, and MMA. The hard-core-soft-shell photonic crystal microsphere shell prepared by the present invention has a glass transition temperature lower than room temperature, can automatically adhere between the hard microspheres after water is removed, and form a crack-free and smooth film, and has a certain elasticity, and can achieve elastic recovery of the film after stretching; at the same time, when the particle size of the core-shell structure photonic crystal microsphere is between 200 and 300nm, the formed film has structural color.

[0009] The first object of the present invention is to provide a photonic crystal microsphere with a hard core and a soft shell which can form an elastic film.

[0010] The second object of the present invention is to provide a method for preparing the hard-core-soft-shell core-shell structured photonic crystal microspheres.

[0011] In addition, the present invention also provides the application of the hard-core-soft-shell core-shell structure photonic crystal microsphere in structural color generation.

[0012] In order to achieve the aforementioned invention object, the present invention adopts the following technical solutions:

[0013] The invention provides a core-shell structured photonic crystal microsphere, wherein the composite structure of a hard core and a soft shell can gradually form a core-shell structure through seed emulsion polymerization.

[0014] The present invention also provides a method for preparing the core-shell structure photonic crystal microspheres, comprising:

[0015] S1, emulsifying a portion of the hard core monomer, the crosslinking agent, the emulsifier and water, and then adding the initiator to react to obtain a polymer seed emulsion;

[0016] S2, adding another portion of the hard core monomer, the crosslinking agent, and the initiator to the obtained polymer seed emulsion, and polymerizing to obtain a hard core microsphere system;

[0017] S3, adding a soft shell monomer, a crosslinking agent, and an initiator to the obtained hard core microsphere system to initiate polymerization to obtain a hard core soft shell photonic crystal microsphere.

[0018] In one embodiment of the present invention, the particle size of the polymer seeds in S1 is about 120 nm, and the polymer dispersibility index (PDI) is less than 0.08.

[0019] In one embodiment of the present invention, the particle size of the hard core microspheres in S2 is about 170-220 nm, and the PDI is less than 0.08.

[0020] In one embodiment of the present invention, the particle size of the hard core soft shell photonic crystal microspheres in S2 is about 200-300, and the PDI is less than 0.08.

[0021] In one embodiment of the present invention, the hard core monomer is one or more of styrene (St), methyl methacrylate (MMA), and acrylonitrile (AN).

[0022] In one embodiment of the present invention, the monomer for the soft shell is selected from:

[0023] ① Ethyl acrylate (EA), or

[0024] ② A combination of ethyl acrylate (EA) and butyl acrylate (BA), or

[0025] ③ Combination of methyl methacrylate (MMA) and butyl acrylate (BA).

[0026] In one embodiment of the present invention, the mass ratio of ethyl acrylate (EA) to butyl acrylate (BA) in the soft shell monomer is (19-20):(0-1).

[0027] In one embodiment of the present invention, the mass ratio of methyl methacrylate (MMA) to butyl acrylate (BA) in the soft shell monomer is 1:3.

[0028] In one embodiment of the present invention, the mass ratio of the hard core monomer in S1 to the hard core monomer in S2 is 1:(1-2). Specifically, it can be 1:1.5.

[0029] In one embodiment of the present invention, the emulsifier used for emulsification is one of sodium dodecyl sulfate (SDS), sodium dodecylbenzene sulfonate, and sodium dodecyl sulfonate.

[0030] In one embodiment of the present invention, the emulsifier accounts for 0.15-0.25wt.% of the total monomer concentration; specifically, 0.2wt.% can be selected. (Total monomer refers to the total mass of the hard core monomer and the soft shell monomer)

[0031] In one embodiment of the present invention, the crosslinking agent may be one or more of diene crosslinking agents such as divinylbenzene (DVB), allyl methacrylate (ALMA), and isoprene.

[0032] In one embodiment of the present invention, the amount of the crosslinking agent in S1 or S2 relative to the monomer for the hard core in this step is 10-14 wt.%.

[0033] In one embodiment of the present invention, the amount of the crosslinking agent in S3 relative to the soft shell monomer in this step is 0.2-1.0 wt.%.

[0034] In one embodiment of the present invention, the initiator may also be one or more of ammonium persulfate (APS), potassium persulfate, and sodium persulfate.

[0035] In one embodiment of the present invention, in S1, S2 or S3, the ratio of initiator to monomer is 0.5-1 wt. %.

[0036] The present invention also provides application of the hard-core soft-shell photonic crystal microspheres in structural chromogenic films.

[0037] Beneficial effects of the present invention:

[0038] The monomer raw materials required for the core-shell structure photonic crystal microspheres prepared by the present invention are low in price, and the glass transition temperature of the hard inner core is above 100°C, so that the entire inner core microsphere can maintain a spherical shape at ambient temperature, which is convenient for self-assembly to form a regular array; the outer shell of the photonic crystal microsphere has a glass transition temperature lower than room temperature, and can form a thin film at room temperature after removing moisture, and the formed film has good softness and flatness, and will not have cracks. The average refractive index of the hard inner core is higher than that of the outer shell, and the refractive index difference between the two can give the formed structural color film a high saturation color, which has broad application prospects in the field of structural color generation. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 The particle size distribution curves of PS seeds, PS cores and PS@P(EA-BA) photonic crystal composite microspheres prepared by seed emulsion polymerization of the present invention are shown in FIG.

[0040] Figure 2 It is the Fourier infrared spectrum of the PS@P(EA-BA) photonic crystal composite microsphere of the present invention;

[0041] Figure 3 A physical picture of a flat structural color film formed by PS@P(EA-BA) photonic crystal composite microspheres prepared in Example 1 of the present invention;

[0042] Figure 4 This is a physical picture of the PS core photonic crystal film prepared in Comparative Example 1 of the present invention;

[0043] Figure 5 This is a scanning electron microscope image of the PS core photonic crystal film prepared in Comparative Example 1 of the present invention;

[0044] Figure 6 This is a scanning electron microscope image of the PS@P(EA-BA) photonic crystal film prepared in Example 1 of the present invention;

[0045] Figure 7 This is a physical picture of the stretching recovery of the PS@P(EA-BA) photonic crystal film prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0046] In order to better understand the present invention, the content of the present invention is further explained below in conjunction with some embodiments, but the following examples are not used to limit the present invention.

[0047] Test method:

[0048] Photonic crystal microsphere particle size and monodispersity test: ZetasizerNano-ZS90 potential and particle size analyzer was used to test the samples.

[0049] Embodiment 1:

[0050] (1) 5 g of St and 0.5 g of DVB were added to 100 mL of deionized water containing 0.065 g of SDS and emulsified at 300 rpm for 30 min. The reaction temperature was then raised to 85 °C and maintained for 10 min. 0.05 g of APS was then added to initiate polymerization for 1 h to obtain PS seeds with a particle size of about 120 nm.

[0051] (2) 7.5 g St and 1 g DVB were added to the reaction system, and then 0.05 g APS was added to initiate polymerization for 1.5 h to obtain a PS core with a particle size of about 220 nm.

[0052] (3) 19 g EA, 1 g BA and 0.04 g ALMA were added into the reaction system, and then 0.1 g APS was added to initiate polymerization for 1.5 h to obtain a core-shell structured PS@P (EA-BA) photonic crystal microsphere emulsion with a particle size of about 280 nm.

[0053] (4) Take 5 mL of the emulsion and drop it on a culture dish. After drying, a flat elastic film is formed, accompanied by the appearance of structural color.

[0054] Embodiment 2:

[0055] (1) 5 g of St and 0.5 g of DVB were added to 100 mL of deionized water containing 0.066 g of SDS and emulsified at 300 rpm for 30 min. The reaction temperature was then raised to 85 °C and maintained for 10 min. 0.05 g of APS was then added to initiate polymerization for 1 h to obtain PS seeds with a particle size of more than 120 nm.

[0056] (2) 7.5 g St and 1 g DVB were added to the reaction system, and then 0.05 g APS was added to initiate polymerization for 1.5 h to obtain a PS core with a particle size of about 190 nm.

[0057] (3) 19 g EA, 1 g BA and 0.04 g ALMA were added into the reaction system, and then 0.1 g APS was added to initiate polymerization for 1.5 h to obtain a core-shell structured PS@P (EA-BA) photonic crystal microsphere emulsion with a particle size of about 250 nm.

[0058] (4) Take 5 mL of the emulsion and drop it on a culture dish. After drying, a flat elastic film is formed, accompanied by the appearance of structural color.

[0059] Embodiment 3:

[0060] (1) 5 g of St and 0.5 g of DVB were added to 100 mL of deionized water containing 0.070 g of SDS and emulsified at 300 rpm for 30 min. The reaction temperature was then raised to 85 °C and maintained for 10 min. 0.05 g of APS was then added to initiate polymerization for 1 h to obtain PS seeds with a particle size of more than 120 nm.

[0061] (2) 7.5 g St and 1 g DVB were added to the reaction system, and then 0.05 g APS was added to initiate polymerization for 1.5 h to obtain a PS core with a particle size of about 170 nm.

[0062] (3) 19 g EA, 1 g BA and 0.04 g ALMA were added into the reaction system, and then 0.1 g APS was added to initiate polymerization for 1.5 h to obtain a core-shell structured PS@P (EA-BA) photonic crystal microsphere emulsion with a particle size of about 210 nm.

[0063] (4) Take 5 mL of the emulsion and drop it on a culture dish. After drying, a flat elastic film is formed, accompanied by the appearance of structural color.

[0064] Embodiment 4:

[0065] (1) 5 g of St and 0.5 g of DVB were added to 100 mL of deionized water containing 0.065 g of SDS and emulsified at 300 rpm for 30 min. The reaction temperature was then raised to 85 °C and maintained for 10 min. 0.05 g of APS was then added to initiate polymerization for 1 h to obtain PS seeds with a particle size of more than 120 nm.

[0066] (2) 7.5 g St and 1 g DVB were added to the reaction system, and then 0.08 g APS was added to initiate polymerization for 1.5 h to obtain a PS core with a particle size of about 230 nm.

[0067] (3) 5 g MMA, 15 g BA and 0.04 g ALMA were added to the reaction system, and then 0.1 g APS was added to initiate polymerization for 1.5 h to obtain a core-shell structured PS@P (MMA-BA) photonic crystal microsphere emulsion with a particle size of about 290 nm.

[0068] (4) Take 5 mL of the emulsion and drop it on a culture dish. After drying, a flat elastic film is formed, accompanied by the appearance of structural color.

[0069] Embodiment 5:

[0070] (1) 5 g of St and 0.5 g of DVB were added to 100 mL of deionized water containing 0.065 g of SDS and emulsified at 300 rpm for 30 min. The reaction temperature was then raised to 85 °C and maintained for 10 min. 0.05 g of APS was then added to initiate polymerization for 1 h to obtain PS seeds with a particle size of more than 120 nm.

[0071] (2) 7.5 g St and 1 g DVB were added to the reaction system, and then 0.1 g APS was added to initiate polymerization for 1.5 h to obtain a PS core with a particle size of about 240 nm.

[0072] (3) 20 g EA and 0.04 g ALMA were added to the reaction system, and then 0.1 g APS was added to initiate polymerization for 1.5 h to obtain a core-shell structured PS@PEA photonic crystal microsphere emulsion with a particle size of about 300 nm.

[0073] (4) Take 5 mL of the emulsion and drop it on a culture dish. After drying, a flat elastic film is formed, accompanied by the appearance of structural color.

[0074] Embodiment 6:

[0075] (1) 5 g of AN and 0.5 g of DVB were added to 100 mL of deionized water containing 0.065 g of SDS and emulsified at 300 rpm for 30 min. The reaction temperature was then raised to 85 °C and maintained for 10 min. 0.05 g of APS was then added to initiate polymerization for 1 h to obtain PAN seeds with a particle size of more than 120 nm.

[0076] (2) 7.5 g AN and 1 g DVB were added to the reaction system, and then 0.05 g APS was added to initiate polymerization for 1.5 h to obtain a PAN core with a particle size of about 220 nm.

[0077] (3) 19 g EA, 1 g BA and 0.04 g ALMA were added into the reaction system, and then 0.1 g APS was added to initiate polymerization for 1.5 h to obtain a core-shell structured PAN@P (EA-BA) photonic crystal microsphere emulsion with a particle size of about 280 nm.

[0078] (4) Take 5 mL of the emulsion and drop it on a culture dish. After drying, a flat elastic film is formed, accompanied by the appearance of structural color.

[0079] Embodiment 7:

[0080] (1) 5 g of MMA and 0.5 g of DVB were added to 100 mL of deionized water containing 0.065 g of SDS, and emulsified at 300 rpm for 30 min. The reaction temperature was then raised to 85 °C and maintained for 10 min. 0.05 g of APS was then added to initiate polymerization for 1 h to obtain PMMA seeds with a particle size of more than 120 nm.

[0081] (2) 7.5 g MMA and 1 g DVB were added to the reaction system, and then 0.20 g APS was added to initiate polymerization for 1.5 h to obtain a PMMA core with a particle size of about 170 nm.

[0082] (3) 19 g EA, 1 g BA and 0.04 g ALMA were added into the reaction system, and then 0.1 g APS was added to initiate polymerization for 1.5 h to obtain a core-shell structured PMMA@P(EA-BA) photonic crystal microsphere emulsion with a particle size of about 250 nm.

[0083] (4) 5 mL of the emulsion was dropped onto a culture dish, and after drying, a flat elastic film was formed, accompanied by the appearance of structural colors.

[0084] (1) 5 g of St and 0.5 g of DVB were added to 100 mL of deionized water containing 0.065 g of SDS and emulsified at 300 rpm for 30 min. The reaction temperature was then raised to 85 °C and maintained for 10 min. 0.05 g of APS was then added to initiate polymerization for 1 h to obtain PS seeds with a particle size of more than 120 nm.

[0085] (2) 7.5 g St and 1 g DVB were added to the reaction system, and then 0.05 g APS was added to initiate polymerization for 1.5 h to obtain PS microspheres with a particle size of about 220 nm.

[0086] (3) Take 5 mL of the emulsion and drop it on a culture dish. After drying, structural color appears, but there is a cracking problem.

[0087] Comparative Example 2:

[0088] (1) 5 g of St and 0.5 g of DVB were added to 100 mL of deionized water containing 0.065 g of SDS and emulsified at 300 rpm for 30 min. The reaction temperature was then raised to 85 °C and maintained for 10 min. 0.05 g of APS was then added to initiate polymerization for 1 h to obtain PS seeds with a particle size of more than 120 nm.

[0089] (2) 7.5 g St and 1 g DVB were added to the reaction system, and then 0.05 g APS was added to initiate polymerization for 1.5 h to obtain a PS core with a particle size of about 220 nm.

[0090] (3) 5 g MMA, 15 g EA and 0.04 g ALMA were added to the reaction system, and then 0.1 g APS was added to initiate polymerization for 1.5 h to obtain a core-shell structured PS@PEA photonic crystal microsphere emulsion with a particle size of about 300 nm.

[0091] (4) 5 mL of the emulsion was dropped onto a petri dish, and a cracked film was formed after drying.

[0092] Comparative Example 3:

[0093] (1) 5 g of St and 0.5 g of DVB were added to 100 mL of deionized water containing 0.065 g of SDS and emulsified at 300 rpm for 30 min. The reaction temperature was then raised to 85 °C and maintained for 10 min. 0.05 g of APS was then added to initiate polymerization for 1 h to obtain PS seeds with a particle size of more than 120 nm.

[0094] (2) 7.5 g St and 1 g DVB were added to the reaction system, and then 0.05 g APS was added to initiate polymerization for 1.5 h to obtain a PS core with a particle size of about 220 nm.

[0095] (3) 20 g BA and 0.04 g ALMA were added to the reaction system, and then 0.1 g APS was added to initiate polymerization for 1.5 h to obtain a core-shell structured PS@PBA photonic crystal microsphere emulsion with a particle size of about 320 nm.

[0096] (4) Take 5 mL of the emulsion and drop it on a culture dish. After drying, a flat film is formed without structural color. However, the film has no strength and has a stringing problem when stretched and cannot be restored.

[0097] Comparative Example 4:

[0098] (1) 12.5 g of St and 1.5 g of DVB were added to 100 mL of deionized water containing 0.065 g of SDS and emulsified at 300 rpm for 30 min. The reaction temperature was then raised to 85 °C and maintained for 10 min. 0.1 g of APS was then added to initiate polymerization for 2.5 h to obtain a PS core.

[0099] (2) 19 g EA, 1 g BA and 0.04 g ALMA were added into the reaction system, and then 0.1 g APS was added to initiate polymerization for 1.5 h to obtain a core-shell structured PS@P (EA-BA) photonic crystal microsphere emulsion.

[0100] (3) Take 5 mL of the emulsion and drop it on a culture dish. After drying, a flat elastic film is formed, but no structural color appears.

[0101] Table 1. Comparison of results of Examples 1-7 and Comparative Examples 1-4

[0102]

[0103]

[0104] Example 8: Optimization of the combination ratio of monomers for soft shell in step (3)

[0105] (1) 5 g of St and 0.5 g of DVB were added to 100 mL of deionized water containing 0.065 g of SDS and emulsified at 300 rpm for 30 min. The reaction temperature was then raised to 85 °C and maintained for 10 min. 0.05 g of APS was then added to initiate polymerization for 1 h to obtain PS seeds with a particle size of about 120 nm.

[0106] (2) 7.5 g St and 1 g DVB were added to the reaction system, and then 0.05 g APS was added to initiate polymerization for 1.5 h to obtain a PS core with a particle size of about 220 nm.

[0107] (3) A certain amount of EA, BA and 0.04 g ALMA were added into the reaction system, and then 0.1 g APS was added to initiate polymerization for 1.5 h to obtain a core-shell structured PS@P (EA-BA) photonic crystal microsphere emulsion with a particle size of about 280 nm.

[0108] (4) 5 mL of the emulsion was dropped onto a petri dish and dried to form a smooth film. The results are shown in Table 2.

[0109] Table 2

[0110] EA addition amount (g) BA addition amount (g) Mass ratio of EA to BA Film Forming Results Structural Color 20 0 Example 5 Elastic and smooth without cracks red 19 1 19:1 (Example 1) Elastic and smooth without cracks green 15 5 15:5 Poor elasticity and easy to deform green 10 10 10:10 Inelastic but not cracking green 5 15 5:15 Inelastic but not cracking No structural color 1 19 1:19 Inelastic but not cracking No structural color 0 20 Comparative Example 3 Inelastic but not cracking No structural color

[0111] Example 9: Optimization of the combination ratio of monomers for soft shell in step (3)

[0112] (1) 5 g of St and 0.5 g of DVB were added to 100 mL of deionized water containing 0.065 g of SDS and emulsified at 300 rpm for 30 min. The reaction temperature was then raised to 85 °C and maintained for 10 min. 0.05 g of APS was then added to initiate polymerization for 1 h to obtain PS seeds with a particle size of more than 120 nm.

[0113] (2) 7.5 g St and 1 g DVB were added to the reaction system, and then 0.08 g APS was added to initiate polymerization for 1.5 h to obtain a PS core with a particle size of about 230 nm.

[0114] (3) A certain amount of MMA, BA and 0.04 g ALMA were added into the reaction system, and then 0.1 g APS was added to initiate polymerization for 1.5 h to obtain a core-shell structured PS@P (MMA-BA) photonic crystal microsphere emulsion with a particle size of about 290 nm.

[0115] (4) 5 mL of the emulsion was dropped onto a petri dish and dried to form a smooth film. The results are shown in Table 3.

[0116] Table 3

[0117] MMA addition amount (g) BA addition amount (g) Mass ratio of MMA to BA Film Forming Results Structural Color 5 15 1:3 (Example 4) Elastic and smooth without cracks green 8 12 1:1.5 The hard film is inelastic and does not crack No structural color 10 10 1:1 The hard film is inelastic and does not crack No structural color 12 8 1.5:1 The hard film is inelastic and does not crack No structural color 15 5 3:1 The hard film is inelastic and does not crack No structural color

[0118] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a hard-core soft-shell photonic crystal composite microsphere capable of forming a self-elastic film, characterized in that: The core-shell structure is gradually formed by seed emulsion polymerization, including the following steps: S1, emulsifying a portion of the hard core monomer, the crosslinking agent, the emulsifier and water, and then adding the initiator to react to obtain a polymer seed emulsion; S2, adding another portion of the hard core monomer, the crosslinking agent, and the initiator to the obtained polymer seed emulsion, and polymerizing to obtain a hard core microsphere system; S3, adding a soft shell monomer, a crosslinking agent, and an initiator to the obtained hard core microsphere system to initiate polymerization to obtain a hard core soft shell photonic crystal microsphere; The hard core monomer is one or more of styrene, methyl methacrylate and acrylonitrile; The soft shell monomer is selected from: ① Ethyl acrylate, or ② A combination of ethyl acrylate and butyl acrylate, or ③Combination of methyl methacrylate and butyl acrylate.

2. The method according to claim 1, characterized in that The mass ratio of ethyl acrylate to butyl acrylate in the monomer for soft shell is (19-20):(0-1).

3. The method according to claim 1, characterized in that: The mass ratio of methyl methacrylate to butyl acrylate in the monomer for the soft shell is 1:

3.

4. The method according to claim 1, characterized in that The emulsifier is one of sodium dodecyl sulfate, sodium dodecylbenzene sulfonate and sodium dodecyl sulfonate.

5. The method according to claim 1, characterized in that The mass ratio of the monomer for the hard core in S1 to the monomer for the hard core in S2 is 1:(1-2).

6. The method according to claim 1, characterized in that The crosslinking agent is one or more of diene crosslinking agents such as divinylbenzene, allyl methacrylate, isoprene, etc.

7. The method according to claim 1, characterized in that The amount of the crosslinking agent in S1 or S2 relative to the monomer for the hard core in this step is 10-14 wt.%.

8. The method according to claim 1, characterized in that The amount of the crosslinking agent in S3 relative to the monomer for the soft shell is 0.2-1.0 wt.%.

9. The method according to claim 1, characterized in that: The initiator is one or more of ammonium persulfate, potassium persulfate and sodium persulfate.

10. The method according to claim 1, characterized in that The particle size of the polymer seeds in S1 is about 120 nm, and the polymer dispersity index is less than 0.

08.

11. The method according to claim 1, characterized in that: The particle size of the hard core microspheres in S2 is about 170-220 nm, and the polymer dispersibility index is less than 0.

08.

12. The method according to claim 1, characterized in that The particle size of the hard-core soft-shell photonic crystal microspheres in S2 is about 200-300, and the polymer dispersibility index is less than 0.

08.

13. Hard-core soft-shell photonic crystal composite microspheres prepared by the method according to any one of claims 1 to 12.

14. A structural chromogenic film, characterized in that: Containing the hard-core soft-shell photonic crystal microspheres according to claim 13.

15. Use of the hard-core soft-shell photonic crystal microspheres according to claim 13 in colored coatings.

Citation Information

Patent Citations

  • Material with schemochrome and capable of being induced to change color through stress and preparation method of material

    CN105182567A

  • Flexible photonic crystal element nano microspheres and preparation method thereof

    CN110804127A

  • Resin particle for making photonic crystal structure and photonic crystal film obtained from the same

    JP2008083545A

  • Manufacturing method of photonic crystal membrane and photonic crystal membrane obtained thereby

    JP2008165030A