Magnetic response flexible sensor and preparation method and application thereof

Through the preparation method of magnetically responsive flexible sensors, combined with electrospinning and functionalized conductive polymer modification, the integration of cell mechanics control and real-time monitoring is achieved, which solves the problem of difficulty in obtaining real-time cell mechanics transduction biochemical information in the existing technology. It realizes remote control of external magnetic fields and monitoring of signal molecules, and is suitable for applications in many fields.

CN118776594APending Publication Date: 2024-10-15WUHAN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410835894.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

It is difficult to integrate cell mechanical manipulation and real-time monitoring of biochemical signals with existing technology, and the characterization of accumulated biochemical information after mechanical loading by conventional flexible sensors is difficult to obtain in real time.

Method used

Using the preparation method of magnetically responsive flexible sensors, an elastic polymer solution containing magnetic materials was prepared through electrospinning. Combined with hydrophilic treatment and functionalized conductive polymer modification, the integration of mechanical control and real-time monitoring was achieved, and remote control was achieved using external magnetic fields. cells and monitor the release of signaling molecules in real time.

Benefits of technology

It achieves remote, instantaneous, reversible multi-directional mechanical control, expands the mechanical control form of flexible sensors, has excellent mechanical control performance and electrochemical sensing performance, and can monitor the release of signal molecules of cells under mechanical stimulation in real time. It is suitable for Tissue engineering and implantable medical devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118776594A_ABST
    Figure CN118776594A_ABST
Patent Text Reader

Abstract

The invention discloses a magnetic response flexible sensor and a preparation method and application thereof. The sensor is prepared through an electrostatic spinning technology, has superparamagnetism and lower Young modulus, and can realize multi-form remote mechanical control through an external magnetic field. The surface of the sensor is modified with a functionalized conductive polymer, and detection of various target objects can be realized by compounding different catalysts. The biosensor has good mechanical stability and electrochemical sensing capability, not only can realize remote mechanical control of cells cultured on the biosensor, but also can dynamically monitor biochemical signal molecules released by the cells in the process in real time, and provides an important tool for in-situ and real-time monitoring of mechanical control and biochemical response of the cells.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the fields of chemistry, material science and biomedical engineering, and particularly relates to a magnetic response flexible sensor and a preparation method and application thereof. Background Art

[0002] Cells in the body can sensitively sense mechanical stimuli and regulate cell behavior and function by converting them into biochemical signal molecules, such as nitric oxide (NO), reactive oxygen species, growth factors, etc. In order to simulate the mechanical microenvironment of cells in the body, a variety of mechanical manipulation methods have been developed, such as using microfluidic chips to simulate the fluid shear force on cells, and using a stretching instrument to apply tensile stress to cells cultured on elastic films. In addition, with the help of high-resolution technologies such as atomic force microscopy, optical tweezers, and magnetic tweezers, single / subcellular local mechanical manipulation can be achieved. In order to evaluate the changes in cell biochemical information caused by mechanical signals, analytical techniques such as PCR, immunoblotting, and fluorescent staining are often used to provide information on cell gene transcription, protein structure and expression, and cell adhesion status. However, since these cell mechanical manipulation and detection technologies are independent of each other, they can usually only characterize the accumulated biochemical information after long-term mechanical loading, and may require the destruction of cell structure, making it difficult to obtain biochemical information of transient changes in cell mechanical transduction in real time.

[0003] Therefore, there is an urgent need to develop an integrated platform that can simultaneously realize multi-form mechanical manipulation and real-time monitoring of biochemical signals. Summary of the invention

[0004] In view of the above technical problems, the primary purpose of the present invention is to break through the limitations of existing mechanical manipulation methods in the application of flexible sensors and provide a magnetically responsive flexible sensor that integrates mechanical manipulation and real-time monitoring.

[0005] Another object of the present invention is to provide a method for preparing the above-mentioned magnetically responsive flexible sensor, which integrates mechanical manipulation and real-time monitoring, and the preparation method is simple and controllable.

[0006] Another object of the present invention is to provide an application of the above-mentioned magnetically responsive flexible sensor to achieve a breakthrough in the real-time monitoring of signal molecules in the process of cell mechanical signal transduction using the magnetically responsive flexible sensor.

[0007] The purpose of the present invention is achieved through the following technical solutions:

[0008] In a first aspect, a method for preparing a magnetically responsive flexible sensor is provided, comprising the following steps:

[0009] Prepare solution A, which is an elastic polymer solution containing magnetic material;

[0010] Electrospinning solution A onto an elastic film to obtain a magnetically responsive flexible substrate;

[0011] The magnetically responsive flexible substrate is hydrophilically treated and then the surface is modified with a functional conductive polymer to obtain a magnetically responsive flexible sensor.

[0012] In a possible implementation manner, the elastic polymer solution is prepared by dissolving the elastic polymer in an organic solvent.

[0013] Specifically, the elastic polymer includes one or both of polyurethane (PU) and polylactic acid.

[0014] In a possible implementation manner, the magnetic material includes an iron-based material and a cobalt-based material. Preferably, the iron-based material is ferroferric oxide nanoparticles (Fe 3 O 4 NPs), and the cobalt-based material is cobalt nanowires.

[0015] In a possible implementation manner, the elastic film includes a combination of one or more of polydimethylsiloxane (PDMS), polyethylene terephthalate, Ecoflex and polymethyl methacrylate.

[0016] In a possible implementation manner, the hydrophilic treatment includes one or more of plasma treatment, polydopamine treatment and polylysine treatment.

[0017] In one possible embodiment, the method for modifying a functionalized conductive polymer on a surface includes:

[0018] The hydrophilically treated magnetically responsive flexible substrate is placed in a solution of a functionalized conductive polymer and reacted to obtain the substrate.

[0019] In an improved implementation manner, the preparation method of the functionalized conductive polymer solution is as follows: the conductive polymer is formulated into a solution, and a tensile enhancer, a molecular or metal catalyst and a conductive enhancer are added and dispersed.

[0020] Specifically, the conductive polymer includes one or more of poly (3,4-ethylenedioxythiophene) (PEDOT), polyacetylene, and polypyrrole.

[0021] Specifically, the molecular catalyst includes one or both of iron porphyrin (FeTCP) and cobalt sulfonated phthalocyanine (CoPcS); the metal catalyst is platinum nanoparticles (Pt NPs).

[0022] Specifically, the conductivity enhancer includes one of dimethyl sulfoxide and ionic liquid.

[0023] Specifically, the tensile enhancer is sorbitol, Triton X-100 or polyethylene oxide.

[0024] In a second aspect, a magnetically responsive flexible sensor is provided, which is prepared by the method described in the first aspect.

[0025] In a possible implementation manner, the magnetically responsive flexible sensor is further connected to a wire.

[0026] The third aspect provides the application of the aforementioned magnetically responsive flexible sensor in cell mechanical manipulation and signal molecule monitoring.

[0027] In a possible implementation manner, the application method in signal molecule monitoring comprises the following steps:

[0028] Setting up a cell culture pool on the magnetically responsive flexible sensor;

[0029] Inoculating cells in a cell culture tank;

[0030] Place a magnet above the cell culture pool, control the deformation amplitude by controlling the distance between the magnets, and monitor the signal molecules released by the cells under mechanical stimulation in real time.

[0031] The present invention has the following technical effects:

[0032] The present invention provides a magnetic response flexible sensor that integrates mechanical manipulation and real-time monitoring, and the preparation method is simple and controllable. Compared with conventional flexible sensors, this sensor can realize remote, instantaneous, reversible and multi-directional mechanical manipulation, expand the mechanical manipulation form of flexible sensors, and facilitate the preparation of a miniaturized control and detection integrated platform.

[0033] The magnetically responsive flexible sensor described in the present invention, based on its excellent mechanical manipulation performance, electrochemical sensing performance and good biocompatibility, realizes remote induction of cell and electrode deformation by external magnetic field, and monitors the release of signal molecules of cells under mechanical stimulation in real time.

[0034] In addition, the magnetic field has good tissue penetration. The magnetically responsive flexible sensor of the present invention can provide a new control and detection platform for the fields of tissue engineering, implantable medical devices, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0036] Figure 1 is a flow chart for preparing magnetically responsive flexible sensors.

[0037] Figure 2is the microstructure diagram of the magnetically responsive flexible sensor, where Figure 2 A is the scanning electron microscope image of the magnetic responsive flexible sensor. Figure 2 B is the projection electron microscope image of the magnetically responsive flexible sensor.

[0038] Figure 3 There are different Fe 3 O 4 (A) Magnetic hysteresis loop and (B) stress-strain curve of magnetically responsive flexible sensors with different NPs contents.

[0039] Figure 4 This is a physical picture of the remote control of the deformation of the magnetic response flexible sensor, where: Figure 4 (A) No external magnetic field, Figure 4 (B) There is an external magnetic field.

[0040] Figure 5 (A) is a schematic diagram of the calculation of the deformation amplitude of the magnetically responsive flexible sensor; Figure 5 (B) is the deformation amplitude of the magnetic response flexible sensor and Fe 3 O 4 Corresponding relationship between NPs content and external magnetic field intensity.

[0041] Figure 6 (A~C) are actual pictures of using magnetically responsive flexible sensors for different forms of mechanical manipulation, where the upper picture is a top view when there is no external magnetic field, and the lower picture is a side view when there is an external magnetic field. Figure 6 (D) is a photo of a single magnetically responsive nanofiber being manipulated by an electromagnetic needle, where: Figure 6 (D1) No current is applied to the external coil of the electromagnetic needle. Figure 6 (D2) A current of 0.8A is applied to the external coil of the electromagnetic needle.

[0042] Figure 7 (A) is the UV spectrum of FeTCP-functionalized conductive polymer PEDOT. Figure 7 (B) is the cyclic voltammetric response of the magnetically responsive flexible sensor to the target NO during deformation.

[0043] Figure 8 (A) is the cyclic voltammetric response of the magnetically responsive flexible sensor of PEDOT modified with CoPcS functionalization to glutathione (GSH); Figure 8 (B) The magnetic responsiveness of the PEDOT conductive polymer functionalized with Pt NPs to hydrogen peroxide (H 2 O 2 )'s cyclic voltammetric response

[0044] Fig. 9 (A) is a fluorescence micrograph characterizing cell viability; Fig. 9(B) is a fluorescence micrograph of the deformation of the magnetically responsive flexible sensor and cells cultured thereon induced by an external magnetic field, wherein the magnetically responsive flexible sensor is marked with yellow fluorescence and the cells are marked with green fluorescence.

[0045] Fig.10 This is the real-time monitoring result of NO release from osteoblasts under different deformation amplitudes by magnetically responsive flexible sensors. Fig.10 The deformation amplitude of (A) is 5%, Fig.10 (B) The deformation amplitude is 10%.

[0046] Fig.11 This is a schematic diagram of the action of the magnetically responsive flexible sensor prepared in the present invention under a magnetic field. DETAILED DESCRIPTION

[0047] The endpoints and any values ​​of the ranges disclosed in the present invention are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be regarded as specifically disclosed in the present invention.

[0048] The following will be combined with the specific embodiments of the present invention and the drawings of the specification to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0049] A method for preparing a magnetically responsive flexible sensor comprises the following steps:

[0050] Prepare solution A, which is an elastic polymer solution containing magnetic material;

[0051] Electrospinning solution A onto an elastic film to obtain a magnetically responsive flexible substrate;

[0052] The magnetically responsive flexible substrate is hydrophilically treated and then the surface is modified with a functional conductive polymer to obtain a magnetically responsive flexible sensor.

[0053] In a possible implementation manner, the elastic polymer solution is prepared by dissolving the elastic polymer in an organic solvent.

[0054] Specifically, the elastic polymer includes one or both of polyurethane (PU) and polylactic acid.

[0055] In a possible implementation manner, the magnetic material includes an iron-based material and a cobalt-based material.

[0056] In a possible implementation manner, the elastic film includes a combination of one or more of polydimethylsiloxane (PDMS), polyethylene terephthalate, Ecoflex and polymethyl methacrylate.

[0057] In a possible implementation manner, the hydrophilic treatment includes one or more of plasma treatment, polydopamine treatment and polylysine treatment.

[0058] In one possible embodiment, the method for modifying a functionalized conductive polymer on a surface includes:

[0059] The hydrophilically treated magnetically responsive flexible substrate is placed in a solution of a functionalized conductive polymer and reacted to obtain the substrate.

[0060] In an improved embodiment, the preparation method of the functionalized conductive polymer solution is as follows: the conductive polymer is formulated into a solution, and a tensile enhancer, a molecular or metal catalyst and a conductive enhancer are added and dispersed.

[0061] Specifically, the conductive polymer includes one or more of poly (3,4-ethylenedioxythiophene), polyacetylene, and polypyrrole.

[0062] Specifically, the molecular catalyst includes one or both of iron porphyrin and sulfonated cobalt phthalocyanine; the metal catalyst is platinum nanoparticles (Pt NPs). The molecular catalyst or metal catalyst is added to improve the sensing performance of the sensor to the target object.

[0063] Specifically, the conductive enhancer includes one of dimethyl sulfoxide and an ionic liquid. Preferably, the ionic liquid is bis(trifluoromethane)sulfonyl imide lithium salt. The addition of the conductive enhancer is conducive to forming a continuous conductive network, improving the conductive properties and electrochemical sensing properties of the material.

[0064] Specifically, the tensile enhancer is sorbitol, Triton X-100 or polyethylene oxide, which is used to enhance the tensile properties of the material.

[0065] It should be noted that the conductive enhancer and the stretch enhancer are two substances that must be added. Only by using them together can the sensor have good conductivity and electrochemical mechanical stability after deformation to ensure its sensing performance, and can also ensure that it can maintain stable performance after multiple deformations.

[0066] Example 1

[0067] PU / Fe 3 O 4 The preparation process of magnetic responsive flexible sensor is as follows Figure 1 As shown, the specific steps are as follows:

[0068] (1) Preparation of electrospinning solution: PU with a molecular weight of 150,000 (mass fraction 10%) was dissolved in a mixed solution of tetrahydrofuran and N,N-dimethylformamide (volume ratio 3:1), and 0.4 g / mL of Fe 3 O 4 NPs, adjust the speed to 500 rpm, and mechanically stir for 1 hour to obtain PU / Fe 3 O 4 Electrospinning solution.

[0069] (2) Preparation of hollow substrate: 3 g of liquid PDMS with a prepolymer and curing agent mass ratio of 10:1 was poured onto a clean silicon wafer with a diameter of 7.5 cm, and spun on a spinner at 600 rpm for 9 seconds, heated at 75°C for 2 hours to cure the PDMS, and peeled off from the silicon wafer to obtain a PDMS film with a thickness of about 200 μm. It was cut into 20×20 mm sheets with a blade, and a 15×15 mm hollow structure was cut out in the middle.

[0070] (3) Preparation of functionalized conductive polymer: 0.1 g sorbitol (5% by mass) was added to 2 mL of commercial conductive polymer PEDOT:PSS solution (Clevios PH1000) and the sorbitol functionalized PEDOT solution (s-PEDOT) was obtained after it was fully dissolved. Then 8 mL

[0071] Anhydrous ethanol, diluted at a ratio of 2:8 (volume ratio), and 1.76 mg of molecular catalyst FeTCP was added

[0072] (0.2 mM) and 0.5 mL of dimethyl sulfoxide were added and ultrasonicated for two hours to obtain a FeTCP-functionalized conductive PEDOT solution (FeTCP / s-PEDOT).

[0073] (4) Preparation of PU / Fe 3 O 4 Magnetic responsive flexible substrate: Use a syringe to draw the homogeneous PU / Fe obtained in step (1) 3 O 4 The electrospinning liquid was fixed on the injection pump of the electrospinning device, the needle was connected to the positive electrode wire, the device was checked, the power was turned on, and various parameters were adjusted. The voltage was about 16 kV, the flow rate of the injection pump was 1 mL / h, and the distance between the needle and the syringe was about 15 cm. The hollow substrate in step (2) was fixed on the rotating drum receiver and the PU / Fe ejected was received at a speed of 1000 rpm. 3 O 4 Nanofibers. Electrospinning was carried out in a closed environment with a chamber temperature of 40 °C, a humidity of 30%, and an electrospinning time of 25 min.

[0074] (5) Modifying the surface of the magnetically responsive substrate with a conductive polymer: The magnetically responsive flexible substrate prepared in step (4) was treated with plasma hydrophilic treatment for 5 minutes, then immersed in the functionalized conductive polymer FeTCP / s-PEDOT solution obtained in step (3) for 20 minutes, and heated at 110°C for 10 minutes.

[0075] On this basis, the edge of the magnetically responsive substrate is connected to the tin foil through conductive carbon glue. After the conductive carbon glue solidifies, liquid PDMS is coated at the connection to insulate and fix the connection point to obtain a magnetically responsive flexible sensor that is easy to electrically connect.

[0076] The above-mentioned magnetically responsive flexible sensor prepared based on electrospinning technology is self-supporting and can achieve instantaneous and reversible magnetic response.

[0077] like Figure 2 (B) The results of transmission electron microscopy show that Fe 3 O 4 NPs are evenly distributed in the nanofibers.

[0078] Figure 3 The hysteresis loop of (A) shows that the sensor has superparamagnetism. Figure 3 The stress-strain curve (B) shows that the sensor has a low Young's modulus and is very soft.

[0079] like Figure 4 Shown is a physical picture of the remotely controlled deformation of the magnetically responsive flexible sensor.

[0080] Figure 5 (B) is the deformation amplitude of the magnetic response flexible sensor and Fe 3 O 4 The corresponding relationship between NPs content and external magnetic field strength. It can be seen from the figure that with the increase of magnetic field intensity, the deformation amplitude increases linearly.

[0081] Figure 6 (A~C) are actual pictures of using magnetically responsive flexible sensors for different forms of mechanical manipulation. It can be seen from the pictures that magnetically responsive flexible sensors can achieve good mechanical manipulation.

[0082] like Figure 7 As shown in (B), the sensor still maintains good electrochemical detection performance for NO during the deformation process.

[0083] Example 2

[0084] The preparation method is the same as in Example 1, except that:

[0085] 1. In step (1), polylactic acid is used as an elastic polymer material for electrospinning to prepare a magnetically responsive flexible substrate;

[0086] 2. In step (3), sulfonated cobalt phthalocyanine (CoPcS) is used instead of iron porphyrin (FeTCP) as a molecular catalyst, Triton X-100 is used instead of sorbitol as a tensile enhancer, and an ionic liquid, lithium bis(trifluoromethane)sulfonyl imide, is used as a conductivity enhancer.

[0087] Example 3

[0088] The preparation method is the same as in Example 1, except that:

[0089] 1. In step (2), polyethylene terephthalate is used to prepare an elastic substrate;

[0090] 2. In step (3), polyethylene oxide is used instead of sorbitol as a tensile enhancer, and an ionic liquid, lithium bis(trifluoromethane)sulfonyl imide, is used as a conductive enhancer.

[0091] Example 4

[0092] The preparation method is the same as in Example 1, except that:

[0093] 1. In step (2), an elastic substrate is prepared using Ecoflex;

[0094] 2. In step (3), platinum nanoparticles (Pt NPs) are used instead of iron porphyrin (FeTCP) as the metal catalyst.

[0095] Application Example 1

[0096] FeTCP / s-PEDOT / PU / Fe 3 O 4 The magnetically responsive flexible sensor monitors the release of signal molecules during cell mechanotransduction in real time. The specific steps are as follows:

[0097] (1) Liquid PDMS with a prepolymer and curing agent mass ratio of 10:1 was poured around a customized metal columnar mold with a length and width of 15×15 mm and a height of 4 mm. The PDMS pouring height was 2 mm. After it was cured, it was removed to obtain a PDMS hollow square frame with a length and width of 15×15 mm and a height of 2 mm.

[0098] (2) A PDMS hollow square frame was placed above the hollow area of ​​the magnetically responsive flexible sensor in Example 1 as a cell culture pool, and sterilized together with the magnetically responsive flexible sensor by UV irradiation on a sterile operating table for 10 hours. After rinsing with PBS three times, a cell culture pool with a density of 1×10 6 MC3T3-E1s were inoculated onto the sensor surface for culture. The fluorescence characterization results of cell activity after 36 hours of culture are shown in Figure 2. Fig. 9As shown in (A), it further demonstrates that the sensor has good biocompatibility.

[0099] (3) After the cells are cultured on the electrode surface in step (3) for 10 hours, real-time monitoring of the release of signal molecules from the cells is performed. A magnet is placed above the magnetically responsive flexible sensor, and the sensor is deformed to different degrees by controlling the distance between the magnet and the sensor. Fig.10 As shown in the figure, at the moment when osteoblasts are stimulated, the sensor detects a rising current signal, and the greater the deformation amplitude, the greater the current. When cells are not inoculated on the sensor surface, there is no obvious current rise. When the cells are incubated with the nitric oxide synthase inhibitor L-NMMA in advance, there is no obvious current rise. The above results prove that the increase in current is due to the oxidation of the signal molecule NO released by the cells under mechanical stimulation on the sensor surface. Fig.11 A schematic diagram showing the operation of a magnetically responsive flexible sensor under a magnetic field.

[0100] The above examples show that the magnetically responsive flexible sensor prepared by the method of the present invention has excellent mechanical manipulation and sensing performance, can remotely induce deformation of the sensor and cells through an external magnetic field, and monitor in real time the signal molecules released by the cells during mechanical transduction.

[0101] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a magnetically responsive flexible sensor, characterized in that: The following steps are involved: Prepare solution A, which is an elastic polymer solution containing magnetic material; Electrospinning solution A onto an elastic film to obtain a magnetically responsive flexible substrate; The magnetically responsive flexible substrate is hydrophilically treated and then the surface is modified with a functional conductive polymer to obtain a magnetically responsive flexible sensor.

2. The method for preparing a magnetically responsive flexible sensor according to claim 1, characterized in that: The elastic polymer solution is prepared by dissolving the elastic polymer in an organic solvent.

3. The magnetically responsive flexible sensor according to claim 1, characterized in that: The magnetic material includes an iron-based material and a cobalt-based material.

4. The magnetically responsive flexible sensor according to claim 1, characterized in that: The elastic film includes a combination of one or more of polydimethylsiloxane, polyethylene terephthalate, Ecoflex and polymethyl methacrylate.

5. The magnetically responsive flexible sensor according to claim 1, characterized in that: The hydrophilic treatment includes one or more of plasma treatment, polydopamine treatment and polylysine treatment.

6. The magnetically responsive flexible sensor according to claim 1, characterized in that: The method for modifying the functional conductive polymer on the surface is as follows: placing the hydrophilic treated magnetically responsive flexible substrate in a solution of the functional conductive polymer to react; The method for preparing the functionalized conductive polymer solution is as follows: the conductive polymer is prepared into a solution, and a tensile enhancer, a molecular or metal catalyst and a conductive enhancer are added and dispersed to obtain the solution.

7. The magnetically responsive flexible sensor according to claim 6, characterized in that: The conductive polymer includes one or more of poly (3,4-ethylenedioxythiophene), polyacetylene, and polypyrrole; the molecular catalyst includes one or two of iron porphyrin and sulfonated cobalt titanium cyanine; the metal catalyst is platinum nanoparticles; the conductive enhancer includes one of dimethyl sulfoxide and ionic liquid; and the tensile enhancer is sorbitol, Triton X-100, or polyethylene oxide.

8. A magnetically responsive flexible sensor, characterized in that: The method is prepared by any one of claims 1 to 7.

9. Application of the magnetically responsive flexible sensor according to claim 8 in cell mechanics manipulation and signal molecule monitoring.

10. The use of the magnetically responsive flexible sensor according to claim 9 in cell mechanics manipulation and signal molecule monitoring, characterized in that: The application method in signal molecule monitoring comprises the following steps: Setting up a cell culture pool on the magnetically responsive flexible sensor; Inoculating cells in a cell culture tank; Place a magnet above the cell culture pool, control the deformation amplitude by controlling the distance between the magnets, and monitor the signal molecules released by the cells under mechanical stimulation in real time.