Superfine composite doping material for water-based paint and preparation method of superfine composite doping material
Through the preparation method of ultra-fine composite additives, the problems of insufficient flocculation and thermal insulation performance of water-based coatings are solved, the stability and thermal insulation performance are improved, and it is suitable for use in the fields of architectural decoration and energy-saving coating.
Patent Information
- Application Number
- CN202410926019.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-10-15
AI Technical Summary
Water-based coatings are prone to flocculation, resulting in reduced stability and insufficient thermal insulation properties, limiting their use in certain application areas.
Using the preparation method of ultra-fine composite additives, by controlling the calcination and stirring process of the powder, the pH value is adjusted to form a uniform colloid and porous structure, thereby improving the stability and heat insulation performance of the coating. The admixture components include fly ash, stone powder, mineral powder, white carbon black, PVP and sodium bicarbonate, and the emulsion is prepared through ball milling, calcination and stirring steps.
It effectively reduces the flocculation phenomenon, improves the uniformity and adhesion of the coating film, enhances the thermal insulation performance, is suitable for industrial production, and is suitable for use in the fields of architectural decoration and energy-saving coating.
Smart Images

Figure CN118772684A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of water-based paint preparation, and in particular to an ultrafine composite admixture for water-based paint and a preparation method thereof. Background Art
[0002] Waterborne coatings have been widely used in architectural decoration, industrial coatings, furniture coatings and other fields due to their advantages such as environmental protection, safety and low volatile organic compound (VOC) emissions. With the increasingly stringent environmental regulations and the increasing demand of consumers for healthy and environmentally friendly products, the research and development and application of waterborne coatings have become an important development direction of the coatings industry. However, waterborne coatings often face many challenges in practical applications, such as film performance, stability, thermal insulation performance and other requirements.
[0003] Although water-based paint technology has made significant progress, there are still some technical bottlenecks that need to be overcome. Among them, the flocculation phenomenon that water-based paints are prone to is an important problem. Flocculation will lead to a decrease in the stability of the paint, affecting the uniformity and adhesion of the coating film, and thus affecting the final coating effect. In addition, traditional water-based paints also have shortcomings in thermal insulation performance, which limits their use in certain specific application areas, such as exterior wall coatings of buildings with high requirements for energy-saving performance. These shortcomings are mainly due to the composition and preparation method of the admixtures, and the existing technology has failed to effectively improve the stability and thermal insulation performance of water-based paints. Summary of the invention
[0004] In order to solve the above problems, the present invention provides an ultrafine composite admixture for water-based coatings and a preparation method thereof.
[0005] In a first aspect, the present invention provides a method for preparing an ultrafine composite admixture for water-based coatings, wherein the flocculation of the water-based coating is reduced and the thermal insulation performance is enhanced by controlling the pH of the coating emulsion. The admixture components are calculated by weight, including 20 to 40 parts of fly ash, 10 to 15 parts of stone powder, 10 to 30 parts of mineral powder, 5 to 10 parts of white carbon black, 10 to 20 parts of PVP, and 5 to 10 parts of sodium bicarbonate. The specific steps are as follows:
[0006] Step 1: firstly, feed the raw material powders according to the mass fractions into a ball mill for mixing to obtain a mixed powder, and then place the mixed powder in a muffle furnace and calcine at 100 to 120 degrees for 3 to 8 hours to obtain a mixed powder;
[0007] Step 2: Pass the calcined powder through a 200-mesh sieve, then add water at a powder-water mass ratio of 1:(2-5), and stir at room temperature to obtain an admixture emulsion;
[0008] Step three, adding a 10% to 30% hydrochloric acid aqueous solution to the admixture emulsion obtained in step two and stirring, adjusting the pH to 8 to 9, and obtaining an admixture emulsion for water-based coatings.
[0009] Preferably, in step 1, the ball milling speed is 200-400 r / min, the ball milling time is 6-12 h, and the ball mill is paused for 5 min every 15 min of operation.
[0010] Preferably, in step 2, the stirring rate is 300-600 r / min, and the stirring time is 3-6 h.
[0011] Preferably, the stirring rate in step three is 200-400 r / min.
[0012] In the second aspect, the present invention provides a water-based coating obtained by mixing an admixture emulsion prepared by the preparation method of the first aspect of the present invention with a polyurethane emulsion having a mass fraction of 30-50% in a ratio of 1:(0.5-2).
[0013] Preferably, the thermal conductivity of the ultrafine composite admixture is 0.04 to 0.15 W / (m·K).
[0014] Compared with the prior art, the present invention has the following beneficial effects:
[0015] 1. The present invention provides an ultrafine composite admixture for water-based coatings and a preparation method thereof. Calcination is introduced in the processing of powders. The gas generated during calcination makes the powders softer and more porous, while reducing the particle size of the powders, thereby increasing the viscosity of the solution and reducing sedimentation.
[0016] 2. In the process of preparing the admixture emulsion, the pH value of the emulsion is adjusted to make it weakly alkaline, which is beneficial for the admixture to form a uniform colloid. When the coating is cured, the coating has uniform pores inside, thereby improving the thermal insulation performance.
[0017] 3. The preparation method provided by the present invention is easy to scale up and automate, and is very suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] In order to more clearly illustrate the embodiments of the present invention or the technical solutions of the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0019] Figure 1 The thermal conductivity curves of the coatings prepared in Examples 1, 2, 3 and Comparative Example 1 of the present invention are shown. DETAILED DESCRIPTION
[0020] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0021] Embodiment 1
[0022] The admixture components are calculated by weight: 40 parts of fly ash, 10 parts of stone powder, 30 parts of mineral powder, 5 parts of white carbon black, 20 parts of PVP, and 5 parts of sodium bicarbonate. The specific steps are as follows:
[0023] Step 1: First, feed the above raw material powders into a ball mill according to the mass fraction for mixing to obtain a mixed powder, and then place the mixed powder in a muffle furnace and calcine at 120 degrees for 3 hours to obtain a mixed powder; the ball mill speed is 200r / min, the ball mill time is 12h, and the ball mill is paused for 5min every 15min of operation.
[0024] Step 2: Pass the calcined powder through a 200-mesh sieve, then add water at a powder-water mass ratio of 1:5, and stir at room temperature to obtain an admixture emulsion; the stirring rate is 300 r / min, and the stirring time is 6 hours.
[0025] Step 3: Add 10% hydrochloric acid aqueous solution dropwise to the admixture emulsion obtained in step 2 and stir, adjust the pH to 9, and obtain an admixture emulsion for water-based coatings at a stirring rate of 200 r / min.
[0026] The prepared admixture emulsion is mixed with a polyurethane emulsion with a mass fraction of 50% in a ratio of 1:0.5 to obtain a water-based coating.
[0027] Embodiment 2
[0028] The admixture components are calculated by weight: 20 parts of fly ash, 15 parts of stone powder, 10 parts of mineral powder, 10 parts of white carbon black, 10 parts of PVP, and 10 parts of sodium bicarbonate. The specific steps are as follows:
[0029] Step 1: first feed the above raw material powders according to the mass fractions into a ball mill for mixing to obtain a mixed powder, and then place the mixed powder in a muffle furnace and calcine at 100 degrees for 8 hours to obtain a mixed powder; in step 1, the ball mill speed is 400r / min, the ball mill time is 6h, and the ball mill is paused for 5min every 15min of operation.
[0030] Step 2: Pass the calcined powder through a 200-mesh sieve, then add water at a powder-water mass ratio of 1:2, and stir at room temperature to obtain an admixture emulsion; in step 2, the stirring rate is 600 r / min and the stirring time is 3 h.
[0031] Step 3: Add 30% hydrochloric acid aqueous solution dropwise to the admixture emulsion obtained in step 2 and stir, adjust pH to 8, and obtain an admixture emulsion for water-based coatings. The stirring rate in step 3 is 400 r / min.
[0032] The prepared admixture emulsion was mixed with a polyurethane emulsion having a mass fraction of 30% in a ratio of 1:2 to obtain a water-based coating.
[0033] Embodiment 3
[0034] The admixture components are calculated by weight: 30 parts of fly ash, 13 parts of stone powder, 22 parts of mineral powder, 6 parts of white carbon black, 15 parts of PVP, and 9 parts of sodium bicarbonate. The specific steps are as follows:
[0035] Step 1: first feed the above raw material powders into a ball mill according to the mass fractions for mixing to obtain a mixed powder, and then place the mixed powder in a muffle furnace and calcine at 110 degrees for 7 hours to obtain a mixed powder; in step 1, the ball mill speed is 350r / min, the ball mill time is 10h, and the ball mill is paused for 5min every 15min of operation.
[0036] Step 2: Pass the calcined powder through a 200-mesh sieve, then add water at a powder-water mass ratio of 1:4, and stir at room temperature to obtain an admixture emulsion; in step 2, the stirring rate is 400 r / min and the stirring time is 5 h.
[0037] Step 3: Add 20% hydrochloric acid aqueous solution dropwise to the admixture emulsion obtained in step 2 and stir, adjust pH to 8, and obtain an admixture emulsion for water-based coatings. The stirring rate in step 3 is 300 r / min.
[0038] The prepared admixture emulsion was mixed with a polyurethane emulsion having a mass fraction of 35% in a ratio of 1:1 to obtain a water-based coating.
[0039] Comparative Example 1
[0040] The admixture components are calculated by weight: 30 parts of fly ash, 13 parts of stone powder, 22 parts of mineral powder, 6 parts of white carbon black, 15 parts of PVP, and 9 parts of sodium bicarbonate. The specific steps are as follows:
[0041] Step 1: first feed the above raw material powders into a ball mill according to the mass fractions for mixing to obtain a mixed powder, and then place the mixed powder in a muffle furnace and calcine at 110 degrees for 7 hours to obtain a mixed powder; in step 1, the ball mill speed is 350r / min, the ball mill time is 10h, and the ball mill is paused for 5min every 15min of operation.
[0042] Step 2: Pass the calcined powder through a 200-mesh sieve, then add water at a powder-water mass ratio of 1:4, and stir at room temperature to obtain an admixture emulsion; in step 2, the stirring rate is 400 r / min and the stirring time is 5 h.
[0043] The prepared admixture emulsion was mixed with a polyurethane emulsion having a mass fraction of 35% in a ratio of 1:1 to obtain a water-based coating.
[0044] like Figure 1 As shown, through reasonable raw material ratios and processing steps, the coatings prepared in Examples 1, 2, and 3 show good performance in thermal conductivity, especially at higher temperatures. The thermal conductivity of Comparative Example 1 is significantly lower than that of each example, verifying the importance of adding different components and optimizing processing steps to improve the thermal conductivity of the coating.
Claims
1. A method for preparing an ultrafine composite admixture for water-based coatings, characterized in that: By controlling the pH of the coating emulsion to reduce the flocculation of the water-based coating and enhance the thermal insulation performance, the admixture components are calculated by weight: 20-40 parts of fly ash, 10-15 parts of stone powder, 10-30 parts of mineral powder, 5-10 parts of white carbon black, 10-20 parts of PVP, and 5-10 parts of sodium bicarbonate. The specific steps are as follows: Step 1: firstly, feed the raw material powders according to the mass fractions into a ball mill for mixing to obtain a mixed powder, and then place the mixed powder in a muffle furnace and calcine at 100 to 120 degrees for 3 to 8 hours to obtain a mixed powder; Step 2: Pass the calcined powder through a 200-mesh sieve, then add water at a powder-water mass ratio of 1:(2-5), and stir at room temperature to obtain an admixture emulsion; Step three, adding a 10% to 30% hydrochloric acid aqueous solution to the admixture emulsion obtained in step two and stirring, adjusting the pH to 8 to 9, and obtaining an admixture emulsion for water-based coatings.
2. The method for preparing the ultrafine composite admixture for water-based coatings according to claim 1, characterized in that: In step 1, the ball milling speed is 200-400 r / min, the ball milling time is 6-12 h, and the ball mill is paused for 5 min every 15 min of operation.
3. The method for preparing the ultrafine composite admixture for water-based coatings according to claim 1, characterized in that: In step 2, the stirring rate is 300-600 r / min, and the stirring time is 3-6 h.
4. The method for preparing the ultrafine composite admixture for water-based coatings according to claim 1, characterized in that: The stirring rate in step 3 is 200-400 r / min.
5. An ultrafine composite admixture for water-based coatings, characterized in that: The admixture emulsion obtained by the preparation method according to any one of claims 1 to 4 is mixed with a polyurethane emulsion with a mass fraction of 30 to 50% in a ratio of 1: (0.5 to 2) to obtain a water-based paint.
6. The ultrafine composite admixture for water-based coatings according to claim 5, characterized in that: The thermal conductivity of the ultrafine composite admixture is 0.04-0.15 W / (m·K).