Process for smelting 26NiCrMoV14-5 ultrahigh-purity steel large steel ingot through electric arc furnace
Through the combination of electric arc furnace smelting and refining processes, the efficient production of 26NiCrMoV14-5 ultra-high purity steel is achieved, solving the problem of element and inclusion control, improving the success rate and market competitiveness, and reducing environmental pollution through waste reuse .
Patent Information
- Application Number
- CN202410794958.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-19
- Publication Date
- 2024-10-15
AI Technical Summary
It is difficult to effectively produce 26NiCrMoV14-5 ultra-high purity steel with existing technology, especially the control of Mn, Si, P, S and other elements and inclusions is not up to standard, and the cost is high and the success rate is low, which affects market competitiveness.
Using electric arc furnace smelting combined with LF refining, VD refining and VCD vacuum casting process, through double slag smelting and refining slagging deoxidation process, the amount of oxygen and slag is controlled, multiple slag making and blowing oxidation operations are performed, combined with vacuum casting and Mold slag protection ensures the uniformity and purity of molten steel composition.
The purity and composition control of 26NiCrMoV14-5 ultra-high purity steel are improved, the production success rate is improved, the cost is reduced, the market competitiveness is enhanced, and environmental pollution is reduced through waste reuse.
Smart Images

Figure SMS_10 
Figure SMS_11 
Figure SMS_12
Abstract
Description
Technical Field
[0001] The invention belongs to the field of steelmaking and relates to a process for smelting large-scale 26NiCrMoV14-5 ultra-high purity steel ingots in an electric arc furnace. Background Art
[0002] Pure steel refers to steel that has low content of other impurity elements in addition to strict control of non-metallic inclusions in the steel; the impurity elements in steel generally refer to O, S, P, N, H, O+P+S+N+H≤80ppm, and also includes controlling elements such as Pb, As, Sb, Bi, Cu, Sn in the steel. This is mainly because the above-mentioned trace elements are difficult to remove during the steelmaking process. With the continuous return of scrap steel, these trace elements are continuously enriched in the steel, and their harmful effects are becoming increasingly prominent.
[0003] At present, the success rate of producing 26NiCrMoV14-5 ultra-high purity steel is extremely low, mainly because the control of elements such as Mn, Si, P, S and inclusions cannot meet the requirements. In addition, the cost is too high and the market competitiveness is weak. Summary of the invention
[0004] The purpose of the present invention is to provide a process for smelting large-scale 26NiCrMoV14-5 ultra-high purity steel ingots in an electric arc furnace, which solves the problem that the success rate of producing 26NiCrMoV14-5 ultra-high purity steel is extremely low and the control of elements such as Mn, Si, P, S and inclusions cannot meet the requirements.
[0005] The technical solution adopted by the present invention is as follows:
[0006] A process for smelting a large ingot of 26NiCrMoV14-5 ultra-high purity steel in an electric arc furnace comprises the following steps:
[0007] S1. Electric arc furnace smelting: The electric furnace is equipped with Ni4 scrap steel and Mo-containing scrap steel with low Mn, P and S content to ensure sufficient Mo element. The harmful elements As, Sn and Sb in the raw materials meet the requirements of this steel. In terms of mass percentage, the melting component S is ≤0.005% in the melting stage.
[0008] S2, LF refining: After ensuring that there is no oxidized slag, the molten steel is put into the LF furnace, first feed aluminum wire 3-5m / t, then add special synthetic slag 700-800kg, after the synthetic slag is completed, add calcium carbide, Al powder, electrode powder for slag making and deoxidation; when the LF furnace slag becomes white, has good fluidity, temperature ≥1580℃, and uniform composition, take samples for analysis, add alloys when it meets the requirements for adjusting the composition, and tap the steel when the chemical composition and temperature of the molten steel meet the requirements;
[0009] S3, VD refining: accurately position the ladle filled with molten steel on the refining station of the VD furnace for vacuum degassing, and take samples for analysis after vacuum degassing; after vacuum degassing, when Al in the molten steel is ≤ 0.012%, other components meet the standards, and the temperature meets the process control range, vacuum casting is carried out;
[0010] S4, VCD vacuum casting: keep the vacuum degree in the vacuum casting room of the vacuum casting station below 67Pa, control the temperature of the hanging ladle after VD at 1600-1610℃, control the pouring temperature of the tundish at 1550-1560℃, start pouring when the molten steel level in the tundish is greater than or equal to 80% of the height of the tundish, and control the casting speed at 2t / min; after the pouring is completed, immediately add protective slag automatically at 1kg / t after the air breaker is opened. The protective slag adopts pre-melted hollow particle continuous casting protective slag, and then open the can cover to add heating agent, and then add carbonized rice husk for heat preservation. After the die drawing time is up, demold in time and transfer to the forging workshop to heat in the furnace and forge into the steel ingot.
[0011] In the electric arc furnace steelmaking of the present invention, electric energy is used as a heat source, electric energy is input into the furnace through graphite electrodes, an electric arc is generated between the electrode and the charge, and the charge is directly heated by the high temperature of the electric arc; in the present invention, Ni4 scrap steel is matched with Mo-containing scrap steel with low Mn, P and S contents, and an electric arc furnace is used to refine molten steel, and the electric arc furnace directly uses the high temperature of the electric arc to heat the charge, with high thermal efficiency, and in the process of electric arc furnace steelmaking, the slag forms a protective layer on the surface of the molten steel, which can isolate the molten steel from the air, and adsorb impurities in the molten steel and fix harmful element oxides; the oxides in the slag react chemically with the impurity elements to oxidize them, thereby removing them or converting them into a form that is easy to discharge.
[0012] In addition, the present invention utilizes the refining slag deoxidation process, which has good deoxidation and desulfurization effects, high slag basicity, good fluidity, can effectively remove sulfur, and there is no resulfurization phenomenon after VD; the present invention adopts vacuum casting, reasonably controls the casting temperature and casting speed, and the component segregation on large steel ingots is controllable; the present invention adopts double vacuum treatment during VD refining and VCD vacuum casting, and the gas content in the steel is low, the inclusion content is small, and the purity is high. The present invention immediately adds the continuous casting hollow particle protective slag during the pouring and breaking process, which has fast slag removal and no crusting of the cap mouth. The addition of the exothermic agent can quickly burn, the cap mouth shrinks ideally, and the cap mouth utilization rate is high.
[0013] The process of smelting 26NiCrMoV14-5 ultra-high purity steel large ingots in an electric arc furnace comprises the following specific steps:
[0014] S1. Electric arc furnace smelting: The electric furnace is equipped with Ni4 scrap steel and Mo-containing scrap steel with low Mn, P and S content to ensure sufficient Mo element. The harmful elements As, Sn and Sb in the raw materials meet the requirements of this steel. In terms of mass percentage, the melting component S is ≤0.005% in the melting stage;
[0015] Ni4 scrap steel and Mo-containing scrap steel are loaded into an electric arc furnace, and the Ni4 scrap steel and Mo-containing scrap steel are melted into molten steel by the heat generated by the electric arc. During the melting process of the scrap steel, slag is made to remove Mn and P. When the molten steel reaches the required composition and temperature, the steel is tapped. The tapping speed is 6-8 tons / min, the tapping temperature is ≥1650°C, the tapping C is ≥0.04% (0.04-0.15%), P ≤0.001%, Mn ≤0.015%, and the harmful elements As, Sn, and Sb meet the requirements of this steel;
[0016] S2, LF refining: After ensuring that there is no oxidized slag, the molten steel is put into the LF furnace, first feed aluminum wire 3-5m / t, then add special synthetic slag 700-800kg, after the synthetic slag is completed, add calcium carbide, Al powder, electrode powder for slag making and deoxidation; when the LF furnace slag becomes white, has good fluidity, temperature ≥1580℃, and uniform composition, take samples for analysis, add alloys when it meets the requirements for adjusting the composition, and tap the steel when the chemical composition and temperature of the molten steel meet the requirements;
[0017] S3, VD refining: accurately position the ladle filled with molten steel on the refining station of the VD furnace, and keep the vacuum degree of the VD furnace below 67Pa for 15-18 minutes for vacuum degassing. After vacuum degassing, take samples for analysis. During the vacuum degassing process, the bottom blowing of argon must be normal, and the Ar gas flow rate must be adjusted to ensure the normal tumbling of the molten steel. After vacuum degassing, when Al in the molten steel is ≤0.012%, other components meet the standards, and the temperature meets the process control range, vacuum casting is carried out;
[0018] S4, VCD vacuum casting: Before vacuum casting, clean the residual slag and steel in the tundish and bake it to above 800℃. After assembling the vacuum casting station, keep the tundish warm and keep the vacuum degree in the vacuum casting chamber of the vacuum casting station below 67Pa. After VD, the hanging ladle temperature is controlled at 1600-1610℃, the tundish pouring temperature is controlled at 1550-1560℃, and the pouring starts when the molten steel level in the tundish is greater than or equal to 80% of the tundish height. The casting speed is controlled at 2t / min , to ensure that the molten steel enters the vacuum chamber in a scattered flow state; after pouring, immediately after the air-breaking valve is opened, protective slag is automatically added at 1kg / t. The protective slag uses pre-melted hollow particle continuous casting protective slag, and then the can cover is opened to add heating agent, and then carbonized rice husk is added for heat preservation. After the die drawing time is up, the mold is removed in time and transferred to the forging workshop for heating and forging. Before smelting this steel, the cold steel and slag of the VD inner screen cover must be cleaned, and the slag on the ladle wall and the edge must also be cleaned to prevent the adhered residue and residual steel from entering the molten steel and causing unqualified components;
[0019] S5. Hot demoulding of the steel ingot and heating in the furnace: the steel ingot is placed on a special pad for the heating furnace. The steel ingot can be stably placed in the hearth of the heating furnace for uniform heating. When the casting reaches the required heating temperature, it is taken out for forging;
[0020] S6. Forging: placing the heated steel ingot into the forging equipment, and performing forging operations according to the forging process requirements to obtain forgings;
[0021] S7, heat treatment: heat treatment is performed on the forging, the heat treatment includes at least one of annealing, normalizing, quenching and tempering, to obtain a large forging of 26NiCrMoV14-5 ultra-high purity steel;
[0022] S8. Material sampling and inspection: Sampling and inspection of large forgings of 26NiCrMoV14-5 ultra-high purity steel.
[0023] The smelting process of the present invention can be summarized as follows: electric arc furnace → LF refining → VD refining → VCD vacuum casting → hot demolding of steel ingots and heating in furnaces → forging and forming → heat treatment → material sampling and inspection. The large steel ingots of 26NiCrMoV14-5 ultra-high purity steel obtained after the above process have high purity, and the above process is industrially reproducible, and the control of elements such as Mn, Si, P, S and inclusions can meet the requirements, and the success rate of producing 26NiCrMoV14-5 ultra-high purity steel is high.
[0024] Furthermore, the synthetic slag includes lime particles, neutral waste furnace lining (mainly composed of Al2O3 corundum), and Al powder; wherein the mass ratio of the lime particles, the neutral waste furnace lining, and the Al powder is 16:4:1.
[0025] The synthetic slag formula of the present invention utilizes waste neutral furnace linings, which belongs to waste recycling and can reduce environmental pollution.
[0026] Further, the standards of other components in the molten steel after step S3VD refining are C content of 0.26-0.29%, Si content ≤0.03%, Mn content ≤0.03%, P content ≤0.002%, S content ≤0.002%, Cr content of 1.60-1.80%, Ni content of 3.40-3.60%, Mo content of 0.40-0.48%, V content of 0.10-0.15%, Al content ≤0.010%, Cu content ≤0.12%, As content ≤0.008%, Sn content ≤0.005%, Sb content ≤0.002%, H ≤1.2ppm, O ≤15ppm, N ≤50ppm, and the following standards need to be met:
[0027] Furthermore, the method for removing Mn and P by slagging during the melting of scrap steel in step S1 is as follows: slagging is performed twice, lime is added at 50-55 kg / ton of steel, lime is added at 20-25 kg / ton of steel for the first slagging, binary basicity of slag is controlled at 2.0-3.0, iron oxide content in slag is controlled at 16-25%, Mn≤0.025%, P≤0.0015%, slag flow is not performed before the scrap steel is completely melted; after the scrap steel is completely melted, the steel is controlled to Water temperature, the temperature of the molten steel during the first slag flowing is ≤1580℃, the slag flow volume is greater than 60% of the total slag volume. After the slag flow meets the requirements, the second slag making is carried out, and the remaining lime is added to carry out the oxidation slag blowing operation. The iron oxide content in the slag is controlled at 15-20%. The second slag flowing operation is carried out, and the slag flow volume is ≥50%. After the operation is completed, the temperature is quickly raised to meet the steelmaking requirements. No slag is added and no material is added during the steelmaking process to keep the bare steel state. After the steelmaking is completed, the slag secretion method is adopted to completely secrete the residual slag in the ladle.
[0028] The present invention adopts double slag method for smelting, and can effectively remove Mn and P by controlling the oxygen consumption, slag amount, first slag flow operating temperature and slag flow amount; the second slag making can effectively control the high temperature to return Mn and P. The total slag amount is small, and the steel material recovery rate is high.
[0029] Furthermore, after sampling and analyzing the molten steel in step S2, when the Si content in the molten steel is ≥0.02%, oxygen is blown in the ladle to reduce silicon, so that the Si content is ≤0.02%, and the slag is secreted as much as possible, and then Al wire is re-fed at 3-4m / t steel, and slag is re-made and deoxidized.
[0030] Furthermore, in step S2, the LF furnace must ensure that the green-white slag is kept for ≥20 minutes, and the color of the refined slag is checked every 5 minutes, so that the slag is kept in a good deoxidation state at all times; in the middle and late stages of deoxidation, calcium carbide and graphite powder are mainly used, and excessive Al powder should not be added, otherwise Al will be difficult to control.
[0031] Furthermore, the vacuum casting station is a vacuum casting ingot mold assembly, and the vacuum casting ingot mold assembly adopts a lower floating base steel ingot mold for vacuum casting. During the assembly process, a process of not brushing the base and not polluting the molten steel is adopted. A bottom pad is prefabricated with a steel plate with a thickness of 20 to 25 according to the shape of the floating base. The bottom pad and the floating base are filled with refractory mud. The bottom pad is cut into the shape of the bottom surface of the mold. The cutting size of the bottom pad is controlled to leave a gap of 10 mm between the bottom inner wall of the mold. The refractory mud filled with the floating base is dried and set aside. When assembling the ingot mold, the gap between the floating base and the mold wall is filled with pure granular steel chips to 30 mm from the bottom surface, and then filled with pure asbestos to 10 mm from the bottom surface, and then sealed and pressed with Ф10 aluminum wire.
[0032] The present invention adopts a floating base installation method, the bottom plate will not be washed and has less adhesion with the steel ingot, can be directly hung during forging, does not pollute molten steel, has very little bottom end cutting amount, and has a high steel ingot recovery rate.
[0033] Furthermore, when the Ni content of the molten steel in step S1 is lower than the target required amount, Ni iron is not added in the electric furnace, and Ni plate is added during the LF refining process in step S2.
[0034] Furthermore, after sampling and analysis in step S2, lime and alloy are added according to the analysis results depending on the component content. The alloy includes metal Cr, Ni plate, and 80VFe. After the alloy is added, electricity is supplied for more than 8 minutes, and the electrode is lifted and stirred for more than 60 seconds. The alloy is completely melted and the composition is uniform.
[0035] Furthermore, the synthetic slag includes lime particles, Al2O3 corundum powder and Al powder; wherein the mass ratio of the lime particles, Al2O3 corundum powder and Al powder is 16:4:1.
[0036] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are:
[0037] 1. The smelting process of a process for smelting 26NiCrMoV14-5 ultra-high purity steel large ingots by an electric arc furnace of the present invention is summarized as follows: electric arc furnace → LF refining → VD refining → VCD vacuum casting → hot demoulding of the steel ingot into the furnace for heating → forging and forming → heat treatment → material sampling and inspection. The 26NiCrMoV14-5 ultra-high purity steel large ingot obtained after the above process has high purity, and the above process is reproducible in industry, and the control of elements such as Mn, Si, P, S and inclusions can meet the requirements, and the success rate of producing 26NiCrMoV14-5 ultra-high purity steel is high;
[0038] 2. The process of smelting 26NiCrMoV14-5 ultra-high purity steel large ingots in an electric arc furnace of the present invention adopts a double slag method for smelting, and can effectively remove Mn and P by controlling the amount of oxygen, the amount of slag, the first slag flow operating temperature and the amount of slag flow, and the second slag making can effectively control the high temperature return of Mn and P, the total slag amount is small, and the steel material recovery rate is high;
[0039] 3. The process of smelting 26NiCrMoV14-5 ultra-high purity steel large ingots in an electric arc furnace of the present invention utilizes a refining slag-making deoxidation process, which has good deoxidation and desulfurization effects, high slag basicity, good fluidity, can effectively remove sulfur, and there is no resulfurization phenomenon after VD;
[0040] 4. The process of smelting 26NiCrMoV14-5 ultra-high purity steel large ingots in an electric arc furnace of the present invention adopts double vacuum treatment in the VD refining and VCD vacuum casting processes, so that the gas content in the steel is low, the inclusion content is small, and the purity is high. DETAILED DESCRIPTION
[0041] In order to make the purpose, technical scheme and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention, that is, the embodiments described are only part of the embodiments of the present invention, rather than all of the embodiments.
[0042] Therefore, the detailed description of the embodiments of the present invention provided below is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without making creative work are within the scope of protection of the present invention.
[0043] It should be noted that relational terms such as "first" and "second" are used only to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or device including the elements.
[0044] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.
[0045] A process for smelting a large ingot of 26NiCrMoV14-5 ultra-high purity steel in an electric arc furnace comprises the following steps:
[0046] S1. Electric arc furnace smelting: The electric furnace is equipped with Ni4 scrap steel and Mo-containing scrap steel with low Mn, P and S content to ensure sufficient Mo element. The harmful elements such as As, Sn and Sb in the raw materials meet the requirements of this steel. In terms of mass percentage, the melting component S is ≤0.005% in the melting stage.
[0047] Ni4 scrap steel and Mo-containing scrap steel are loaded into an electric arc furnace, and the Ni4 scrap steel and Mo-containing scrap steel are melted into molten steel by the heat generated by the electric arc. During the melting process of the scrap steel, slag is made to remove Mn and P. When the molten steel reaches the required composition and temperature, the steel is tapped. The tapping speed is 6-8 tons / min, the tapping temperature is ≥1650°C, the tapping C is ≥0.04% (0.04-0.15%), P ≤0.001%, Mn ≤0.015%, and harmful elements such as As, Sn, Sb meet the requirements of this steel;
[0048] The method for slagging and removing Mn and P during the melting of scrap steel is as follows: slagging is performed twice, lime is added at 50-55kg / ton of steel, lime is added at 20-25kg / ton of steel for the first slagging, binary basicity of slag is controlled at 2.5-3, iron oxide content in slag is controlled at 16-25%, Mn≤0.025%, P≤0.0015%, and slag flow is not performed before the scrap steel material is completely melted; after the scrap steel material is completely melted, the temperature of molten steel is controlled, the temperature of molten steel in the first slag flow is ≤1580°C, the amount of slag flow is greater than 60% of the total slag amount, and after the slag flow meets the requirements, the second slagging is performed, the remaining lime is added, and the oxidation slag operation is performed, the iron oxide content in the slag is controlled at 15-20%, the second slag flow operation is performed, the slag flow amount is ≥50%, and the temperature is quickly raised to meet the tapping requirements; during the tapping process, no slag is added and no material is added to keep the bare steel state, and after the tapping is completed, the slag remaining in the ladle is completely drained by slag secretion;
[0049] S2. LF refining: After ensuring that there is no oxidized slag, the molten steel is put into the LF furnace, first feed aluminum wire 3-5m / t, then add special synthetic slag 700-800kg, after the synthetic slag is completed, add calcium carbide, Al powder, electrode powder for slag making and deoxidation; when the LF furnace slag becomes white, has good fluidity, temperature ≥1580℃, and uniform composition, take samples for analysis, after sampling and analysis, according to the analysis results, add lime and alloy according to the component content, the alloy includes metal Cr, Ni plate, 80VFe, after the alloy is added, supply electricity for more than 8 minutes, lift the electrode and stir for more than 60s, the alloy is completely melted, the composition is uniform, when the white slag is kept for ≥20min, the steel After the chemical composition and temperature of the water meet the requirements, the steel is tapped; the synthetic slag includes lime particles, neutral waste furnace lining, and Al powder; the mass ratio of lime particles, neutral waste furnace lining, and Al powder is 16:4:1 or the synthetic slag includes lime particles, Al2O3 corundum powder, and Al powder; the mass ratio of lime particles, Al2O3 corundum powder, and Al powder is 16:4:1; after the molten steel is sampled and analyzed, when the Si content in the molten steel is ≥0.02%, oxygen is blown in the ladle to reduce silicon, so that the Si content is ≤0.02%, and the slag is secreted as much as possible, and then Al wire is re-fed 3-4m / t steel, slag is re-made and deoxidized, and step S2 is repeated;
[0050] S3, VD refining: accurately position the ladle filled with molten steel on the refining station of the VD furnace, and maintain the vacuum degree of the VD furnace below 67Pa for 15-18 minutes for vacuum degassing. After vacuum degassing, sample analysis must be performed. During the vacuum degassing process, the bottom blowing of argon must be normal, and the Ar gas flow rate must be adjusted to ensure normal tumbling of the molten steel; after vacuum degassing, when Al≤0.012% in the molten steel, other components meet the standards, and the temperature meets the process control range, vacuum casting is performed; Step S3 The standards for other components in the molten steel after VD refining are C content of 0.26-0.29%, Si content of 0.26-0.29%, and Si content of 0.26-0.29%. ≤0.03%, Mn content ≤0.03%, P content ≤0.002%, S content ≤0.002%, Cr content 1.60-1.80%, Ni content 3.40-3.60%, Mo content 0.40-0.48%, V content 0.10-0.15%, Al content ≤0.010%, Cu content ≤0.12%, As content ≤0.008%, Sn content ≤0.005%, Sb content ≤0.002%, H ≤1.2ppm, O ≤15ppm, N ≤50ppm, and the following standards must be met:
[0051] S4, VCD vacuum casting: Before vacuum casting, clean the residual slag and steel in the tundish and bake it to above 800℃. After assembling the vacuum casting station, keep the tundish warm and keep the vacuum degree in the vacuum casting chamber of the vacuum casting station below 67Pa. After VD, the hanging ladle temperature is controlled at 1600-1610℃, the tundish pouring temperature is controlled at 1550-1560℃, and the pouring starts when the molten steel level in the tundish is greater than or equal to 80% of the tundish height. The casting speed is controlled at 2t / min , to ensure that the molten steel enters the vacuum chamber in a scattered flow state; after pouring, immediately after the air-breaking valve is opened, protective slag is automatically added at 1kg / t. The protective slag uses pre-melted hollow particle continuous casting protective slag, and then the can cover is opened to add heating agent, and then carbonized rice husk is added for heat preservation. After the die drawing time is up, the mold is removed in time and transferred to the forging workshop for heating and forging. Before smelting this steel, the cold steel and slag of the VD inner screen cover must be cleaned, and the slag on the ladle wall and the edge must also be cleaned to prevent the adhered residue and residual steel from entering the molten steel and causing unqualified components;
[0052] S5. Hot demoulding of the steel ingot and heating in the furnace: the steel ingot is placed on a special pad for the heating furnace. The steel ingot can be stably placed in the hearth of the heating furnace for uniform heating. When the casting reaches the required heating temperature, it is taken out for forging;
[0053] S6. Forging: placing the heated steel ingot into the forging equipment, and performing forging operations according to the forging process requirements to obtain forgings;
[0054] S7. Heat treatment: heat treatment is performed on the forging, wherein the heat treatment includes at least one of annealing, normalizing, quenching, and tempering to obtain a large 26NiCrMoV14-5 ultra-high purity steel forging.
[0055] S8. Material sampling and inspection: Sampling and inspection of large forgings of 26NiCrMoV14-5 ultra-high purity steel.
[0056] In the electric arc furnace steelmaking of the present invention, electric energy is used as a heat source, electric energy is input into the furnace through graphite electrodes, an electric arc is generated between the electrode and the charge, and the charge is directly heated by the high temperature of the electric arc; in the present invention, Ni4 scrap steel is matched with Mo-containing scrap steel with low Mn, P and S contents, and an electric arc furnace is used to refine molten steel, and the electric arc furnace directly uses the high temperature of the electric arc to heat the charge, with high thermal efficiency, and in the process of electric arc furnace steelmaking, the slag forms a protective layer on the surface of the molten steel, which can isolate the molten steel from the air, and adsorb impurities in the molten steel and fix harmful element oxides; the oxides in the slag react chemically with the impurity elements to oxidize them, thereby removing them or converting them into a form that is easy to discharge.
[0057] In addition, the present invention utilizes the refining slag deoxidation process, which has good deoxidation and desulfurization effects, high slag basicity, good fluidity, can effectively remove sulfur, and there is no resulfurization phenomenon after VD; the present invention adopts vacuum casting, reasonably controls the casting temperature and casting speed, and the component segregation on large steel ingots is controllable; the present invention adopts double vacuum treatment during VD refining and VCD vacuum casting, and the gas content in the steel is low, the inclusion content is small, and the purity is high. The present invention immediately adds the continuous casting hollow particle protective slag during the pouring and breaking process, which has fast slag removal and no crusting of the cap mouth. The addition of the exothermic agent can quickly burn, the cap mouth shrinks ideally, and the cap mouth utilization rate is high.
[0058] The smelting process of the present invention is summarized as follows: electric arc furnace → LF refining → VD refining → VCD vacuum casting → hot demoulding of steel ingots into furnaces for heating → forging and molding → heat treatment → material sampling and inspection. The large-scale 26NiCrMoV14-5 ultra-high purity steel ingot obtained after the above process has high purity, and the above process is industrially reproducible, and the control of elements such as Mn, Si, P, S and inclusions can meet the requirements, and the success rate of producing 26NiCrMoV14-5 ultra-high purity steel is high. Waste neutral furnace lining is used in the synthetic slag formula of the present invention, which belongs to waste recycling and can reduce environmental pollution.
[0059] In step S1, the present invention adopts double slag smelting, and can effectively remove Mn and P by controlling the oxygen consumption, slag amount, first slag flow operating temperature and slag flow amount; the second slag making can effectively control the high temperature to return Mn and P. The total slag amount is small, and the steel material recovery rate is high.
[0060] Furthermore, in step S2, the LF furnace must ensure that the green-white slag is kept for ≥20 minutes, and the color of the refined slag is checked every 5 minutes, so that the slag is kept in a good deoxidation state at all times; in the middle and late stages of deoxidation, calcium carbide and graphite powder are mainly used, and excessive Al powder should not be added, otherwise Al will be difficult to control.
[0061] Furthermore, the vacuum casting station is a vacuum casting ingot mold assembly, and the vacuum casting ingot mold assembly adopts a lower floating base steel ingot mold for vacuum casting. During the assembly process, a process of not brushing the base and not polluting the molten steel is adopted. A bottom pad is prefabricated with a steel plate with a thickness of 20 to 25 according to the shape of the floating base. The bottom pad and the floating base are filled with refractory mud. The bottom pad is cut into the shape of the bottom surface of the mold. The cutting size of the bottom pad is controlled to leave a gap of 10 mm between the bottom inner wall of the mold. The refractory mud filled with the floating base is dried and set aside. When assembling the ingot mold, the gap between the floating base and the mold wall is filled with pure granular steel chips to 30 mm from the bottom surface, and then filled with pure asbestos to 10 mm from the bottom surface, and then sealed and pressed with Ф10 aluminum wire.
[0062] The present invention adopts a floating base installation method, the bottom plate will not be washed and has less adhesion with the steel ingot, can be directly hung during forging, does not pollute molten steel, has very little bottom end cutting amount, and has a high steel ingot recovery rate.
[0063] Furthermore, when the Ni content of the molten steel in step S1 is lower than the target required amount, Ni iron is not added in the electric furnace to increase Ni, and Ni plates are added during the LF refining process in step S2.
[0064] Example 1
[0065] The preferred embodiment of the present invention provides a process for smelting 26NiCrMoV14-5 ultra-high purity steel large ingots by electric arc furnace, according to the above-mentioned process flow of electric arc furnace → LF refining → VD refining → VCD vacuum casting → hot demoulding of steel ingots into furnace for heating → forging and forming → heat treatment → material sampling and inspection, using an electric arc furnace with furnace number 232-134, the composition of molten steel after VD is controlled within the following standards, the standards are shown in Table 1. (Gas unit: ppm, solid unit is mass percentage %)
[0066] Table 1 Control standards for composition of molten steel after VD for furnace numbers 232-134
[0067]
[0068] Example 2
[0069] The preferred embodiment of the present invention provides a process for smelting 26NiCrMoV14-5 ultra-high purity steel large ingots by electric arc furnace, according to the above-mentioned process flow of electric arc furnace → LF refining → VD refining → VCD vacuum casting → hot demolding of steel ingots into furnace for heating → forging and forming → heat treatment → material sampling and inspection, using electric arc furnaces with furnace numbers of 232-144, the composition of molten steel after VD is controlled within the following standards, the standards are shown in Table 2. (Gas unit: ppm, solid unit is mass percentage %)
[0070] Table 2 Control standards for composition of molten steel after VD for furnace numbers 232-144
[0071]
[0072] Example 3
[0073] The preferred embodiment of the present invention provides a process for smelting 26NiCrMoV14-5 ultra-high purity steel large ingots by electric arc furnace, according to the above-mentioned process flow of electric arc furnace → LF refining → VD refining → VCD vacuum casting → hot demolding of steel ingots into furnace for heating → forging and forming → heat treatment → material sampling and inspection, using electric arc furnaces with furnace numbers of 232-149, the composition of molten steel after VD is controlled within the following standards, the standards are shown in Table 3. (Gas unit: ppm, solid unit is mass percentage %)
[0074] Table 3 Control standards for composition of molten steel after VD for furnace numbers 232-149
[0075]
[0076] Example 4
[0077] The preferred embodiment of the present invention provides a process for smelting 26NiCrMoV14-5 ultra-high purity steel large ingots by electric arc furnace, according to the above-mentioned process flow of electric arc furnace → LF refining → VD refining → VCD vacuum casting → hot demolding of steel ingots into furnace for heating → forging and forming → heat treatment → material sampling and inspection, using an electric arc furnace with furnace number 232-154, the composition of molten steel after VD is controlled within the following standards, the standards are shown in Table 4. (Gas unit: ppm, solid unit is mass percentage %)
[0078] Table 4 Control standards for composition of molten steel after VD for furnace number 232-154
[0079]
[0080] Example 5
[0081] The preferred embodiment of the present invention provides a process for smelting 26NiCrMoV14-5 ultra-high purity steel large ingots by electric arc furnace, according to the above-mentioned process flow of electric arc furnace → LF refining → VD refining → VCD vacuum casting → hot demoulding of steel ingots into furnace for heating → forging and forming → heat treatment → material sampling and inspection, using an electric arc furnace with furnace number 232-160, the composition of molten steel after VD is controlled within the following standards, the standards are shown in Table 5. (Gas unit: ppm, solid unit is mass percentage %)
[0082] Table 5 Control standards for composition of molten steel after VD for furnace numbers 232-160
[0083]
[0084] Example 6
[0085] The preferred embodiment of the present invention provides a process for smelting 26NiCrMoV14-5 ultra-high purity steel large ingots by electric arc furnace, according to the above-mentioned process flow of electric arc furnace → LF refining → VD refining → VCD vacuum casting → hot demoulding of steel ingots into furnace for heating → forging and forming → heat treatment → material sampling and inspection, using electric arc furnaces with furnace numbers of 232-163, the composition of molten steel after VD is controlled within the following standards, the standards are shown in Table 6. (Gas unit: ppm, solid unit is mass percentage %)
[0086] Table 6 Control standards for composition of molten steel after VD for furnace numbers 232-163
[0087]
[0088] Example 7
[0089] The preferred embodiment of the present invention provides a process for smelting 26NiCrMoV14-5 ultra-high purity steel large ingots by electric arc furnace, according to the above-mentioned process flow of electric arc furnace → LF refining → VD refining → VCD vacuum casting → hot demolding of steel ingots into furnace for heating → forging and forming → heat treatment → material sampling and inspection, using electric arc furnaces with furnace numbers of 232-165, the composition of molten steel after VD is controlled within the following standards, the standards are shown in Table 7. (Gas unit: ppm, solid unit is mass percentage %)
[0090] Table 7 Control standards for composition of molten steel after VD for furnace numbers 232-165
[0091]
[0092] Test Example 1
[0093] The yield of electric furnace steel material in the above Examples 1-5 was tested, and the test results are shown in Table 8; the testing method is prior art and will not be elaborated in detail here.
[0094] Table 8 Electric furnace steel material recovery rate
[0095]
[0096] It can be seen from Table 8 that the average electric furnace steel material recovery rate of the present invention is as high as 89.72%.
[0097] Test Example 2
[0098] The present invention takes Example 1 and Example 2 as examples, and performs finished product composition detection on the 26NiCrMoV14-5 products obtained in Example 1 and Example 2. The detection results are shown in Table 9; the composition requirements of ultra-high purity steel 26NiCrMoV14-5 are shown in Table 10; (Gas unit: ppm, solid unit is mass percentage %)
[0099] Table 9 26NiCrMoV14-5 product composition test results
[0100]
[0101]
[0102] Table 10 Requirements for the composition of ultra-high purity steel 26NiCrMoV14-5
[0103]
[0104]
[0105] Combining Table 9 and Table 10, it can be seen that the 26NiCrMoV14-5 products obtained in Example 1 and Example 2 of the present invention meet the composition requirements of ultra-high purity steel 26NiCrMoV14-5, which indicates that the present invention can prepare 26NiCrMoV14-5 ultra-high purity steel.
[0106] Test Example 3
[0107] The present invention takes Example 1 and Example 2 as examples, and performs inclusion rating and harmful element sum detection on the 26NiCrMoV14-5 products obtained in Example 1 and Example 2. The detection results are shown in Table 11; the inclusion requirement standard of ultra-high purity steel 26NiCrMoV14-5 is shown in Table 12. (Gas unit: ppm, solid unit is mass percentage %)
[0108] Table 11 Inclusion rating and total harmful element test results of 26NiCrMoV14-5 product
[0109]
[0110] Table 12 Requirements for inclusions in ultra-high purity steel 26NiCrMoV14-5
[0111]
[0112] Comparing Table 11 and Table 12, the inclusion rating of the 26NiCrMoV14-5 products obtained in Example 1 and Example 2 of the present invention meets the inclusion requirement of ultra-high purity steel 26NiCrMoV14-5.
[0113] The above description is only a preferred embodiment of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions and improvements made by any technician familiar with the field within the spirit and principle of the present invention should be included in the scope of protection of the present invention.
Claims
1. A process for smelting large-scale ingots of 26NiCrMoV14-5 ultra-high purity steel in an electric arc furnace, characterized in that: The following steps are involved: S1. Electric arc furnace smelting: The electric furnace is equipped with Ni4 scrap steel and Mo-containing scrap steel with low Mn, P and S content to ensure sufficient Mo element. The harmful elements As, Sn and Sb in the raw materials meet the requirements of this steel. In terms of mass percentage, the melting component S is ≤0.005% in the melting stage. S2, LF refining: After ensuring that there is no oxidized slag, the molten steel is put into the LF furnace, first feed aluminum wire 3-5m / t, then add special synthetic slag 700-800kg, after the synthetic slag is completed, add calcium carbide, Al powder, electrode powder for slag making and deoxidation; when the LF furnace slag becomes white, has good fluidity, temperature ≥1580℃, and uniform composition, take samples for analysis, add alloys when it meets the requirements for adjusting the composition, and tap the steel when the chemical composition and temperature of the molten steel meet the requirements; S3, VD refining: accurately position the ladle filled with molten steel on the refining station of the VD furnace for vacuum degassing, and take samples for analysis after vacuum degassing; after vacuum degassing, when Al in the molten steel is ≤ 0.012%, other components meet the standards, and the temperature meets the process control range, vacuum casting is carried out; S4, VCD vacuum casting: keep the vacuum degree in the vacuum casting room of the vacuum casting station below 67Pa, control the temperature of the hanging ladle after VD at 1600-1610℃, control the pouring temperature of the tundish at 1550-1560℃, start pouring when the molten steel level in the tundish is greater than or equal to 80% of the height of the tundish, and control the casting speed at 2t / min; after the pouring is completed, immediately add protective slag automatically at 1kg / t after the air breaker is opened. The protective slag adopts pre-melted hollow particle continuous casting protective slag, and then open the can cover to add heating agent, and then add carbonized rice husk for heat preservation. After the die drawing time is up, demold in time and transfer to the forging workshop to heat in the furnace and forge into the steel ingot.
2. The process for smelting 26NiCrMoV14-5 ultra-high purity steel large ingots in an electric arc furnace according to claim 1, characterized in that: The specific steps are as follows: S1. Electric arc furnace smelting: The electric furnace is equipped with Ni4 scrap steel and Mo-containing scrap steel with low Mn, P and S content to ensure sufficient Mo element. The harmful elements As, Sn and Sb in the raw materials meet the requirements of this steel. In terms of mass percentage, the melting component S is ≤0.005% in the melting stage. Ni4 scrap steel and Mo-containing scrap steel are loaded into an electric arc furnace, and the Ni4 scrap steel and Mo-containing scrap steel are melted into molten steel by the heat generated by the electric arc. During the melting process of the scrap steel, slag is made to remove Mn and P. When the molten steel reaches the required composition and temperature, the steel is tapped. The tapping speed is 6-8 tons / min, the tapping temperature is ≥1650°C, the tapping C is ≥0.04% (0.04-0.15%), P ≤0.001%, Mn ≤0.015%, and the harmful elements As, Sn, and Sb meet the requirements of this steel; S2, LF refining: After ensuring that there is no oxidized slag, the molten steel is put into the LF furnace, first feed aluminum wire 3-5m / t, then add special synthetic slag 700-800kg, after the synthetic slag is completed, add calcium carbide, Al powder, electrode powder for slag making and deoxidation; when the LF furnace slag becomes white, has good fluidity, temperature ≥1580℃, and uniform composition, take samples for analysis, add alloys when it meets the requirements for adjusting the composition, and tap the steel when the chemical composition and temperature of the molten steel meet the requirements; S3, VD refining: accurately position the ladle filled with molten steel on the refining station of the VD furnace, and keep the vacuum degree of the VD furnace below 67Pa for 15-18 minutes for vacuum degassing. After vacuum degassing, take samples for analysis. During the vacuum degassing process, the bottom blowing of argon must be normal, and the Ar gas flow rate must be adjusted to ensure the normal tumbling of the molten steel. After vacuum degassing, when Al in the molten steel is ≤0.012%, other components meet the standards, and the temperature meets the process control range, vacuum casting is carried out; S4, VCD vacuum casting: Before vacuum casting, clean the residual slag and steel in the tundish and bake it to above 800℃. After assembling the vacuum casting station, keep the tundish warm and keep the vacuum degree in the vacuum casting chamber of the vacuum casting station below 67Pa. The temperature of the hanging ladle after VD is controlled at 1600-1610℃, and the pouring temperature of the tundish is controlled at 1550-1560℃. When the molten steel level in the tundish is greater than or equal to 80% of the height of the tundish, pouring is started. The casting speed is controlled at 2t / min to ensure that the molten steel enters the vacuum chamber in a scattered state. After the pouring is completed, the protective slag is automatically added at 1kg / t immediately after the air-breaking valve is opened. The protective slag adopts pre-melted hollow particle continuous casting protective slag, and then the can cover is opened to add the heating agent, and then carbonized rice husk is added for heat preservation. After the die drawing time is up, the die is removed in time and transferred to the forging workshop for heating and forging into the furnace. S5. Hot demoulding of the steel ingot and heating in the furnace: the steel ingot is placed on a special pad in the heating furnace, and the steel ingot is stably placed in the hearth of the heating furnace for uniform heating. When the casting reaches the required heating temperature, it is taken out for forging; S6. Forging: placing the heated steel ingot into the forging equipment, and performing forging operations according to the forging process requirements to obtain forgings; S7. Heat treatment: heat treatment is performed on the forging, wherein the heat treatment includes at least one of annealing, normalizing, quenching, and tempering to obtain a large 26NiCrMoV14-5 ultra-high purity steel forging. S8. Material sampling and inspection: Sampling and inspection of large forgings of 26NiCrMoV14-5 ultra-high purity steel.
3. The process for smelting 26NiCrMoV14-5 ultra-high purity steel large ingots in an electric arc furnace according to claim 1 or 2, characterized in that: The synthetic slag comprises lime particles, neutral waste furnace lining material and Al powder, wherein the mass ratio of the lime particles, neutral waste furnace lining material and Al powder is 16:4:
1.
4. The process for smelting 26NiCrMoV14-5 ultra-high purity steel large ingots in an electric arc furnace according to claim 1, characterized in that: Step S3: The standards of other components in the molten steel after VD refining are C content of 0.26-0.29%, Si content of ≤0.03%, Mn content of ≤0.03%, P content of ≤0.002%, S content of ≤0.002%, Cr content of 1.60-1.80%, Ni content of 3.40-3.60%, Mo content of 0.40-0.48%, V content of 0.10-0.15%, Al content of ≤0.010%, Cu content of ≤0.12%, As content of ≤0.008%, Sn content of ≤0.005%, Sb content of ≤0.002%, H of ≤1.2ppm, O of ≤15ppm, N of ≤50ppm, and the following standards need to be met:
5. The process for smelting 26NiCrMoV14-5 ultra-high purity steel large ingots in an electric arc furnace according to claim 2, characterized in that: The method for removing Mn and P by slagging during the melting of scrap steel in step S1 is as follows: slagging is performed twice, lime is added at 50-55 kg / ton of steel, lime is added at 20-25 kg / ton of steel for the first slagging, binary basicity of slag is controlled at 2.0-3.0, iron oxide content in slag is controlled at 16-25%, Mn≤0.025%, P≤0.0015%, slag flow is not performed before the scrap steel material is completely melted; after the scrap steel material is completely melted, the temperature of molten steel is controlled The temperature of the molten steel during the first slag flowing is ≤1580℃, and the amount of slag flowing is greater than 60% of the total slag. After the slag flowing meets the requirements, the second slag making is carried out, and the remaining lime is added to blow the oxidation slag. The iron oxide content in the slag is controlled at 15-20%. The second slag flowing operation is carried out, and the slag flowing amount is ≥50%. After the operation is completed, the temperature is quickly raised to meet the steelmaking requirements; no slag is added and no material is added during the steelmaking process to keep the bare steel state. After the steelmaking is completed, the slag secretion method is adopted to completely secrete the residual slag in the ladle.
6. The process for smelting 26NiCrMoV14-5 ultra-high purity steel large ingots in an electric arc furnace according to claim 1, characterized in that: After the molten steel is sampled and analyzed in step S2, when the Si content in the molten steel is ≥0.02%, oxygen is blown in the ladle to reduce silicon, so that the Si content is ≤0.02%, and the slag is secreted as much as possible, and then Al wire 3-4m / t steel is re-fed to re-slag and deoxidize.
7. The process for smelting 26NiCrMoV14-5 ultra-high purity steel large ingots in an electric arc furnace according to claim 1, characterized in that: In step S2, the LF furnace must ensure that the green-white slag is kept for ≥20 minutes, and the color of the refined slag is checked every 5 minutes, so that the slag is kept in a good deoxidation state at all times.
8. The process for smelting 26NiCrMoV14-5 ultra-high purity steel large ingots in an electric arc furnace according to claim 1, characterized in that: The vacuum casting station is for vacuum casting ingot mold assembly. The vacuum casting ingot mold assembly adopts a lower floating base steel ingot mold for vacuum casting. During the assembly process, a process of not brushing the base and not polluting the molten steel is adopted. A bottom pad is prefabricated with a steel plate with a thickness of 20 to 25 mm according to the shape of the floating base. The bottom pad and the floating base are filled with refractory mud. The bottom pad is cut into the shape of the bottom surface of the mold. The cutting size of the bottom pad is controlled to leave a gap of 10 mm between the bottom inner wall of the mold. The refractory mud filled with the floating base is dried and set aside. When assembling the ingot mold, the gap between the floating base and the mold wall is filled with pure granular steel chips to 30 mm from the bottom surface, and then filled with pure asbestos to 10 mm from the bottom surface, and then sealed and pressed with Ф10 aluminum wire.
9. The process for smelting 26NiCrMoV14-5 ultra-high purity steel large ingots in an electric arc furnace according to claim 2, characterized in that: When the Ni content of the molten steel in step S1 is lower than the target required amount, Ni iron is not added in the electric furnace to match Ni, and Ni plate is added during the LF refining process in step S2.
10. The process for smelting 26NiCrMoV14-5 ultra-high purity steel large ingots in an electric arc furnace according to claim 2, characterized in that: After sampling and analysis in step S2, lime and alloy are added according to the analysis results depending on the component content. The alloy includes metal Cr, Ni plate, and 80VFe. After the alloy is added, power is supplied for more than 8 minutes, and the electrode is lifted and stirred for more than 60 seconds. The alloy is completely melted and the composition is uniform.