Optical laminate
By optimizing the thickness and peeling force of the surface protection film and spacer in the optical laminate, combined with the peelable adhesive layer design, the problems of insufficient transportability and peelability of the existing optical laminate are solved, and excellent optical laminates are achieved. Laminate performance.
Patent Information
- Application Number
- CN202411010213.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2019-08-21
- Filing Date
- 2020-06-19
- Publication Date
- 2024-10-15
AI Technical Summary
In the process of thinning the existing optical laminate, there are problems such as insufficient conveyability and insufficient peelability of the surface protective film and separator.
An optical laminate is designed, including a polarizing plate with a thickness of less than 60 μm, a surface protection film with a thickness of more than 40 μm, and a spacer with a thickness of 35 μm to 80 μm. The peeling force of the surface protection film is 0.10N/25mm~0.50N/2. 5mm, the elastic modulus is 2.00×109Pa or more, and the peeling force of the separator is less than 0.28N/25mm. It is temporarily bonded to the opposite side of the polarizer through a peelable adhesive layer and surface protection film to achieve excellent transportability and Peelability.
It achieves excellent conveyability of the optical laminate and excellent peelability of the surface protection film and separator, thereby improving the thinness and performance of the image display device.
Smart Images

Figure CN118778166A_ABST
Abstract
Description
[0001] This case is a divisional application of an application with a filing date of June 19, 2020, application number 202080058474.5, and invention name “Optical Laminate”. Technical Field
[0002] The present invention relates to optical stacks. Background Art
[0003] In a liquid crystal display device, which is a representative image display device, polarizers are arranged on both sides of the liquid crystal unit due to its image formation method. The polarizer is typically manufactured by dyeing a polyvinyl alcohol (PVA) resin film with a dichroic substance such as iodine (for example, Patent Documents 1 and 2). In recent years, the demand for thinner image display devices has increased. Therefore, further thinning is also required for the polarizer. A thin polarizer (a polarizing plate including the polarizer in practical applications) can be provided, for example, in the form of an optical laminate formed by laminating an adhesive layer, a surface protection film, and an insulator. However, such an optical laminate has problems such as insufficient transportability and insufficient peelability of the surface protection film and the insulator.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent No. 5048120
[0007] Patent Document 2: Japanese Patent Application Publication No. 2013-156391 Summary of the invention
[0008] Problem that the invention aims to solve
[0009] The present invention has been made to solve the above-mentioned conventional problems, and its main object is to provide an optical laminate having a thin polarizing plate, a surface protection film and a separator, and having excellent transportability and excellent releasability of the surface protection film and the separator.
[0010] Solutions for solving problems
[0011] The optical laminate of the present invention comprises: a polarizing plate; an adhesive layer provided on one side of the polarizing plate; a separator temporarily bonded to the side of the adhesive layer opposite to the polarizing plate in a releasable manner; and a surface protection film temporarily bonded to the side of the polarizing plate opposite to the adhesive layer in a releasable manner, wherein the thickness of the polarizing plate is 60 μm or less, the thickness of the surface protection film is 40 μm or more, the peeling force of the surface protection film is 0.10 N / 25 mm to 0.50 N / 25 mm, and the elastic modulus of the surface protection film is 2.00×10 9Pa or more, the thickness of the separator is 35 μm to 80 μm, and the peeling force of the separator is less than 0.28 N / 25 mm.
[0012] In one embodiment, the polarizing plate includes a polarizer, and the polarizer is composed of a polyvinyl alcohol-based resin film containing iodine.
[0013] In one embodiment, the polarizer has a thickness of 10 μm or less.
[0014] In one embodiment, the polarizer has an iodine content of 10 wt % to 25 wt %.
[0015] Effects of the Invention
[0016] According to the present invention, for an optical laminate comprising a thin polarizing plate, a surface protection film and an insulator, by optimizing the thickness, peeling force and elastic modulus of the surface protection film, and the thickness and peeling force of the insulator, it is possible to achieve an optical laminate with excellent transportability and excellent peeling properties of the surface protection film and the insulator. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 This is a schematic cross-sectional view of an optical layered body according to one embodiment of the present invention. DETAILED DESCRIPTION
[0018] Hereinafter, embodiments of the present invention will be described, but the present invention is not limited to these embodiments.
[0019] A. Overall structure of optical laminate
[0020] Figure 1 1 is a schematic cross-sectional view of an optical laminate according to an embodiment of the present invention. The optical laminate 100 shown in the figure comprises: a surface protection film 10, a polarizing plate 20, an adhesive layer 30, and a separator 40. The thickness of the polarizing plate 20 is 60 μm or less. Furthermore, the thickness of the surface protection film 10 is 40 μm or more, the peeling force thereof is 0.10 N / 25 mm to 0.50 N / 25 mm, and the elastic modulus thereof is 2.00 × 10 9 Pa or more. Furthermore, the thickness of the separator 40 is 35 μm to 80 μm, and the peeling force thereof is less than 0.28 N / 25 mm. The components of the optical laminate will be described in more detail below.
[0021] B.Polarizing plate
[0022] The polarizing plate 20 typically includes a polarizer 22 and a protective layer disposed on one side or both sides thereof. Preferably, as shown in the example in the figure, in the polarizing plate 20, the protective layer 21 is disposed on one side of the polarizer 22. The thickness of the polarizing plate is 60 μm or less, preferably 40 μm or less, and more preferably 35 μm or less. The lower limit of the thickness of the polarizing plate may be, for example, 20 μm.
[0023] B-1. Polarizer
[0024] The polarizer 22 is typically made of a polyvinyl alcohol (PVA)-based resin film containing iodine.
[0025] The upper limit of the thickness of the polarizer is 10 μm in one embodiment, and 3 μm in another embodiment, and the lower limit of the thickness is 1 μm in one embodiment.
[0026] The iodine content of the polarizer can be appropriately set to take into account both sufficient polarization performance and optimal monomer transmittance. The iodine content is preferably 10% to 25% by weight, and more preferably 15% to 25% by weight. Despite having such an extremely high iodine content, the polarizer used in the embodiment of the present invention can achieve very excellent heat resistance that was previously difficult to achieve. In more detail, in a polarizer with an extremely high iodine content, changes in optical properties under high temperature environments can be significantly suppressed. In this specification, "iodine content" refers to the amount of total iodine contained in the polarizer (PVA-based resin film). More specifically, iodine in the polarizer is in the form of iodide ions (I - ), polyiodide ions (I3 - 、I5 - ) and other forms, the iodine content in this specification refers to the amount of iodine including all these forms. The iodine content can be calculated, for example, by the standard curve method of fluorescent X-ray analysis. It should be noted that the polyiodide ions exist in the polarizer in the form of PVA-iodine complex. By forming such a complex, absorption dichroism can be exhibited in the wavelength range of visible light. Specifically, the complex of PVA and triiodide ion (PVA·I3 - ) has an absorption peak near 470nm, and the complex of PVA and pentaiodide ion (PVA·I5 - ) has an absorption peak near 600nm. As a result, polyiodide ions can absorb light in a wide range of visible light depending on their form. On the other hand, iodide ions (I - ) has an absorption peak near 230nm and does not substantially participate in the absorption of visible light. Therefore, the polyiodide ions present in the form of a complex with PVA mainly interfere with the absorption performance of the polarizer.
[0027] The single transmittance (Ts) of the polarizer is preferably 30.0% to 43.0%, more preferably 35.0% to 41.0%. The polarization degree of the polarizer is preferably 99.9% or more, more preferably 99.95% or more, and further preferably 99.98% or more. By setting the single transmittance to be lower and increasing the polarization degree, the contrast can be improved, the black display can be made darker, and an image display device with excellent image quality can be achieved. It should be noted that the single transmittance is a value measured by a spectrophotometer with an integrating sphere. The single transmittance is the Y value obtained by measuring the 2-degree field of view (C light source) of JIS Z8701 and correcting the visual sensitivity. For example, it can be measured using a spectrophotometer with an integrating sphere (manufactured by JASCO Corporation, product name: V7100).
[0028] B-2. PVA resin film
[0029] As PVA resins for forming PVA resin films, for example, polyvinyl alcohol and ethylene-vinyl alcohol copolymers can be cited. Polyvinyl alcohol can be obtained by saponifying polyvinyl acetate. Ethylene-vinyl alcohol copolymers can be obtained by saponifying ethylene-vinyl acetate copolymers. The saponification degree of PVA resins is usually 85 mol% or more and less than 100 mol%, preferably 95.0 mol% to 99.95 mol%, and more preferably 99.0 mol% to 99.93 mol%. The saponification degree can be calculated based on JIS K6726-1994. By using a PVA resin with such a saponification degree, a polarizer with excellent durability can be obtained. When the saponification degree is too high, there is a concern that gelation will occur.
[0030] The thickness of the PVA-based resin film is not particularly limited and can be set according to the desired thickness of the polarizer. The thickness of the PVA-based resin film is, for example, 10 μm to 200 μm.
[0031] In one embodiment, the PVA-based resin film may be a PVA-based resin layer formed on a substrate. The laminate of the substrate and the PVA-based resin layer may be obtained, for example, by a method of applying a coating solution containing the above-mentioned PVA-based resin to a substrate or a method of laminating a PVA-based resin film on a substrate. As the substrate, any appropriate resin substrate may be used, for example, a thermoplastic resin substrate may be used.
[0032] B-3. Protective layer
[0033] As the protective layer, any appropriate resin film can be used. As the forming material of the resin film, for example, cellulose resins such as (meth) acrylic resins, cellulose diacetate, cellulose triacetate, cycloolefin resins such as norbornene resins, olefin resins such as polypropylene, ester resins such as polyethylene terephthalate resins, polyamide resins, polycarbonate resins, and copolymer resins thereof can be cited. It should be noted that "(meth) acrylic resin" refers to acrylic resin and / or methacrylic resin.
[0034] In one embodiment, as the (meth)acrylic resin, a (meth)acrylic resin having a glutarimide structure can be used. The (meth) acrylic resin having a glutarimide structure (hereinafter also referred to as glutarimide resin) is described in, for example, Japanese Patent Application Laid-Open Nos. 2006-309033, 2006-317560, 2006-328329, 2006-328334, 2006-337491, 2006-337492, 2006-337493, 2006-337569, 2007-009182, 2009-161744, and 2010-284840, and these descriptions are incorporated herein by reference.
[0035] When a polarizer is produced using a laminate of a substrate and a PVA-based resin layer, the substrate may be used directly as a protective layer without being peeled off. Alternatively, the substrate may be peeled off and a protective layer may be bonded to the polarizer.
[0036] The thickness of the protective layer is preferably 5 mm or less, more preferably 1 mm or less, further preferably 1 μm to 500 μm, and most preferably 5 μm to 150 μm. When surface treatment is performed, the thickness of the protective layer includes the thickness of the surface treatment layer.
[0037] The protective layer is bonded to the polarizer via any appropriate adhesive layer (adhesive layer, pressure-sensitive adhesive layer).
[0038] C. Surface protection film
[0039] As shown in the example, the surface protection film 10 is temporarily bonded to the polarizing plate 20 on the side opposite to the adhesive layer 30 in a releasable manner. More specifically, the surface protection film 10 includes a base film and an adhesive layer, and the surface protection film 10 and the polarizing plate 20 are bonded together via the adhesive layer.
[0040] C-1. Base film
[0041] The substrate film of the surface protection film can be made of any appropriate resin film. As the forming material of the resin film, ester resins such as polyethylene terephthalate resins, cycloolefin resins such as norbornene resins, olefin resins such as polypropylene, polyamide resins, polycarbonate resins, and their copolymer resins can be cited. Preferably, ester resins (particularly polyethylene terephthalate resins) are used. When such a material is used, there is an advantage that the elastic modulus is high enough and is not easily deformed even when tension is applied during transportation and / or lamination.
[0042] The thickness of the substrate film is preferably 38 μm or more, more preferably 48 μm or more. The upper limit of the thickness of the substrate film may be, for example, 128 μm. Such a thickness has the advantage that deformation is not easily caused even when tension is applied during transportation and / or lamination.
[0043] C-2. Adhesive layer
[0044] As the adhesive forming the adhesive layer in the above-mentioned surface protection film, any appropriate adhesive can be adopted. As the base resin of the adhesive, for example, acrylic resin, styrene resin, silicone resin can be cited. From the viewpoints of chemical resistance, adhesion for preventing the infiltration of the treatment liquid during immersion, and the degree of freedom to the adherend, acrylic resin is preferred. As the cross-linking agent that can be included in the adhesive, for example, isocyanate compounds, epoxy compounds, aziridine compounds can be cited. The adhesive can include a silane coupling agent, for example. The mixing prescription of the adhesive can be appropriately set according to the purpose.
[0045] The thickness of the pressure-sensitive adhesive layer is preferably 2 μm or more, more preferably 5 μm or more. The upper limit of the thickness is, for example, 40 μm.
[0046] C-3. Characteristics of surface protection film
[0047] The thickness of the surface protection film is 40 μm or more, preferably 50 μm or more. The upper limit of the thickness of the surface protection film can be, for example, 130 μm. It should be noted that the thickness of the surface protection film refers to the total thickness of the substrate film and the adhesive layer. By making the thickness of the surface protection film such a range, an optical laminate with excellent transportability can be obtained. If the thickness of the surface protection film is thinner than 40 μm, the transportability will become insufficient.
[0048] The peeling force of the surface protection film is 0.10N / 25mm to 0.50N / 25mm, preferably 0.10N / 25mm to 0.35N / 25mm. By making the peeling force of the surface protection film in such a range, an optical laminate having excellent peeling properties of the surface protection film and the separator can be obtained. If the peeling force of the surface protection film is less than 0.10N / 25mm, the surface protection film will float when the separator is peeled off. Furthermore, if it is greater than 0.50N / 25mm, delamination will occur when the surface protection film is peeled off.
[0049] The elastic modulus of the surface protection film is 2.00×10 9 Pa or more, preferably 2.50×10 9 Pa or more. The upper limit of the elastic modulus of the surface protection film may be 8.00×10 9 Pa. By setting the elastic modulus of the surface protection film to such a range, an optical laminate having excellent transportability can be obtained. 9 Pa, wrinkles and bends may occur in the film during transportation.
[0050] D. Adhesive layer
[0051] The adhesive layer 30 is typically made of an acrylic adhesive. As shown in the example in the figure, the adhesive layer 30 is formed on one surface of the polarizing plate 20 and is provided for the purpose of bonding the liquid crystal panel and the polarizing plate 20 together.
[0052] The thickness of the adhesive layer is preferably 100 μm or less, more preferably 50 μm or less, and further preferably 30 μm or less. The lower limit of the thickness may be, for example, 1 μm.
[0053] E. Isolate
[0054] As shown in the example of the figure, the separator 40 may be temporarily bonded to the side of the adhesive layer 30 opposite to the polarizing plate 20 in a releasable manner. The separator protects the adhesive layer until it is actually used and enables the polarizing plate to be rolled.
[0055] Examples of materials for forming the separator include ester resins such as polyethylene terephthalate resins, cycloolefin resins such as norbornene resins, olefin resins such as polypropylene, polyamide resins, polycarbonate resins, and copolymers thereof. Preferably, the resin is an ester resin (particularly polyethylene terephthalate resin).
[0056] The thickness of the separator is 35 μm to 80 μm, preferably 40 μm to 60 μm. By setting the thickness of the separator to such a range, an optical laminate having excellent transportability and excellent separator peelability can be obtained. If the thickness of the separator is thinner than 35 μm, the transportability becomes insufficient. Furthermore, if the thickness of the separator is thicker than 80 μm, poor pickup may occur when the separator is peeled off.
[0057] The peeling force of the separator is less than 0.28N / 25mm, preferably less than 0.10N / 25mm. By making the peeling force of the separator in such a range, an optical laminate having excellent peeling property of the separator can be obtained. If the peeling force of the separator is more than 0.28N / 25mm, it will cause poor pickup when the separator is peeled.
[0058] F. Method for producing an optical laminate
[0059] F-1. Polarizer
[0060] The manufacturing method of the polarizer of the embodiment of the present invention includes at least stretching and dyeing the PVA-based resin film. Typically, the manufacturing method includes a process of preparing the PVA-based resin film, a stretching process, a dyeing process, a cross-linking process, a cleaning process, and a drying process. In addition, a swelling process may be provided before the stretching process as needed. The various processes supplied to the PVA-based resin film can be performed in any appropriate order and timing. Therefore, the various processes can be performed in the above-mentioned order or in an order different from the above-mentioned order. As needed, one process can also be performed multiple times. Furthermore, processes other than the above (for example, an insolubilization process) can also be performed at any appropriate time. It should be noted that when the PVA-based resin film is a PVA-based resin layer formed on a substrate, the laminate of the substrate and the PVA-based resin layer is supplied to the above-mentioned process.
[0061] Each step will be described below. As described above, each step can be performed in any appropriate order and is not limited to the order described.
[0062] (Stretching process)
[0063] In the stretching process, the PVA resin film is typically uniaxially stretched to 3 to 7 times. The stretching direction can be the length direction of the film (MD direction) or the width direction of the film (TD direction). The stretching method can be dry stretching, wet stretching, or a combination thereof. In addition, the PVA resin film can also be stretched during a cross-linking process, a swelling process, a dyeing process, etc. It should be noted that the stretching direction can correspond to the absorption axis direction of the obtained polarizer.
[0064] (Swelling process)
[0065] The swelling process is usually carried out before the dyeing process. The swelling process is carried out, for example, by immersing the PVA-based resin film in a swelling bath. As the swelling bath, water such as distilled water and pure water is usually used. The swelling bath may also contain any other appropriate components other than water. As other components, solvents such as alcohols, additives such as surfactants, iodides, etc. may be mentioned. As iodides, for example, potassium iodide, lithium iodide, sodium iodide, zinc iodide, aluminum iodide, lead iodide, copper iodide, barium iodide, calcium iodide, tin iodide, and titanium iodide may be mentioned. Potassium iodide is preferably used. The temperature of the swelling bath is, for example, 20°C to 45°C. In addition, the immersion time is, for example, 10 seconds to 300 seconds.
[0066] (Dyeing process)
[0067] The dyeing step is a step of dyeing the PVA resin film with a dichroic substance. It is preferably carried out by adsorbing the dichroic substance. As the adsorption method, for example, there can be mentioned: a method of immersing the PVA resin film in a dyeing solution containing a dichroic substance, a method of applying the dyeing solution to the PVA resin film, and a method of spraying the dyeing solution on the PVA resin film. Preferably, the PVA resin film is immersed in the dyeing solution. This is because the dichroic substance can be well adsorbed.
[0068] As the above-mentioned dichroic substance, for example, iodine and dichroic dyes can be mentioned. Iodine is preferred. When iodine is used as the dichroic substance, an iodine aqueous solution is preferably used as the dyeing solution. The iodine content of the iodine aqueous solution is preferably 0.04 to 5.0 parts by weight relative to 100 parts by weight of water. In order to increase the solubility of iodine relative to water, iodide is preferably mixed in the iodine aqueous solution. As the iodide, potassium iodide is preferably used. The content of iodide is preferably 0.3 to 15 parts by weight relative to 100 parts by weight of water.
[0069] The liquid temperature of the dyeing liquid during dyeing can be set to any appropriate value, for example, 20° C. to 50° C. When the PVA-based resin film is immersed in the dyeing liquid, the immersion time is, for example, 5 seconds to 5 minutes.
[0070] (Cross-linking process)
[0071] In the cross-linking step, a boron compound is usually used as a cross-linking agent. Examples of the boron compound include boric acid and borax. Boric acid is preferred. In the cross-linking step, the boron compound is usually used in the form of an aqueous solution.
[0072] When using an aqueous boric acid solution, the boric acid concentration of the aqueous boric acid solution is, for example, 1 to 15% by weight, preferably 1 to 10% by weight. The aqueous boric acid solution may further contain an iodide such as potassium iodide, or a zinc compound such as zinc sulfate or zinc chloride.
[0073] The cross-linking step can be performed by any appropriate method. For example, the method of immersing the PVA-based resin film in an aqueous solution containing a boron compound, the method of applying the aqueous solution containing a boron compound to the PVA-based resin film, or the method of spraying the aqueous solution containing a boron compound onto the PVA-based resin film. Preferably, the film is immersed in an aqueous solution containing a boron compound.
[0074] The temperature of the solution used for cross-linking is, for example, 25° C. or higher, preferably 30° C. to 85° C., and more preferably 40° C. to 70° C. The immersion time is, for example, 5 seconds to 800 seconds, and preferably 8 seconds to 500 seconds.
[0075] (Cleaning process)
[0076] The washing step is typically performed after the cross-linking step. The washing step is typically performed by immersing the PVA-based resin film in a washing liquid. A representative example of the washing liquid is pure water. Potassium iodide may be added to the pure water.
[0077] The temperature of the cleaning liquid is, for example, 5° C. to 50° C. The immersion time is, for example, 1 second to 300 seconds.
[0078] (Drying process)
[0079] The drying process can be carried out by any appropriate method. As the drying method, for example, natural drying, air drying, reduced pressure drying, and heating drying can be cited. Preferably, heating drying is used. From the viewpoint of shortening the drying time, when heating drying is performed, the heating temperature is, for example, 30°C to 100°C. In another embodiment, it is preferably below 50°C, more preferably below 45°C, and further preferably below 40°C. The lower limit of the heating temperature is not particularly limited, and is the lower limit temperature that can be set in the heating drying device. For example, it is 30°C. By making the heating temperature of the drying process such a range, the free boric acid content of the polarizer can be adjusted to within a specified range. In addition, the drying time is, for example, 20 seconds to 10 minutes. In one embodiment, heating drying is performed in two or more stages. In this case, it is preferred that the heating temperature of at least any stage is a temperature within the above range. By setting the heating temperature to the above range when heating drying is performed, a polarizer with very excellent heat resistance can be obtained.
[0080] F-2.Polarizing plate
[0081] A resin film as a protective layer is bonded to the surface of the polarizer obtained in F-1 (the surface opposite to the resin substrate). Then, the resin substrate is peeled off to obtain a polarizing plate having a protective layer / polarizer structure. If necessary, a resin film as another protective layer can be bonded to the peeled surface.
[0082] F-3. Optical laminate
[0083] An adhesive layer is formed on the polarizer side of the polarizing plate obtained in F-2, and a separator is temporarily bonded to the surface of the adhesive layer in a removable manner. Furthermore, a surface protection film is temporarily bonded to the surface of the polarizing plate opposite to the adhesive layer in a removable manner, thereby obtaining an optical laminate 100.
[0084] Example
[0085] Hereinafter, the present invention will be specifically described by way of examples, but the present invention is not limited to these examples. It should be noted that the measuring methods of the various properties are as follows.
[0086] (1) Transportability
[0087] In the step of conveying the polarizing plate while bringing the surface of the polarizing plate into contact with the guide roller, it is visually checked whether the polarizing plate is bent, damaged, etc. The conveying speed is set to 5 m / min to 30 m / min.
[0088] ○: Can be transported without any problems.
[0089] △: The wire was caught in the roller during transportation, but no bending or damage occurred.
[0090] ×: The sheet was caught in the roller during transportation, causing bending, damage, etc.
[0091] (2) Evaluation of peeling of surface protection film
[0092] A starting tape (Cellotape (registered trademark) CT-24 manufactured by NICHIBAN CO., LTD.) was attached to a corner of the surface protection film, and the peeling state of the surface protection film was visually confirmed.
[0093] ○: The surface protection film can be peeled off without any problem.
[0094] △: There are few cases where the surface protection film does not follow the starting tape. The success rate is 80% to 100%.
[0095] ×: The surface protection film does not follow the starting tape. The success rate is 80% or less. Even if the surface protection film can be peeled off, the separator will float up and the polarizing plate will delaminate.
[0096] (3) Evaluation of the separation of the separator
[0097] A starting tape (Cellotape (registered trademark) CT-24 manufactured by NICHIBAN CO., LTD.) was attached to a corner of the separator, and the peeling state of the separator was visually confirmed.
[0098] ○: The separator can be peeled off without any problem.
[0099] △: There are few separator films that do not follow the starting tape. The success rate is 80% to 100%.
[0100] ×: The separator film does not follow the starting tape. The success rate is 80% or less. Or peeling occurs between the surface protection film and the polarizing plate.
[0101] (4) Peel strength of surface protection film
[0102] The optical laminate was cut into a size of 25 mm × 150 mm, and after the separator was peeled off, the adhesive layer was bonded to the glass in such a way that it was in contact with the glass. The stress (N / 25 mm) when the surface protection film was peeled off at a speed of 300 mm / min in the 90° direction was measured using an adhesive film peeling analyzer (manufactured by Kyowa Interface Science Co., Ltd., model: VPA-2). The measurement temperature was set to 25°C.
[0103] (5) Peel force of separator
[0104] The optical laminate was cut into a size of 25 mm × 150 mm and attached to a glass with double-sided tape (manufactured by Nitto Denko Corporation, No. 500) in such a way that the surface protection film surface was in contact with the double-sided tape. The stress (N / 25 mm) when the separator was peeled off at a speed of 300 mm / min in the 90° direction was measured using an adhesive film peeling analyzer (manufactured by Kyowa Interface Science Co., Ltd., model: VPA-2). The measurement temperature was set to 25°C.
[0105] [Example 1]
[0106] As a thermoplastic resin substrate, an amorphous isophthalic acid copolymer polyethylene terephthalate (IPA copolymer PET) film (thickness: 100 μm) with a water absorption of 0.75% and a Tg of 75° C. was used. One side of the substrate was subjected to a corona treatment, and an aqueous solution containing polyvinyl alcohol (polymerization degree 4200, saponification degree 99.2 mol%) and acetoacetyl-modified PVA (polymerization degree 1200, acetoacetyl modification degree 4.6%, saponification degree 99.0 mol% or more, manufactured by Nippon Synthetic Chemical Industry Co., Ltd., trade name "GOHSEFIMER Z200") in a ratio of 9:1 was applied to the corona-treated surface and dried to form a PVA-based resin layer with a thickness of 11 μm, thereby producing a laminate.
[0107] The obtained laminate was stretched in the air to 4.5 times in a direction perpendicular to the longitudinal direction of the laminate at 140° C. using a tenter stretching machine (stretching treatment).
[0108] Next, the laminate was immersed in a dyeing bath (an aqueous solution having an iodine concentration of 1.4% by weight and a potassium iodide concentration of 9.8% by weight) at a liquid temperature of 25° C. for 12 seconds to perform dyeing (dyeing treatment).
[0109] Next, the laminate was immersed in a cleaning bath (pure water) at a liquid temperature of 25° C. for 6 seconds (first cleaning treatment).
[0110] Next, the film was immersed in a cross-linking bath (an aqueous solution having a boron concentration of 1% by weight and a potassium iodide concentration of 1% by weight) at a liquid temperature of 60° C. for 16 seconds (cross-linking treatment).
[0111] Next, the laminate was immersed in a cleaning bath (aqueous solution having a potassium iodide concentration of 1% by weight) at a liquid temperature of 25° C. for 3 seconds (second cleaning treatment).
[0112] Next, the laminate was dried in an oven at 40° C. for 8 seconds (first drying treatment).
[0113] Finally, the laminate was dried in an oven at 40°C for 13 seconds (second drying process) to obtain a laminate (polarizing plate) having a PVA resin layer (polarizer) with a thickness of 1.2 μm. The iodine content of the obtained polarizer was 18.6% by weight and the single-body transmittance was 39.9%.
[0114] An adhesive layer is formed on the polarizer side surface of the polarizing plate obtained above, and a separator is temporarily bonded to the surface of the adhesive layer in a releasable manner. Furthermore, a surface protection film is temporarily bonded to the surface of the polarizing plate opposite to the adhesive layer in a releasable manner to obtain an optical laminate. The obtained optical laminate is subjected to the evaluations of (1) to (3) above. The results are shown in Table 1.
[0115] [Examples 2 to 12 and Comparative Examples 1 to 10]
[0116] An optical layered body was obtained in the same manner as in Example 1 except that the thickness, peeling force and elastic modulus of the surface protection film and the thickness and peeling force of the separator were changed as shown in Table 1. The obtained optical layered body was subjected to the same evaluation as in Example 1. The results are shown in Table 1.
[0117] [Table 1]
[0118]
[0119] As is clear from Table 1, the optical layered bodies of Examples (especially Example 1) of the present invention are excellent in conveyance properties and excellent in releasability of the surface protection film and the separator.
[0120] According to Comparative Example 1, when the thickness of the surface protection film is less than 40 μm, the transportability is insufficient. According to Comparative Examples 2 and 5, when the peeling force of the surface protection film exceeds 0.50 N / 25 mm, delamination occurs when the surface protection film is peeled off. According to Comparative Examples 3 and 4, when the peeling force of the surface protection film is less than 0.10 N / 25 mm, the surface protection film floats when the separator is peeled off. According to Comparative Example 9, the elastic modulus of the surface protection film is 2.00 × 10 9 Pa or less, wrinkles are generated during transport. Furthermore, according to Comparative Examples 6 and 7, when the thickness of the separator is less than 35 μm, the transportability becomes insufficient, and according to Comparative Example 10, when the thickness of the separator exceeds 80 μm, poor pickup occurs when the separator is peeled off. According to Comparative Example 8, when the peeling force of the separator exceeds 0.28 N / 25 mm, poor pickup occurs when the separator is peeled off.
[0121] Industrial Applicability
[0122] The optical layered body of the present invention can be suitably used in an image display device.
[0123] Description of Reference Numerals
[0124] 10 Surface protection film
[0125] 20 polarizing plate
[0126] 21 Protective layer
[0127] 22 polarizer
[0128] 30 Adhesive layer
[0129] 40 Isolate
[0130] 100 Optical laminate
Claims
1. An optical laminate, comprising: a polarizing plate; an adhesive layer provided on one side of the polarizing plate; a separator temporarily bonded to the side of the adhesive layer opposite to the polarizing plate in a releasable manner; and a surface protection film temporarily bonded to the side of the polarizing plate opposite to the adhesive layer in a releasable manner, The thickness of the polarizing plate is 60 μm or less. The thickness of the surface protection film is 40 μm to 87 μm. The peeling force of the surface protection film is 0.10N / 25mm~0.50N / 25mm. The elastic modulus of the surface protection film is 2.00×10 9 Pa~3.91×10 9 Pa, The thickness of the separator is 35 μm to 60 μm. The peeling force of the separator was 0.15 N / 25 mm or less.
2. The optical layered body according to claim 1, wherein: The separator has a peel force of less than 0.10 N / 25 mm.
3. The optical layered body according to claim 1 or 2, wherein: The polarizing plate includes a polarizer, and the polarizer is a polarizer having a thickness of 10 μm or less and made of a polyvinyl alcohol-based resin film containing iodine.
4. The optical laminate according to claim 3, wherein: The iodine content of the polarizer is 10 wt % to 25 wt %.