Hierarchical-structure two-dimensional tri-metal oxide / carbon material and preparation method and application thereof
By using 2-methylimidazole inducer and the assembly of Zn2+ and Co,Ni-LDH nanosheets at room temperature, Co,Ni-LDH@ZIF-8 nanocomposites were prepared and treated at high temperature in an air atmosphere to solve the problem This solves the problem in the existing technology that the microwave absorption performance of bimetallic LDH and MOF combined materials cannot be effectively exerted, and realizes the preparation of efficient, economical, and environmentally friendly microwave absorption materials with excellent electromagnetic response characteristics and commercialization potential.
Patent Information
- Application Number
- CN202410744682.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-11
- Publication Date
- 2024-10-15
AI Technical Summary
The existing technology is difficult to prepare two-dimensional hierarchical structure nanocomposites with excellent microwave absorption properties through a simple, economical and environmentally friendly method, especially the combination of bimetallic LDH and MOF, which fails to effectively take advantage of its structural advantages and microwave absorption. ability.
By using 2-methylimidazole as an inducer at room temperature, combining Zn2+ with Co,Ni-LDH nanosheets, and using ultrasonic dispersion and stirring in-situ self-assembly methods, Co,Ni-LDH@ZIF-8 nanocomposites were prepared , and undergo high-temperature treatment in an air atmosphere to form a three-metal oxide/carbon material with hierarchical structure characteristics, optimizing its electromagnetic parameters and wave-absorbing properties.
The close combination of bimetallic LDH nanosheets and ZIF-8 is achieved to form a stable structure, which significantly improves the microwave absorption performance and electromagnetic response capability of the material. It has commercial application prospects, and the preparation process is simple, low energy consumption, and suitable for large-scale Production.
Smart Images

Figure CN118772840A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a hierarchical two-dimensional tri-metal oxide / carbon material, a preparation method and application thereof, and belongs to the technical field of microwave attenuation materials. Background Art
[0002] As we all know, the microwave attenuation performance of materials is not only highly related to the intrinsic electromagnetic properties of each component of the microwave absorber, but also closely related to its microstructure. Therefore, focusing on the composition and microstructure design of the material is of great significance to obtaining high-performance microwave absorption (wave absorbing) materials. Among them, the construction of two-dimensional (2D) hierarchical multi-component nanocomposites has many advantages in achieving the improvement of material absorbing performance, mainly including the following aspects: 1. The 2D hierarchical structure can increase the response cross-section of the material to microwaves; 2. The 2D hierarchical structure can improve the impedance matching between the material and the free medium; 3. The multi-component nanostructure can not only provide a variety of loss conditions, but also effectively enhance the interface polarization; 4. The 2D hierarchical structure plays an important role in reducing the density and wear resistance of the material and increasing the adaptability of the material to multiple scenarios, and has a good guiding role in the design of high-efficiency absorbing materials. When 2D materials are studied as absorbing materials, they are usually used as supporting materials. Due to their large cross-section, they provide a rich skeleton platform for the composite of heterogeneous components. Common 2D materials include graphene, two-dimensional transition metal carbonitride (MXene), etc. However, their relatively expensive price, harsh material preparation environment and cumbersome post-processing conditions have caused certain obstacles to their wider application development. Therefore, how to explore and prepare 2D composite absorbing materials with good economic value and application potential has always been our main concern and research content.
[0003] Layered double hydroxide (LDH) materials exhibit two-dimensional structural characteristics and are usually composed of binary transition metal compounds (Al 3+ 、Co 2+ 、Zn 2+ , Mn 2+ , Fe 2+ 、Ni 2+ As a microwave absorbing material, it has unique composition and structural advantages, which can not only provide a larger microwave signal receiving cross section, but also provide an efficient microwave loss medium. In a recent study, we used ferromagnetic metal materials (Co 2+ 、Ni 2+), using 2-methylimidazole as an induction agent, a simple material preparation method was used to successfully prepare Co, Ni-LDH nanosheets with 2D structural characteristics at room temperature. After high-temperature heat treatment, its derivatives showed good microwave absorption performance, but limited by the single composition of Co, Ni-LDH nanosheet derivatives, its structural advantages and microwave absorption capacity were not effectively exerted. Based on this consideration, how to take advantage of its composition and structural advantages and use green, efficient and simple methods to prepare materials with excellent microwave absorption performance has important research and application value.
[0004] Metal-organic framework materials (MOFs) are usually nano-sized porous structural materials due to their designable composition and flexible structure. They are rich in variety and diverse in structure. They have been widely and deeply studied in many fields, and also have important research in the field of microwave absorption. Based on the above analysis, we combine the excellent properties of LDH and MOF, use 2D material LDH nanosheets as the supporting template, and construct a nanocomposite material combining LDH and MOF to promote the formation of multi-component and multi-interface, thereby realizing the transfer of excellent performance between materials of different scales. The hierarchical nanocomposite prepared by designing LDH nanosheets loaded with MOF (Co, Ni-LDH@ZIF-8) can enhance the charge separation and electron transfer in the material, increase the interface polarization and relaxation process, increase the unit receiving area of the composite material for electromagnetic signals, and tune the synergistic attenuation of multiple components, and then prepare high-performance and multi-level microwave absorbing materials. However, there are few designs and studies on this type of two-dimensional hierarchical nanocomposite microwave absorbing materials constructed by combining MOF and LDH. The use of simple material preparation technology, low energy consumption to achieve a uniform and effective combination of the two and give the material performance improvement, long-term stability, energy saving and environmental protection, high efficiency and economic benefits, and meet the needs of industrial production are our long-term focus. Therefore, based on the above analysis and discussion, it is urgent to carry out and solve the research work of designing, preparing and adjusting the two-dimensional hierarchical structure Co, Ni-LDH@ZIF-8 derived absorbing materials with good impedance matching and microwave attenuation characteristics by simple, economical, environmentally friendly and efficient means. Summary of the invention
[0005] The purpose of the present invention is to provide an economical, environmentally friendly, efficient, safe and rapid preparation method of a zeolite imidazolate framework (ZIF-8) material loaded with 2D layered LDH nanosheets, so that it has commercial application prospects, and the derivatives of this type of material exhibit two-dimensional hierarchical structural characteristics and have excellent microwave attenuation performance.
[0006] The technical solution of the present invention:
[0007] A method for preparing a hierarchical two-dimensional trimetallic oxide / carbon material comprises the following steps:
[0008] S1 uniformly mixes water, methanol, divalent nickel salt and divalent cobalt salt according to a preset ratio to obtain a mixed solution A;
[0009] S2: adding a predetermined amount of the imidazole compound methanol solution dropwise to the mixed solution A to obtain a mixed solution B;
[0010] S3 centrifuges the mixed solution B, washes and dries the centrifugal product, and obtains 2D layered bimetallic Co, Ni-LDH nanosheet material.
[0011] S4 ultrasonically disperses the 2D layered Co, Ni-LDH nanosheets obtained in S3 in a mixed solvent of methanol and water in a preset ratio to obtain a mixed solution C;
[0012] In the mixed solution C, the mass / volume ratio of the Co, Ni-LDH nanosheet material to the methanol and water mixed solvent is 1-8 mg / ml, and the volume ratio of methanol to water is 1-4:1;
[0013] S5, while continuously stirring the mixed solution C, adding a preset amount of zinc nitrate hexahydrate to the mixed dispersion C to obtain a mixed solution D;
[0014] S6: adding the imidazole compound methanol solution dropwise to the mixed solution D according to a preset amount to obtain a mixed solution E;
[0015] S7: centrifuging the mixed solution E, washing and drying the centrifugal product to obtain a hierarchical two-dimensional tri-metal oxide / carbon material.
[0016] Preferably, in S1, in the mixed solution A, the volume ratio of water to methanol is 1:1, the molar ratio of divalent cobalt salt to divalent nickel salt is 3:5, and the divalent nickel salt and the divalent cobalt salt are hydrochloride or nitrate of nickel and cobalt, respectively;
[0017] In S2, in the mixed solution B, the molar ratio of the total amount of the mixed metal salt to the imidazole compound is 1:5, and the volume ratio of methanol to water is 2:1; the metal salt is composed of the divalent nickel salt and the divalent cobalt salt in the mixed solution A.
[0018] Preferably, the S1 specifically comprises the following steps:
[0019] First, 20 ml of methanol and 20 ml of water were measured respectively, added into a beaker, and then 6 mmol of nickel salt and 3.6 mmol of cobalt salt were added to obtain a mixed solution A.
[0020] Preferably, the S2 specifically includes the following steps:
[0021] At room temperature, using a magnetic stirrer at a rate of 400 revolutions per minute for 2 to 3 hours, during which time, the dropwise addition of the imidazole compound methanol solution is completed, and after the dropwise addition is completed, the stirring is continued at a rate of 400 revolutions per minute for 3 to 5 hours;
[0022] The preparation method of the imidazole compound methanol solution is as follows: weigh 48 mmol of 2-methylimidazole into a beaker and add 20 ml of methanol, and dissolve the mixture with ultrasound to obtain the imidazole compound methanol solution.
[0023] Preferably, in step S4, 60 mg of 2D layered Co, Ni-LDH nanosheets are added to a mixed solution of 20 ml of methanol and 10 ml of water and ultrasonically dispersed to obtain a mixed solution C.
[0024] Preferably, in step S5, while continuously stirring the mixed solution C, 1.8 mmol of zinc nitrate hexahydrate is added to the mixed solution C, and the mixed solution C is stirred at a constant speed of 400 rpm by a magnetic stirrer for 0.5 to 2 hours. The setting of appropriate stirring speed and stirring time is intended to increase the Zn 2+ The contact opportunities on the surface of LDH nanosheets and the promotion of adsorption uniformity between the two provide sufficient reaction conditions for the subsequent uniform growth of ZIF-8.
[0025] Preferably, in step S6, the method for preparing the methanol solution of imidazole compounds comprises the following steps: weighing 24 mmol of 2-methylimidazole into a beaker and adding 10 ml of methanol, and dissolving by ultrasonic assistance. The use of an appropriate ratio of 2-methylimidazole organic ligand and solvent can effectively avoid excessive addition of raw materials and solvents, effectively promoting the reaction while avoiding economic waste.
[0026] Preferably, in the steps S3 and S7, the cleaning is performed by washing with a methanol solution, the number of washings is 4 times, and the drying condition is vacuum drying in a 60°C environment. Methanol as a reaction solvent has good solubility for metal ions and organic ligands. After the reaction is completed, it can be used as a cleaning liquid to wash away a small amount of metal ions and organic ligands that are not involved, thereby improving the purity of the product. In addition, the boiling point of the methanol solvent is low, and it can evaporate and dry at a relatively low temperature. The purpose of selecting vacuum drying is to achieve a rapid drying effect in a very short time.
[0027] The present invention also provides a hierarchical two-dimensional trimetal oxide / carbon material prepared by the above preparation method, wherein the hierarchical two-dimensional trimetal oxide / carbon material is a hierarchical Co, Ni-LDH nanosheet loaded with a zeolite imidazolate framework ZIF-8.
[0028] The present invention also provides the application of hierarchical two-dimensional trimetal oxide / carbon material in electromagnetic wave absorption, comprising the following steps: placing the hierarchical two-dimensional trimetal oxide / carbon material in an open tubular furnace, heating to 400°C, and keeping warm at 400°C for 1 hour to obtain a high-temperature treated product; mixing the high-temperature treated product with paraffin in proportion, the mixing ratio being a mass ratio of product to paraffin of 4:1, to form a coaxial annular sheet with an inner diameter of 3.04 mm, an outer diameter of 7.00 mm and a thickness of 2 mm; the calcination process setting in a 400°C air environment is intended to promote the conversion of metal substances and organic substances into magnetic metal oxides and graphite carbon to form a material with effective electromagnetic response characteristics. Its advantage is that compared with the commonly used high-temperature argon environment calcination behavior, it has a low calcination temperature (low energy consumption) and a wide distribution of air atmosphere (high economic benefits). In addition, compared with the metal element substance obtained by high-temperature reduction in an argon environment, the metal oxide obtained by calcining in an air atmosphere has the characteristics of corrosion resistance and oxidation resistance, and has a wider application environment.
[0029] Use vector network analyzer to test electromagnetic parameters in the 2-18GHz frequency band;
[0030] Agilent PNA software was used to output electromagnetic parameters according to the Nicolson and Ross and Weir algorithm;
[0031] When the thickness is 1.7 mm, the maximum absorption intensity is -67.61 dB; when the thickness is 1.75 mm, the maximum absorption width is 5.8 GHz.
[0032] Compared with the existing related technologies, the present invention has the following significant advantages:
[0033] 1. For bimetallic LDH nanosheets loaded with zeolite imidazolate framework (Co, Ni-LDH@ZIF-8), (1) the implementation conditions of the present invention are safe, mild, efficient, economical, and environmentally friendly. Under room temperature, bimetallic LDH nanosheets loaded with zeolite imidazolate framework material are obtained by stirring in situ self-assembly growth in a methanol and water mixed solution system. Zn 2+ The electrostatic force between the anions of the imidazole compound and the LDH nanosheets causes Zn 2+Depositing on the surface of Co, Ni-LDH nanosheets, the in-situ growth process promotes the close combination of ZIF-8 and Co, Ni-LDH, thereby forming an LDH nanosheet@ZIF-8 composite material with stable structural characteristics; (2) the optimal volume ratio of the mixed reaction solvent is selected to be Vmethanol:Vwater=1-4:1; (3) the present invention uses the prepared bimetallic Co, Ni-LDH nanosheets as a template, utilizes the controllable growth characteristics of MOF (ZIF-8) with easily adjustable elemental composition and structure, and grows and constructs Co, Ni-LDH@ZIF-8 at room temperature, and the performance of the derived hierarchical structure nanocomposite material has a high degree of designability and adjustability;
[0034] Second, for the two-dimensional hierarchical structure Co, Ni-LDH@ZIF-8 derived electromagnetic absorption materials, (1) the multi-component synergistic effect of bimetallic LDH nanosheets and ZIF-8 composite material derivatives, as well as the construction of multilayer structures, further promotes the performance transfer between different levels of interfaces and different scales, improves the material's response to electromagnetic waves, and thus enhances the material's absorption performance; (2) the three metal ions (Co from bimetallic Co, Ni-LDH and monometallic Zn-ZIF-8) 2+ 、Ni 2+ 、Zn 2+ ) precursor, which enhances the electromagnetic performance response of the composite material and optimizes the electromagnetic parameters of the material; (3) air is selected as the high-temperature treatment atmosphere to avoid the use of expensive inert gases (argon or nitrogen, etc.), which has the characteristics of energy saving, safety, environmental protection, and economy.
[0035] 3. The reaction process of the present invention is simple, the temperature is low, it is easy to control and does not require large-scale equipment and harsh reaction conditions, and can achieve large-scale mass production.
[0036] 4. The material prepared by the present invention has good electromagnetic response absorption behavior, and the size density of the sample is small. When added in a low proportion in a matrix such as paraffin, excellent wave absorbing performance can be obtained. The sample is in powder form and can be mixed with alloy flakes and organic solvents and then coated on a polymer film to form an absorption sheet for use. It can be processed into any shape according to the needs of use and can also be used as a coating additive. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 This is a scanning electron microscope image of the Co,Ni-LDH-30@ZIF-8 sample prepared in Example 1 of the present invention.
[0038] Figure 2 This is a scanning electron microscope image of the Co,Ni-LDH-60@ZIF-8 sample prepared in Comparative Example 1 of the present invention.
[0039] Figure 3This is a scanning electron microscope image of the Co,Ni-LDH-120@ZIF-8 sample prepared in Comparative Example 2 of the present invention.
[0040] Figure 4 This is a scanning electron microscope image of the Co,Ni-LDH-240@ZIF-8 sample prepared in Comparative Example 3 of the present invention.
[0041] Figure 5 These are electronic photographs of Co,Ni-LDH-30@ZIF-8, Co,Ni-LDH-60@ZIF-8, Co,Ni-LDH-120@ZIF-8, and Co,Ni-LDH-240@ZIF-8 samples in the present invention before and after high-temperature treatment.
[0042] Figure 6 These are the XRD patterns of Co,Ni-LDH-30@ZIF-8, Co,Ni-LDH-60@ZIF-8, Co,Ni-LDH-120@ZIF-8, and Co,Ni-LDH-240@ZIF-8 samples in the present invention.
[0043] Figure 7 These are the XRD patterns of Co,Ni-LDH-30@ZIF-8-D, Co,Ni-LDH-60@ZIF-8-D, Co,Ni-LDH-120@ZIF-8-D, and Co,Ni-LDH-240@ZIF-8-D samples in the present invention.
[0044] Figure 8 This is a scanning electron microscope image of the Co,Ni-LDH-30@ZIF-8-D sample in the present invention.
[0045] Fig. 9 This is a scanning electron microscope image of the Co,Ni-LDH-60@ZIF-8-D sample in the present invention.
[0046] Fig.10 This is a scanning electron microscope image of the Co,Ni-LDH-120@ZIF-8-D sample in the present invention.
[0047] Fig.11 This is a scanning electron microscope image of the Co,Ni-LDH-240@ZIF-8-D sample in the present invention.
[0048] Fig.12 This is a diagram of the microwave absorption performance of the Co,Ni-LDH-30@ZIF-8-D sample in the present invention.
[0049] Fig.13 This is a diagram of the microwave absorption performance of the Co,Ni-LDH-60@ZIF-8-D sample in the present invention.
[0050] Fig.14 This is a diagram of the microwave absorption performance of the Co,Ni-LDH-120@ZIF-8-D sample in the present invention.
[0051] Fig.15 This is a diagram of the microwave absorption performance of the Co,Ni-LDH-240@ZIF-8-D sample in the present invention. DETAILED DESCRIPTION
[0052] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the present invention is further explained below in conjunction with specific implementation methods.
[0053] The present invention is inspired by the high aspect ratio and high specific surface area of two-dimensional hierarchical structure materials for high reception rate of electromagnetic waves, as well as the promotion effect of the formation of multi-component and multi-interface structures of hierarchical structure materials on the improvement of composite material absorption performance. We firstly realize the effective combination of two-dimensional layered bimetallic Co, Ni-LDH nanosheet metal organic framework structure (ZIF-8) thin layers by utilizing the in-situ self-assembly controllable growth process, and then successfully construct a trimetallic oxide / carbon composite absorber with hierarchical structure characteristics by using temperature-controlled pyrolysis technology in air atmosphere. At present, the combination of LDH and MOF is mainly used in the fields of photoelectrocatalysis, energy, and electrochemical equipment. Compared with the electrocatalytic oxygen reduction catalyst developed by Li et al. based on CoAl-LDH@ZIF-67 composite material, the Co, Ni-LDH@ZIF-8 composite material prepared by the present invention has the advantages of reasonable material selection and simple preparation method. In the preparation process of CoAl-LDH@ZIF-67 composite material, the preparation of CoAl-LDH was prepared by reflux heating (97℃), and the reaction time was as long as 48 hours. In this work, the preparation of Co, Ni-LDH can be completed by stirring at room temperature for 3 to 5 hours, which has the advantages of short time and low energy consumption. Secondly, in terms of component selection, the combination of ferromagnetic metal substances cobalt and nickel greatly increases the magnetic response loss performance of the material. ZIF-8 is selected as the composite component, and its derivative ZnO component with semiconductor properties also increases the dielectric loss performance of the material. They are of great significance to the improvement of the composite material's wave absorption performance. Therefore, the combination of Co, Ni-LDH@ZIF-8 broadens the research prospects of combining LDH and MOF to develop wave absorbing materials. This type of nanocomposite wave absorbing material exhibits adjustable electromagnetic response characteristics and has good electromagnetic wave absorption performance.
[0054] The present invention provides a simple, economical, environmentally friendly and rapid preparation method of a layered bimetallic Co, Ni-LDH nanosheet-loaded zeolite imidazolate framework ZIF-8 material, which has commercial application prospects, and the derivatives of this type of nanocomposite material have good electromagnetic wave absorption performance. The two-dimensional layered bimetallic LDH nanosheet-loaded zeolite imidazolate framework ZIF-8 nanocomposite material is composed of an ultrasonic dispersion of bimetallic Co, Ni-LDH nanosheets, zinc ions (Zn 2+ ), a metal ion solution system composed of LDH nanosheets, methanol, and water in a certain proportion is mixed and dispersed, and then stirred with an imidazole compound at room temperature for 3 to 5 hours to obtain a two-dimensional layered Co, Ni-LDH@ZIF-8 nanocomposite material. In this method, the preferred volume ratio of methanol and water in the mixed reaction solution is Vmethanol: Vwater = 1 to 4: 1; then the bimetallic Co, Ni-LDH nanosheet-loaded zeolite imidazolate framework ZIF-8 material (Co, Ni-LDH@ZIF-8) prepared above is treated by a suitable treatment method to obtain an electromagnetically responsive absorbing material. The preferred process is as follows: weigh a certain mass of Co, Ni-LDH@ZIF-8 material in a tubular furnace, in an air atmosphere, the heating rate is 3°C / min, the furnace temperature is adjusted to 400°C, and after keeping warm for 1 hour, naturally cool down to obtain a Co, Ni-LDH@ZIF-8-D material with electromagnetic response characteristics. The present invention is further described below by examples:
[0055] Example 1
[0056] The preparation method of the zeolite imidazolate framework nanoparticle modified bimetallic LDH nanosheet material sample Co, Ni-LDH-60@ZIF-8 of the present invention is as follows:
[0057] First, 20 ml of methanol and 20 ml of water were measured in a 100 ml beaker, and 1.43 g of nickel chloride hexahydrate and 0.86 g of cobalt chloride hexahydrate were added to the mixed solution, and then mixed and stirred at room temperature (about 400 rpm) for 3 hours; during this time, 2-methylimidazole methanol solution was prepared, and 3.94 g of 2-methylimidazole was weighed and dissolved in 20 ml of methanol solution with ultrasound assistance; then, the prepared 2-methylimidazole methanol solution was slowly added to Co under stirring. 2+ and Ni 2+ The mixture is placed in a mixed metal ion solution and stirred for 3 to 5 hours, and then centrifuged, washed with methanol, and vacuum dried to obtain a two-dimensional layered bimetallic Co, Ni-LDH nanosheet material;
[0058] Next, 60 mg of two-dimensional layered bimetallic Co, Ni-LDH nanosheets (2 mg / ml) were dispersed in a mixed solvent of 20 ml methanol and 10 ml water, and ultrasonic-assisted dispersion was performed for 10 minutes. 0.54 g zinc nitrate hexahydrate was added, and then uniformly mixed and stirred (about 400 rpm) at room temperature for 1 hour; during this time, a 2-methylimidazole methanol solution was prepared, and 1.97 g of 2-methylimidazole was weighed and ultrasonically dissolved in 20 ml of methanol solution; the uniform stirring process was continued, and the prepared 2-methylimidazole methanol solution was slowly added dropwise to the above-mentioned mixed metal ion solution, and the stirring reaction was continued for 4 hours. Co, Ni-LDH-60@ZIF-8 was obtained through centrifugation, methanol washing, vacuum drying and other processes.
[0059] Figure 1 This is a scan of the sample Co,Ni-LDH-60@ZIF-8. Figure 1 It can be seen that the layered bimetallic Co,Ni-LDH nanosheets are used as the matrix material, and the zeolite imidazolate framework ZIF-8 is evenly distributed on the nanosheets to form a tightly attached layer, forming a hierarchical structure Co,Ni-LDH-60@ZIF-8 material.
[0060] Comparative Example 1
[0061] The same preparation process as in Example 1 was adopted for the two-dimensional layered bimetallic Co, Ni-LDH nanosheet material; subsequently, the content of the two-dimensional layered bimetallic Co, Ni-LDH nanosheets in Example 1 was changed to 30 mg (1 mg / ml), and the other implementation conditions and steps were exactly the same as in Example 1 to obtain Co, Ni-LDH-30@ZIF-8.
[0062] Figure 2 This is the scanning electron microscope image of the sample Co,Ni-LDH-30@ZIF-8. Figure 2 It can be seen that the Co,Ni-LDH-30@ZIF-8 obtained in this case presents the same two-dimensional hierarchical structural characteristics as Co,Ni-LDH-60@ZIF-8, and ZIF-8 is uniformly dispersed and stably bound to the surface of Co,Ni-LDH.
[0063] Comparative Example 2
[0064] The same preparation process as in Example 1 was adopted for the two-dimensional layered bimetallic Co, Ni-LDH nanosheet material; subsequently, the content of the two-dimensional layered bimetallic Co, Ni-LDH nanosheets in Example 1 was changed to 120 mg (4 mg / ml), and the other implementation conditions and steps were exactly the same as in Example 1 to obtain Co, Ni-LDH-120@ZIF-8.
[0065] Figure 3This is the scanning electron microscope image of the sample Co,Ni-LDH-120@ZIF-8. Figure 3 It can be seen that the Co,Ni-LDH-120@ZIF-8 obtained in this case presents the same two-dimensional hierarchical structural characteristics as Co,Ni-LDH-30@ZIF-8, and ZIF-8 is uniformly dispersed and stably bound to the surface of Co,Ni-LDH.
[0066] Comparative Example 3
[0067] The same preparation process as in Example 1 was adopted for the two-dimensional layered bimetallic Co, Ni-LDH nanosheet material; subsequently, the content of the two-dimensional layered bimetallic Co, Ni-LDH nanosheets in Example 1 was changed to 240 mg (8 mg / ml), and the other implementation conditions and steps were exactly the same as in Example 1 to obtain Co, Ni-LDH-240@ZIF-8.
[0068] Figure 4 This is the scanning electron microscope image of the sample Co,Ni-LDH-240@ZIF-8. Figure 4 It can be seen that the Co,Ni-LDH-240@ZIF-8 obtained in this case presents the same two-dimensional hierarchical structural characteristics as Co,Ni-LDH-30@ZIF-8, and ZIF-8 is uniformly dispersed and stably bound to the surface of Co,Ni-LDH.
[0069] By comparing Example 1 with Comparative Examples 1-3, it can be seen that the present invention prepares a layered bimetallic Co, Ni-LDH nanosheet-loaded zeolite imidazolate framework ZIF-8 nanocomposite material by adjusting the amount of the two-dimensional layered bimetallic Co, Ni-LDH nanosheet material used. In this process, the precursor Zn 2+ The amount of layered bimetallic Co, Ni-LDH nanosheets was adjusted while the amount of 2-methylimidazole was unchanged. The hierarchical structured Co, Ni-LDH and ZIF-8 nanocomposites with uniform combination in different proportions were prepared.
[0070] Preparation and performance test analysis of absorbing samples:
[0071] The present invention further processes the samples prepared in Example 1 and Comparative Examples 1, 2, and 3 to demonstrate their application potential in the field of electromagnetic wave absorption. The steps for preparing the absorbing samples are as follows:
[0072] The samples Co, Ni-LDH-60@ZIF-8, Co, Ni-LDH-30@ZIF-8, Co, Ni-LDH-120@ZIF-8, and Co, Ni-LDH-240@ZIF-8 in the core-shell structure embodiment 1 and comparative examples 1, 2, and 3 were placed in an open tube furnace, and then heated to 400 degrees Celsius for 1 hour, and the samples obtained after high temperature treatment were Co, Ni-LDH-60@ZIF-8-D, Co, Ni-LDH-30@ZIF-8-D, Co, Ni-LDH-120@ZIF-8-D, and Co, Ni-LDH-240@ZIF-8-D, respectively. The heating rate was 3 degrees Celsius per minute. Subsequently, Co,Ni-LDH-60@ZIF-8-D, Co,Ni-LDH-30@ZIF-8-D, Co,Ni-LDH-120@ZIF-8-D, and Co,Ni-LDH-240@ZIF-8-D were mixed with paraffin to prepare electromagnetic parameter test samples.
[0073] Figure 5 The electron photos of Co,Ni-LDH-30@ZIF-8, Co,Ni-LDH-60@ZIF-8, Co,Ni-LDH-120@ZIF-8, and Co,Ni-LDH-240@ZIF-8 samples before and after high temperature treatment are shown in Figure 1. The samples are in powder form before and after high temperature treatment. Due to the consistency of elemental composition, there is no obvious color difference between the samples before high temperature treatment. The samples before high temperature treatment are all light yellow, and the products after high temperature treatment are consistent black.
[0074] Figure 6 The X-ray diffraction patterns of Co,Ni-LDH-30@ZIF-8, Co,Ni-LDH-60@ZIF-8, Co,Ni-LDH-120@ZIF-8, and Co,Ni-LDH-240@ZIF-8 samples show that the prepared nanocomposites have the crystal structure characteristics of both Co,Ni-LDH and ZIF-8, and also prove the effective combination of the two substances.
[0075] Figure 7These are the XRD patterns of samples Co,Ni-LDH-30@ZIF-8-D, Co,Ni-LDH-60@ZIF-8-D, Co,Ni-LDH-120@ZIF-8-D, and Co,Ni-LDH-240@ZIF-8-D after high-temperature treatment. It can be seen from the figure that compared with the samples before high-temperature treatment, the samples after high-temperature treatment undergo obvious changes in physical properties, among which the metal components undergo obvious material transformation. Since the samples are treated at high temperature in an air environment, the metal substances of each component are converted into their respective metal oxides to form a trimetallic oxide complex.
[0076] Figure 8 , 9 , 10, and 11 are scanning electron microscope images of the samples Co,Ni-LDH-60@ZIF-8-D, Co,Ni-LDH-30@ZIF-8-D, Co,Ni-LDH-120@ZIF-8-D, and Co,Ni-LDH-240@ZIF-8-D after high temperature treatment, respectively. It can be seen from the figures that the products after high temperature treatment still retain the original two-dimensional layered structure, and dense nanoparticles are evenly distributed on the surface of the two-dimensional sheets. These particles mainly come from ZIF-8 high temperature derived metal oxides and carbon composites.
[0077] The electromagnetic parameters of samples Co,Ni-LDH-30@ZIF-8-D, Co,Ni-LDH-60@ZIF-8-D, Co,Ni-LDH-120@ZIF-8-D, and Co,Ni-LDH-240@ZIF-8-D were calculated and analyzed to draw reflection loss curves at different absorber thicknesses, such as Figures 12 to 15 As shown in the figure, it can be seen that Co,Ni-LDH-30@ZIF-8-D, Co,Ni-LDH-60@ZIF-8-D, Co,Ni-LDH-120@ZIF-8-D, and Co,Ni-LDH-240@ZIF-8-D all exhibit excellent electromagnetic wave absorption performance at different calculated thicknesses. Fig.12 The reflection loss curve of Co,Ni-LDH-30@ZIF-8-D sample at different thicknesses is shown. When the thickness is 2.33 mm, the maximum absorption width is 5.8 GHz, and when the thickness is 6.0 mm, the maximum absorption intensity reaches -30.78 dB. Fig.13 The reflection loss curves of Co,Ni-LDH-60@ZIF-8-D samples at different thicknesses are shown. When the thickness is 1.75 mm, the maximum absorption width is -5.6 GHz, and when the thickness is 1.71 mm, the maximum absorption intensity is -67.61 dB. Compared with the previously prepared Co,Ni-LDH nanosheets (RL min =-20.06dB,EABmax =4.76GHz), with significant improvements in both absorption intensity (increased by approximately -47.5dB) and absorption bandwidth (increased by approximately 1GHz). Fig.14 The reflection loss curve of the sample Co,Ni-LDH-120@ZIF-8-D at different thicknesses is shown. When the thickness is 2.76 mm, the maximum reflection loss value is -59.09 dB, and when the thickness is 1.8 mm, the maximum absorption width is 5.52 GHz. Fig.15 The reflection loss curve of the sample Co, Ni-LDH-240@ZIF-8-D at different thicknesses is shown. When the thickness is 2.87 mm, the maximum absorption intensity is -56.2 dB, and when the thickness is 1.92 mm, the effective absorption width is 5.52 GHz. In summary, the hierarchical bimetallic Co, Ni-LDH nanosheets loaded with zeolite imidazolate framework ZIF-8 materials have excellent electromagnetic wave absorption performance.
[0078] The electromagnetic reflection loss value in the case analysis is derived from the calculation of electromagnetic parameters. The electromagnetic parameter test is tested in the 2-18 GHz frequency band using a network analyzer (VNA, N5245A, Agilent, USA). The mass ratio of samples Co, Ni-LDH-60@ZIF-8-D, Co, Ni-LDH-30@ZIF-8-D, Co, Ni-LDH-120@ZIF-8-D, Co, Ni-LDH-240@ZIF-8-D to paraffin is 1:4. All samples are pressed into standard ring holes (inner diameter: 3.04 mm, outer diameter 7.00 mm) by the same mold to maintain the certainty of the geometric shape. The thickness of all rings is maintained at 2 mm. Agilent PNA software automatically outputs relevant electromagnetic parameters according to the Nicolson and Ross and Weir algorithm.
[0079] The present invention uses 2-methylimidazole to induce the formation of cobalt and nickel bimetallic LDH nanosheets at room temperature, and then uses the prepared Co, Ni-LDH nanosheets as a matrix to load a zeolite imidazolate framework ZIF-8 composite material, and performs high-temperature heat treatment in an air environment to obtain a trimetallic oxide / C nanocomposite material with hierarchical structural characteristics. In this process, the optimal ratio of the content of the bimetallic Co, Ni-LDH nanosheets to the mixed metal ions is selected, and the imidazole compound is used as the interlayer anion substance of the hydrotalcite and the Zn 2+ The electrostatic force between Zn 2+The coordination effect between Zn-ZIF-8 and 2-methylimidazole, using a mixed solution of water and methanol as a reaction solvent, finally makes Zn-ZIF-8 uniformly and stably combined and evenly distributed on the surface of Co, Ni-LDH to form a two-dimensional hierarchical structure. Subsequently, high-temperature heat treatment is used to construct a more refined two-dimensional hierarchical structure material. The porous, lightweight, and uniformly distributed two-dimensional trimetallic oxide / carbon nanocomposite material obtained by high-temperature thermal conversion in an air atmosphere can overcome the shortcomings of the unit counterpart. The electromagnetic parameters of the composite material are adjusted by regulating the composition content of metal ions and the number of interfaces. The synergistic effect and interface effect generated by the multi-element magnetoelectric composite further improve the impedance matching and attenuation performance of the material, so that the electromagnetic absorption performance of the hierarchical composite material is significantly improved, thereby making it have excellent potential as an electromagnetic wave absorption material. The invention has a simple preparation process, low temperature, easy control, and does not require large-scale equipment and harsh reaction conditions, and can achieve large-scale mass production.
[0080] The above-mentioned examples are merely examples for clearly explaining the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes can be made based on the description. It is not necessary and impossible to list all the embodiments here. However, these obvious changes or modifications derived from the spirit of the present invention are still within the scope of protection of the present invention.
Claims
1. A method for preparing a hierarchical two-dimensional trimetallic oxide / carbon material, characterized in that: The following steps are involved: S1 uniformly mixes water, methanol, divalent nickel salt and divalent cobalt salt according to a preset ratio to obtain a mixed solution A; S2: adding a predetermined amount of the imidazole compound methanol solution dropwise to the mixed solution A to obtain a mixed solution B; S3 centrifuges the mixed solution B, washes and dries the centrifugal product to obtain a 2D layered bimetallic Co, Ni-LDH nanosheet material; S4 ultrasonically disperses the 2D layered Co, Ni-LDH nanosheets obtained in S3 in a mixed solvent of methanol and water in a preset ratio to obtain a mixed solution C; In the mixed solution C, the mass / volume ratio of the Co, Ni-LDH nanosheet material to the methanol and water mixed solvent is 1-8 mg / ml, and the volume ratio of methanol to water is 1-4:1; S5, while continuously stirring the mixed solution C, adding a preset amount of zinc nitrate hexahydrate to the mixed dispersion C to obtain a mixed solution D; S6: adding the imidazole compound methanol solution dropwise to the mixed solution D according to a preset amount to obtain a mixed solution E; S7: centrifuging the mixed solution E, washing and drying the centrifugal product to obtain a hierarchical two-dimensional tri-metal oxide / carbon material.
2. The method for preparing a hierarchical two-dimensional trimetallic oxide / carbon material according to claim 1, characterized in that: In S1, in the mixed solution A, the volume ratio of water to methanol is 1:1, the molar ratio of divalent cobalt salt to divalent nickel salt is 3:5, and the divalent nickel salt and the divalent cobalt salt are hydrochloride or nitrate of nickel and cobalt, respectively; In S2, in the mixed solution B, the molar ratio of the total amount of the mixed metal salt to the imidazole compound is 1:5, and the volume ratio of methanol to water is 2:1; the metal salt is composed of the divalent nickel salt and the divalent cobalt salt in the mixed solution A.
3. The method for preparing a hierarchical two-dimensional trimetallic oxide / carbon material according to claim 1, characterized in that: The S1 specifically includes the following steps: First, 20 ml of methanol and 20 ml of water were measured respectively, added into a beaker, and then 6 mmol of nickel salt and 3.6 mmol of cobalt salt were added to obtain a mixed solution A.
4. The method for preparing a hierarchical two-dimensional trimetallic oxide / carbon material according to claim 1, characterized in that: The S2 specifically includes the following steps: At room temperature, using a magnetic stirrer at a rate of 400 revolutions per minute for 2 to 3 hours, during which time, the dropwise addition of the imidazole compound methanol solution is completed, and after the dropwise addition is completed, the stirring is continued at a rate of 400 revolutions per minute for 3 to 5 hours; The preparation method of the imidazole compound methanol solution is as follows: weigh 48 mmol of 2-methylimidazole into a beaker and add 20 ml of methanol, and dissolve the mixture with ultrasound to obtain the imidazole compound methanol solution.
5. The method for preparing a hierarchical two-dimensional trimetallic oxide / carbon material according to claim 1, characterized in that: In the step S4, 60 mg of 2D layered Co, Ni-LDH nanosheets are added to a mixed solution of 20 ml of methanol and 10 ml of water and ultrasonically dispersed to obtain a mixed solution C.
6. The method for preparing a hierarchical two-dimensional trimetallic oxide / carbon material according to claim 1, characterized in that: In the step S5, while the mixed solution C is continuously stirred, 1.8 mmol of zinc nitrate hexahydrate is added to the mixed solution C, and the mixed solution is stirred uniformly at a rate of 400 rpm by a magnetic stirrer for 0.5 to 2 hours.
7. The method for preparing a hierarchical two-dimensional trimetallic oxide / carbon material according to claim 1, characterized in that: In step S6, the method for preparing the methanol solution of imidazole compounds comprises the following steps: weighing 24 mmol of 2-methylimidazole into a beaker and adding 10 ml of methanol, and dissolving by ultrasound.
8. The method for preparing a hierarchical two-dimensional trimetallic oxide / carbon material according to claim 1, characterized in that: In the steps S3 and S7, the cleaning is performed by using a methanol solution, the number of cleaning times is 4 times, and the drying condition is vacuum drying in an environment of 60°C.
9. The hierarchical two-dimensional trimetallic oxide / carbon material prepared by the preparation method according to any one of claims 1 to 8, characterized in that: The hierarchical two-dimensional trimetallic oxide / carbon material is a hierarchical Co, Ni-LDH nanosheet loaded with a zeolite imidazolate framework ZIF-8.
10. Application of a hierarchical two-dimensional trimetallic oxide / carbon material in electromagnetic wave absorption, characterized in that: The method comprises the following steps: placing the hierarchical two-dimensional trimetallic oxide / carbon material in an open tube furnace, heating it to 400° C., and keeping it at 400° C. for 1 hour to obtain a high-temperature treated product; mixing the high-temperature treated product with paraffin wax in a proportion, wherein the mass ratio of the product to the paraffin wax is 4:1, to prepare a coaxial annular sheet with an inner diameter of 3.04 mm, an outer diameter of 7.00 mm, and a thickness of 2 mm; Use vector network analyzer to test electromagnetic parameters in the 2-18GHz frequency band; Agilent PNA software was used to output electromagnetic parameters according to the Nicolson and Ross and Weir algorithm; When the thickness is 1.7 mm, the maximum absorption intensity is -67.61 dB; when the thickness is 1.75 mm, the maximum absorption width is 5.8 GHz.