Magnesium alloy electrophoretic coating process
Through the magnesium alloy electrophoretic coating process, alkaline solution and chemical conversion treatment are used to form a uniform conversion film, and combined with high-temperature pretreatment technology, the problems of paint film adhesion and environmental protection costs in magnesium alloy surface treatment are solved, and high adhesion is achieved , low pollution, low cost magnesium alloy coating effect.
Patent Information
- Application Number
- CN202310368948.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-10
- Publication Date
- 2024-10-15
AI Technical Summary
Magnesium alloy surface treatment technology started late. The matching between coating pretreatment and electrophoretic coating is poor, resulting in poor paint film adhesion. Moreover, traditional phosphating/chromate conversion coating has environmental pollution problems and cannot meet environmental protection requirements. Micro-arc oxidation coating increases production costs.
A magnesium alloy electrophoretic coating process is adopted, including alkaline solution and activation treatment, chemical conversion treatment, high temperature pretreatment and electrophoretic coating, using zirconate titanic acid, hydrogen peroxide, film-forming aids and silane coupling agents and other ingredients to form Uniform and dense conversion coating, and high-temperature pretreatment to release the micro-crack structure on the surface of the film to improve paint film adhesion.
An economical and environmentally friendly magnesium alloy electrophoretic coating process has been realized. The adhesion of the paint film is significantly improved, the cost is low, the pollution is small, the corrosion resistance is equivalent to that of traditional phosphate conversion coating, and it is suitable for industrial production.
Smart Images

Figure HDA0004167959530000011 
Figure HDA0004167959530000021 
Figure HDA0004167959530000022
Abstract
Description
Technical Field
[0001] The invention relates to the field of magnesium alloy surface treatment, in particular to a magnesium alloy electrophoretic coating process. Background Art
[0002] Magnesium alloy has low density and good mechanical properties, making it an ideal metal structural material for lightweighting automobiles. However, magnesium alloy has poor corrosion resistance and requires high quality of surface protective coatings. Cathodic electrophoretic coating technology is a commonly used coating method in the automotive field, but the effect is not ideal when applied to magnesium substrates. On the one hand, magnesium alloy surface treatment technology started late, and the matching between coating pretreatment and electrophoretic coating is poor, resulting in poor adhesion of the paint film; on the other hand, the traditional phosphating / chromate conversion coating pretreatment process has environmental pollution problems and cannot meet the current environmental impact assessment requirements. Although the micro-arc oxidation coating pretreatment has excellent performance, it will greatly increase production costs. Driven by the dual needs of "environmental protection requirements + energy costs", companies are in urgent need of developing an electrophoretic coating process suitable for magnesium alloys. Summary of the invention
[0003] In view of the above problems, the purpose of the present invention is to provide an economical and environmentally friendly magnesium alloy electrophoretic coating process, which not only achieves strong adhesion of the electrophoretic paint film, but also takes into account the production requirements of low pollution and low cost.
[0004] The technical solution of the present invention is:
[0005] A magnesium alloy electrophoretic coating process, the specific steps are as follows:
[0006] Step 1: Pre-treatment of magnesium alloy
[0007] (1) Soak the magnesium alloy in an alkaline solution containing sodium hydroxide, sodium silicate, and sodium carbonate at room temperature for 3 to 5 minutes to remove residual grease and dirt on the surface;
[0008] (2) The magnesium alloy after alkali washing is washed with running water and then immersed in an activation treatment solution containing citric acid, lactic acid, and sodium dodecyl sulfate, and treated at room temperature for 5s to 2min to coarsen the surface of the magnesium matrix and increase the active points, which is conducive to the uniform deposition of film-forming substances during the chemical conversion process;
[0009] Step 2: Chemical conversion of magnesium alloy
[0010] The magnesium alloy after pretreatment is treated by dipping or spraying with a conversion treatment solution, and a uniform and dense conversion film is formed within 30s to 10min at room temperature.
[0011] The conversion treatment solution contains: zirconate titanic acid and / or zirconate titanate, hydrogen peroxide, film-forming aid, silane coupling agent, and the pH value is in the range of 2.0 to 3.5;
[0012] Step 3: High temperature pretreatment before painting
[0013] The magnesium alloy parts after chemical conversion treatment are hung in a blast drying oven at 170-190°C and left to stand for 10-15 minutes. The hydrated compounds in the conversion film are dehydrated and condensed after high-temperature pretreatment, causing the micro-crack structure on the surface of the film to be further released, which is conducive to the formation of mechanical interlocking with the subsequent electrophoretic paint film and improving the adhesion of the paint film;
[0014] Step 4: Apply electrophoretic paint
[0015] (1) mixing the electrophoretic paint with deionized water in a weight ratio of 1:3 to 1:5, and stirring continuously for 48 hours in a constant temperature water area of 25±1°C to fully mature to form an electrophoretic paint liquid;
[0016] (2) immersing the magnesium alloy chemical conversion component after high temperature pretreatment in the prepared electrophoretic paint solution, with the magnesium alloy component as the cathode and the stainless steel plate as the anode, for electrophoretic coating;
[0017] (3) The magnesium alloy parts after electrophoresis are rinsed with running water, drained, and high-temperature cured at 170 to 190° C. for 20 to 30 minutes.
[0018] In the magnesium alloy electrophoretic coating process, in the alkaline solution of step 1, the concentrations of sodium hydroxide, sodium silicate and sodium carbonate are 20-40 g / l, 20-40 g / l and 10-30 g / l respectively, and the balance is water.
[0019] In the magnesium alloy electrophoretic coating process, in the activation treatment solution in step 1, the concentrations of citric acid, lactic acid, and sodium dodecylbenzene sulfonate are 20-40 g / l, 5-15 g / l, and 0.5-2 g / l, respectively, and the balance is water.
[0020] In the magnesium alloy electrophoretic coating process, in the conversion treatment solution in step 2, the concentration of zirconyl titanic acid and / or zirconyl titanate is 2 to 5 g / l, the concentration of hydrogen peroxide is 2 to 5 g / l, the concentration of film-forming aid is 0.5 to 5 g / l, the concentration of silane coupling agent is 1 to 5 g / l, and the balance is water.
[0021] In the magnesium alloy electrophoretic coating process, the zirconic titanic acid is one of fluorozirconic acid and fluorotitanic acid or a combination thereof, the zirconic titanate is one of potassium fluorozirconate and potassium fluorotitanate or a combination thereof, the film-forming aid is one of phytic acid and tannic acid or a combination thereof, and the silane coupling agent is one of γ-aminopropyltriethoxysilane, γ-(2,3-epoxypropyloxy)propyltrimethoxysilane, and γ-(methacryloyloxy)propyltrimethoxysilane or a combination of two or more thereof.
[0022] In the magnesium alloy electrophoretic coating process, the film thickness after the chemical conversion treatment in step 2 can be controlled within the range of 100nm to 5μm, and the corrosion resistance is equivalent to that of the traditional phosphate conversion film.
[0023] In the magnesium alloy electrophoretic coating process, in step 3, before high-temperature pretreatment, the magnesium alloy chemical conversion parts need to be fully cleaned with deionized water and drained; the parts after high-temperature pretreatment are cooled at room temperature and then used for standby.
[0024] In the magnesium alloy electrophoretic coating process, in step 4, the aging process of the prepared electrophoretic paint solution is carried out by magnetic stirring.
[0025] In the magnesium alloy electrophoretic coating process, in step 4, the electrophoretic coating voltage is 60-140V, the electrophoretic time is 2-3min, the distance between the anode and cathode plates is 3-5cm, and the temperature of the electrophoretic paint solution is controlled at 25±2°C.
[0026] The magnesium alloy electrophoretic coating process, after electrophoretic coating, the electrophoretic paint film adhesion of the magnesium alloy parts is ≥20MPa.
[0027] The design concept of the present invention is:
[0028] (1) Chemical conversion solution ideas
[0029] First, fluorozirconate (salt) and fluorotitanate (salt) will generate colloidal zirconium and titanium oxides when they meet alkali in aqueous solution. These two oxidation products have high chemical stability and are ideal film-forming substances. However, due to the uneven microscopic surface structure of magnesium alloy, there is a large potential difference between the matrix phase and the intermetallic compound. When the magnesium alloy is immersed in an acidic zirconate (titanate) salt aqueous solution, under the action of the micro-galvanic couple, the intermetallic compound with a more positive potential acts as a micro-cathode, and a rapid hydrogen evolution reaction will occur around it, resulting in OH near the intermetallic compound. - The amount of zirconium oxide deposited is significantly higher than that in other locations. This uneven film state will not only reduce its protective effect on the substrate, but also affect the subsequent coating performance. In order to solve this problem, it is necessary to add an appropriate amount of oxidant to the zirconium-titanium base liquid to inhibit the excessive hydrogen evolution reaction in the micro-cathode area on the substrate surface and ensure the uniform deposition of zirconium-titanium oxide at each location.
[0030] Secondly, the corrosion resistance of zirconium-based ceramic conversion film is not ideal, which is related to its extremely thin film thickness to a certain extent. Adding an appropriate amount of inorganic or organic film-forming additives and coordinating zirconium titanium oxide to participate in the film-forming reaction can improve the film thickness to a certain extent and enhance its protective performance.
[0031] Finally, in order to further improve the adhesion between the conversion film and the paint film, a small amount of silane coupling agent is used to modify the film-forming liquid, so that a certain amount of organic film-forming substance is doped on the surface of the conversion film, which facilitates better interface bonding with the organic coating.
[0032] (2) High temperature coating pretreatment ideas:
[0033] The chemical conversion treatment is carried out in an aqueous solution, and the film-forming substances will exist in the form of a large number of hydrated compounds on the surface of the magnesium substrate. Under high temperature conditions, the dehydration and condensation of the hydrated compounds will increase the stress inside the conversion film, resulting in the expansion of the size of the microcracks on the surface of the film layer. Considering that a high-temperature curing process of 170-190°C must be carried out after electrophoretic coating, if the microcracks on the surface of the chemical conversion film expand at this stage, it will inevitably cause incomplete coating of the electrophoretic paint film, and local defects will seriously affect the adhesion of the paint film. Therefore, we designed to pre-treat the magnesium alloy chemical conversion film at a high temperature of 170-190°C before electrophoretic coating to fully release the microcracks on the surface of the conversion film, which is conducive to the subsequent filling of the electrophoretic paint liquid. On the one hand, the problem of local defects between the film and the substrate interface is solved. On the other hand, with the help of the "tooth" structure provided by the microcracks on the surface of the conversion film, a mechanical interlocking effect is formed between the electrophoretic paint film to increase the physical connection force and improve the adhesion of the paint film.
[0034] The present invention has the following advantages and beneficial effects:
[0035] 1. The magnesium alloy chemical conversion treatment liquid of the present invention does not contain phosphates and polluting ions such as chromium, zinc, and nickel, has little pollution to the environment, meets the enterprise pollutant emission standards, and is a green and environmentally friendly process. Moreover, the process is simple, low-cost, and can be operated at room temperature. It can be treated by immersion or spraying. A protective film with uniform color, complete and dense coating can be formed on the surface of the magnesium substrate at room temperature in a short time. The film formation is stable, and the treatment liquid is easy to control, without precipitated waste residue, etc., which is suitable for industrial production. The thickness of the magnesium alloy chemical conversion film prepared by this process is controllable in the range of 100nm to 5μm, has good bonding with the magnesium substrate, and its corrosion resistance is comparable to that of traditional phosphate conversion films.
[0036] 2. The high-temperature pretreatment process of magnesium alloy coating of the present invention can solve the local defects of the electrophoretic paint film on the chemical conversion film, and reasonably utilize the microcrack structure of the chemical conversion film to significantly improve the adhesion of the paint film. The adhesion of the electrophoretic paint film under high-temperature pretreatment conditions is ≥20MPa, which is more than 4 times higher than that without adding high-temperature pretreatment conditions. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1.Macromorphology of the new chemical conversion film on magnesium alloy and two traditional phosphate conversion films after 48 hours of full immersion corrosion test (the corrosion medium is 3.5wt% sodium chloride aqueous solution): (a) New chemical conversion film Example 1; (b) New chemical conversion film Comparative Example 1; (c) Phosphate conversion film Comparative Example 2; (d) Phosphate conversion film Comparative Example 3.
[0038] Figure 2 .Cross-sectional morphology of magnesium alloy chemical conversion-electrophoretic composite coating: (a) Example 1; (b) Comparative Example 1.
[0039] Figure 3 .Macromorphology of magnesium alloy chemical conversion-electrophoretic composite coating after pulling test: (a) Example 1; (b) Comparative Example 1. DETAILED DESCRIPTION
[0040] In the specific implementation process, the magnesium alloy electrophoretic coating process of the present invention is mainly divided into the following four steps:
[0041] Step 1: Pretreatment: Use alkaline solution to remove the oil stains on the sample surface and soak at room temperature for 3 to 5 minutes. After alkali washing, the magnesium alloy is washed with running water and then soaked in the activation treatment solution at room temperature for 5 seconds to 2 minutes to coarsen the surface of the magnesium matrix and increase the active points, which is conducive to the uniform deposition of the film-forming material during the chemical conversion process;
[0042] In the alkaline solution, the concentrations of sodium hydroxide, sodium silicate and sodium carbonate are 30 g / l, 30 g / l and 20 g / l respectively, and the balance is water. In the activation treatment solution, the concentrations of citric acid, lactic acid and sodium dodecylbenzene sulfonate are 30 g / l, 10 g / l and 1 g / l respectively, and the balance is water.
[0043] Step 2 Chemical conversion treatment: The magnesium alloy after pretreatment is treated by immersion or spraying with a conversion treatment solution. A uniform and dense conversion film is formed at room temperature, generally within 30s to 10min.
[0044] Step 3: High temperature pretreatment: The magnesium alloy parts after chemical conversion treatment are hung in a blast drying oven at 170-190°C and left to stand for 10-15 minutes to allow the hydrated compounds inside the conversion film to dehydrate and condense after high temperature pretreatment, causing the micro-crack structure on the surface of the film to be further released, which is conducive to the formation of mechanical interlocking with the subsequent electrophoretic paint film and improving the adhesion of the paint film.
[0045] Step 4: Apply electrophoretic paint: KLL-6051 electrophoretic paint from Wuhan Collier New Materials Co., Ltd. is mixed with deionized water in a weight ratio of 1:4, and stirred continuously in a constant temperature water area of 25±1℃ for 48 hours to fully mature to form an electrophoretic paint liquid. The magnesium alloy chemical conversion parts after high temperature pretreatment are immersed in the prepared electrophoretic paint liquid as the cathode, and the stainless steel plate is used as the anode for electrophoretic coating. The electrophoretic voltage is set to 60~140V, the electrophoretic time is 2~3min, the distance between the anode and cathode plates is 3~5cm, and the temperature of the electrophoretic paint liquid is controlled to 25±2℃. Rinse the magnesium alloy parts after electrophoresis with running water, drain, and cure at high temperature at 170~190℃ for 20~30min.
[0046] The technical solution of the present invention is further described in detail below through embodiments, comparative examples and drawings.
[0047] Example 1
[0048] In this embodiment, the sample is an extruded AZ31 magnesium alloy, and the specific steps are as follows:
[0049] (1) Pretreatment: Soak in alkaline solution at room temperature for 5 minutes, rinse with water, soak in activation solution, and let stand at room temperature for 2 minutes;
[0050] (2) Chemical conversion treatment: The chemical conversion treatment solution is an aqueous solution of 2g / l potassium fluorozirconate, 2g / l potassium fluorotitanate, 2g / l hydrogen peroxide, 1g / l phytic acid, and 1g / l γ-aminopropyltriethoxysilane, with a temperature of 23°C and a pH value of 2.5, and the solution is soaked for 10 minutes. The conversion film prepared by this method is off-white and has a thickness of about 4.8μm;
[0051] (3) High temperature pretreatment: stand at 180°C for 10 min, then cool to room temperature;
[0052] (4) Electrophoretic coating: The electrophoretic voltage was set to 100 V, the electrophoretic time was 2 min, the distance between the cathode and anode plates was 3 cm, and the electrophoretic paint liquid temperature was controlled at 25 ° C. The magnesium alloy parts after electrophoresis were cured at 180 ° C for 30 min.
[0053] Example 2
[0054] In this embodiment, the sample is a forged AZ80 magnesium alloy, and the specific steps are as follows:
[0055] (1) Pretreatment: Soak in alkaline solution at room temperature for 5 minutes, rinse with water, soak in activation solution, and let stand at room temperature for 3 minutes;
[0056] (2) Chemical conversion treatment: The chemical conversion treatment solution is an aqueous solution of 2g / l fluorozirconic acid, 2g / l fluorotitanic acid, 2g / l hydrogen peroxide, 1g / l tannic acid, and 1g / l γ-(methacryloyloxy)propyltrimethoxysilane, with a temperature of 23°C and a pH value of 2.5, and the spraying time is 30s. The conversion film prepared by this method is off-white and has a thickness of about 130nm;
[0057] (3) High temperature pretreatment: stand at 180°C for 10 min, then cool to room temperature;
[0058] (4) Electrophoretic coating: The electrophoretic voltage was set to 80 V, the electrophoretic time was 2 min, the distance between the cathode and anode plates was 3 cm, and the electrophoretic paint liquid temperature was controlled at 25 ° C. The magnesium alloy parts after electrophoresis were cured at 180 ° C for 30 min.
[0059] Example 3
[0060] In this embodiment, the sample is an extruded AZ31 magnesium alloy, and the specific steps are as follows:
[0061] (1) Pretreatment: Soak in alkaline solution at room temperature for 5 minutes, rinse with water, soak in activation solution, and let stand at room temperature for 3 minutes;
[0062] (2) Chemical conversion treatment: The chemical conversion treatment solution is an aqueous solution of 2g / l potassium fluorozirconate, 2g / l fluorozirconic acid, 2g / l hydrogen peroxide, 1g / l phytic acid, and 1g / l γ-(methacryloyloxy)propyltrimethoxysilane, at a temperature of 25°C and a pH value of 2.5, and the immersion time is 2 minutes. The conversion film prepared by this method is off-white and has a thickness of about 1.2μm;
[0063] (3) High temperature pretreatment: stand at 180°C for 10 min, then cool to room temperature;
[0064] (4) Electrophoretic coating: The electrophoretic voltage was set to 90 V, the electrophoretic time was 2 min, the distance between the cathode and anode plates was 3 cm, and the electrophoretic paint liquid temperature was controlled at 25 ° C. The magnesium alloy parts after electrophoresis were cured at 180 ° C for 30 min.
[0065] Example 4
[0066] In this embodiment, the sample is cast pure magnesium, and the specific steps are as follows:
[0067] (1) Pretreatment: Soak in alkaline solution at room temperature for 5 minutes, rinse with water, soak in activation solution, and let stand at room temperature for 3 minutes;
[0068] (2) Chemical conversion treatment: The chemical conversion treatment solution is an aqueous solution of 2g / l fluorozirconic acid, 2g / l fluorotitanic acid, 5g / l hydrogen peroxide, 1g / l phytic acid, and 1g / l γ-(methacryloyloxy)propyltrimethoxysilane, with a temperature of 25°C and a pH value of 2.6, and the immersion time is 5 minutes. The conversion film prepared by this method is off-white and has a thickness of about 2.8μm;
[0069] (3) High temperature pretreatment: stand at 180°C for 10 min, then cool to room temperature;
[0070] (4) Electrophoretic coating: The electrophoretic voltage was set to 90 V, the electrophoretic time was 2 min, the distance between the cathode and anode plates was 3 cm, and the electrophoretic paint liquid temperature was controlled at 25 ° C. The magnesium alloy parts after electrophoresis were cured at 180 ° C for 30 min.
[0071] Comparative Example 1
[0072] In this comparative example, the sample is an extruded AZ31 magnesium alloy, and the specific steps are as follows:
[0073] (1) Pretreatment: Soak in alkaline solution at room temperature for 5 minutes, rinse with water, soak in activation solution, and let stand at room temperature for 2 minutes;
[0074] (2) Chemical conversion treatment: The chemical conversion treatment solution is an aqueous solution of 2g / l potassium fluorozirconate, 2g / l potassium fluorotitanate, 2g / l hydrogen peroxide, 1g / l phytic acid, and 1g / l γ-aminopropyltriethoxysilane, with a temperature of 23°C and a pH value of 2.5, and the solution is soaked for 10 minutes. The conversion film prepared by this method is off-white and has a thickness of about 4.8μm;
[0075] (3) Electrophoretic coating: The electrophoretic voltage was set to 100 V, the electrophoretic time was 2 min, the distance between the cathode and anode plates was 3 cm, and the electrophoretic paint liquid temperature was controlled at 25 ° C. The magnesium alloy parts after electrophoresis were cured at 180 ° C for 30 min.
[0076] Comparative Example 2
[0077] In this comparative example, the sample is an extruded AZ31 magnesium alloy, and the specific steps are as follows:
[0078] (1) The pretreatment conditions are the same as those in process 1;
[0079] (2) Chemical conversion treatment: The homogenized sample was immersed in a manganese phosphate solution described in Patent Publication No. CN1475602A, pH = 3.5, solution temperature 50°C, film formation for 10 min, and the formed phosphate conversion film was light gray with a thickness of about 4.5 μm;
[0080] (3) Electrophoretic coating: The electrophoretic voltage was set to 100 V, the electrophoretic time was 2 min, the distance between the cathode and anode plates was 3 cm, and the electrophoretic paint liquid temperature was controlled at 25 ° C. The magnesium alloy parts after electrophoresis were cured at 180 ° C for 30 min.
[0081] Comparative Example 3
[0082] In this comparative example, the sample is an extruded AZ31 magnesium alloy, and the specific steps are as follows:
[0083] (1) The pretreatment conditions are the same as those in process 1;
[0084] (2) Chemical conversion treatment: Conversion treatment: The sample after homogenization treatment was immersed in the phosphate solution described in Patent Publication No. CN102191493A, the pH value was adjusted to 2.85, the solution temperature was controlled to 50°C, and the film forming time was 10 min. The obtained film layer was uniform and dense, with a light gray surface and a thickness of about 3.5 μm.
[0085] (3) Electrophoretic coating: The electrophoretic voltage was set to 90 V, the electrophoretic time was 2 min, the distance between the cathode and anode plates was 3 cm, and the electrophoretic paint liquid temperature was controlled at 25 ° C. The magnesium alloy parts after electrophoresis were cured at 180 ° C for 30 min.
[0086] The results of the performance test are as follows:
[0087] 1. Surface condition after electrophoretic coating
[0088] The surface of the chemical conversion film-electrophoretic composite coating prepared according to the above examples 1 to 4 and comparative examples 1 to 3 is uniformly grayish white, without pits and shrinkage holes. The thickness of the electrophoretic paint film is in the range of 20 to 25 μm, which meets the requirements for industrial use.
[0089] 2. Chemical conversion film corrosion resistance test
[0090] According to GB10124-88 full immersion corrosion test standard, the magnesium alloy conversion coating samples (not electrophoretically coated) prepared according to the methods of Example 1 and Comparative Examples 1 to 3 were completely immersed in a 3.5wt% NaCl solution, and the ratio of the volume of the corrosive medium to the working area of the sample was greater than 20ml / cm 2 , pH = 6.5 ~ 7, temperature controlled at 25 ± 1 ° C. After 48 hours, the corrosion morphology of the film layer was observed. Two pittings with a radius of less than 1 mm appeared on the surface of Example 1, see attached Figure 1 (a); Comparative Example 1 The surface of the chemical conversion film is uniform and no obvious corrosion occurs, see Attached Figure 1 (b); Comparative Examples 2 to 3 have 2 to 4 pittings with a radius of less than 1 mm on the surface of the phosphate coating, see Attached Figure 1 (c) Figure 1 (d).
[0091] 3. Adhesion test after electrophoretic coating
[0092] Philips XL30 FEG scanning electron microscope was used to observe the microscopic cross-sectional morphology of Example 1 and Comparative Example 1. The test results are shown in the attached figure. Figure 2 As shown. According to GB / T 5210-2006 standard, the electrophoretic composite coatings prepared by the processes of Examples 1 to 4 and Comparative Examples 1 to 3 were subjected to adhesion tests using a PosiTest AT-A pull-off tester. First, the surface of the electrophoretic coating to be tested was gently polished with 500# to remove grease and dirt on the coating surface, and an adhesive was used to attach a test column with a diameter of 20 mm to the electrophoretic coating to be tested. Let it stand at room temperature for 24 hours, and after the adhesive is fully cured, it was tested using a pull-off tester. Among them, the paint film adhesion under the conditions of Examples 1 to 4 was about 20MPa, and all of them were adhesive fractures, and the actual paint film adhesion was greater than or equal to 20MPa. The paint film adhesion under the conditions of Comparative Examples 1 to 3 were 4.5MPa, 5.1MPa, and 6.2MPa, respectively, and the paint film fracture position was the chemical conversion film / electrophoretic paint film interface.
[0093] Combined with the above results, it can be seen that the corrosion resistance of the magnesium alloy chemical conversion film of the present invention is not inferior to that of the traditional phosphate conversion film, and the corrosion resistance is even higher than that of the phosphate conversion film without high temperature pretreatment process, see attached Figure 1 In Examples 1 to 4, after adding a high temperature pretreatment step before electrophoretic coating, the microcracks on the surface of the chemical conversion film are perfectly filled by the electrophoretic paint film, and the mechanical interlocking structure formed significantly improves the adhesion of the paint film, see the attached Figure 2 (a); In Examples 1 to 4, the paint film adhesion can reach more than 20 MPa, and the pull-out failure is the adhesive fracture, see attached Figure 3 (a). In comparative example 1, without adding a high temperature pretreatment step, there are local defects between the chemical conversion film and the electrophoretic paint film, see attached Figure 2 (b) The paint film adhesion is only 4.5MPa, and the pull-out failure position is at the interface of the chemical conversion film / electrophoretic paint film, see attached Figure 3 (b).
[0094] In addition, the chemical conversion treatment solution can be used for immersion or spraying to achieve uniform film formation on the substrate surface at room temperature. Its corrosion resistance is comparable to that of the traditional phosphate conversion film. Combined with the high-temperature pretreatment process, the hydrated compounds inside the chemical conversion film are released in advance. The fully expanded microcracks can form a mechanical interlocking structure with the electrophoretic paint film, significantly improving the adhesion of the paint film and forming a good interface bond with the electrophoretic paint film.
[0095] The implementation results show that the magnesium alloy electrophoretic coating process of the present invention is simple to operate, efficient, low-cost, has no emission of polluting ions such as phosphate, chromium, and nickel, and the prepared electrophoretic composite coating has strong bonding with the substrate. It is an electrophoretic coating method suitable for industrial production of magnesium alloys.
Claims
1. A magnesium alloy electrophoretic coating process, characterized in that: The specific steps are as follows: Step 1: Pre-treatment of magnesium alloy (1) Soak the magnesium alloy in an alkaline solution containing sodium hydroxide, sodium silicate, and sodium carbonate at room temperature for 3 to 5 minutes to remove residual grease and dirt on the surface; (2) The magnesium alloy after alkali washing is washed with running water and then immersed in an activation treatment solution containing citric acid, lactic acid, and sodium dodecyl sulfate, and treated at room temperature for 5s to 2min to coarsen the surface of the magnesium matrix and increase the active points, which is conducive to the uniform deposition of film-forming substances during the chemical conversion process; Step 2: Chemical conversion of magnesium alloy The magnesium alloy after pretreatment is treated by dipping or spraying with a conversion treatment solution, and a uniform and dense conversion film is formed within 30s to 10min at room temperature. The conversion treatment solution contains: zirconate titanic acid and / or zirconate titanate, hydrogen peroxide, film-forming aid, silane coupling agent, and the pH value is in the range of 2.0 to 3.5; Step 3: High temperature pretreatment before painting The magnesium alloy parts after chemical conversion treatment are hung in a blast drying oven at 170-190°C and left to stand for 10-15 minutes. The hydrated compounds in the conversion film are dehydrated and condensed after high-temperature pretreatment, causing the micro-crack structure on the surface of the film to be further released, which is conducive to the formation of mechanical interlocking with the subsequent electrophoretic paint film and improving the adhesion of the paint film; Step 4: Apply electrophoretic paint (1) mixing the electrophoretic paint with deionized water in a weight ratio of 1:3 to 1:5, and stirring continuously for 48 hours in a constant temperature water area of 25±1°C to fully mature to form an electrophoretic paint liquid; (2) immersing the magnesium alloy chemical conversion component after high temperature pretreatment in the prepared electrophoretic paint solution, with the magnesium alloy component as the cathode and the stainless steel plate as the anode, for electrophoretic coating; (3) The magnesium alloy parts after electrophoresis are rinsed with running water, drained, and high-temperature cured at 170 to 190° C. for 20 to 30 minutes.
2. The magnesium alloy electrophoretic coating process according to claim 1, characterized in that: In the alkaline solution of step 1, the concentrations of sodium hydroxide, sodium silicate and sodium carbonate are 20-40 g / l, 20-40 g / l and 10-30 g / l respectively, and the balance is water.
3. The magnesium alloy electrophoretic coating process according to claim 1, characterized in that: In the activation treatment solution of step 1, the concentrations of citric acid, lactic acid and sodium dodecylbenzene sulfonate are 20-40 g / l, 5-15 g / l and 0.5-2 g / l respectively, and the balance is water.
4. The magnesium alloy electrophoretic coating process according to claim 1, characterized in that: In the conversion treatment solution of step 2, the concentration of zirconyl titanic acid and / or zirconyl titanate is 2-5 g / l, the concentration of hydrogen peroxide is 2-5 g / l, the concentration of film-forming aid is 0.5-5 g / l, the concentration of silane coupling agent is 1-5 g / l, and the balance is water.
5. The magnesium alloy electrophoretic coating process according to claim 1 or 4, characterized in that: The zirconyl titanic acid is one of fluorozirconic acid and fluorotitanic acid or a combination thereof, the zirconyl titanate is one of potassium fluorozirconate and potassium fluorotitanate or a combination thereof, the film-forming aid is one of phytic acid and tannic acid or a combination thereof, and the silane coupling agent is one of γ-aminopropyltriethoxysilane, γ-(2,3-epoxypropoxy)propyltrimethoxysilane, and γ-(methacryloyloxy)propyltrimethoxysilane or a combination of two or more thereof.
6. The magnesium alloy electrophoretic coating process according to claim 1 or 4, characterized in that: The thickness of the film after the chemical conversion treatment in step 2 is controllable within the range of 100 nm to 5 μm, and the corrosion resistance is comparable to that of the traditional phosphate conversion film.
7. The magnesium alloy electrophoretic coating process according to claim 1, characterized in that: In step 3, before high-temperature pretreatment, the magnesium alloy chemical conversion parts need to be fully cleaned with deionized water and drained; the parts after high-temperature pretreatment are cooled at room temperature and then used for later use.
8. The magnesium alloy electrophoretic coating process according to claim 1, characterized in that: In step 4, the aging process of the prepared electrophoretic paint solution is carried out by magnetic stirring.
9. The magnesium alloy electrophoretic coating process according to claim 1, characterized in that: In step 4, electrophoretic coating, the electrophoretic voltage is 60-140 V, the electrophoretic time is 2-3 min, the distance between the anode and cathode plates is 3-5 cm, and the temperature of the electrophoretic paint solution is controlled at 25±2°C.
10. The magnesium alloy electrophoretic coating process according to claim 1, characterized in that: After electrophoretic coating, the electrophoretic paint film adhesion of magnesium alloy parts is ≥20MPa.