Refractory for continuous casting and refractory member
By adding free carbon components and forming a continuous void layer in the zirconia-carbonaceous refractory, optimizing the particle size composition and organizational structure, the corrosion resistance and heat resistance of the zirconia-carbonaceous refractory in components such as continuous casting nozzles are solved. It solves the problem of insufficient impact resistance and achieves high durability and low thermal expansion without preheating.
Patent Information
- Application Number
- CN202380024111.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-02
- Filing Date
- 2023-02-17
- Publication Date
- 2024-10-15
AI Technical Summary
Existing zirconia-carbon refractories have insufficient corrosion resistance and thermal shock resistance in components such as continuous casting nozzles, and perform poorly especially when used without preheating.
By optimizing the particle size composition and organizational structure of the refractory, increasing the free carbon component by 8-16%, ensuring the main body of the zirconia component, and forming a similar-shaped continuous void layer around the large particles, controlling the particle size distribution and void layer thickness, To improve the density and thermal expansion of refractory materials.
Significantly improves the corrosion resistance and thermal shock resistance of zirconia-carbon refractory, ensuring excellent durability even without preheating, reducing thermal expansion, and balancing strength and wear resistance.
Smart Images

Figure CN118786104A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a zirconia-carbonaceous (ZrO2-C) refractory for continuous casting and a refractory component such as a nozzle for continuous casting using the refractory. Background Art
[0002] Zirconia-carbon refractories, including zirconia-graphite, have superior corrosion resistance due to their main component, zirconia, compared to alumina and silica. Therefore, they are widely used in powder lines of immersion nozzles that require particularly high corrosion resistance (e.g., Patent Document 1).
[0003] As described in Patent Document 1, it is effective to reduce the amount of graphite and increase the amount of zirconium oxide to improve the corrosion resistance of zirconia-graphite refractory. However, if the amount of graphite is reduced, the problem of reduced thermal shock resistance occurs.
[0004] Patent Literature Patent Document 1: Japanese Patent Application Publication No. 2002-338347 Summary of the invention
[0005] In recent years, since continuous casting refractory parts such as continuous casting nozzles are increasingly used in a state of insufficient preheating or no preheating, it is desired to improve the thermal shock resistance as well as the corrosion resistance.
[0006] The technical problem to be solved by the present invention is to improve the corrosion resistance and thermal shock resistance of zirconia-carbon refractory and refractory parts for continuous casting.
[0007] The inventors found that controlling the pore morphology inside the refractory while achieving the densification of the refractory is the key when repeatedly testing and studying to improve the corrosion resistance and thermal shock resistance of zirconium oxide-carbonaceous refractory. Moreover, it was found that the particle size composition (volume ratio) of the refractory particles in the refractory is one of the important control factors, so that the present invention was completed.
[0008] That is, according to one aspect of the present invention, the following refractory for continuous casting can be provided. A refractory for continuous casting, comprising 8 mass % or more and 16 mass % or less of free carbon components, the main component of the remainder being a zirconium oxide component, and the total content of the free carbon component and other components other than the zirconium oxide component is less than 5 mass %, characterized in that: When the portion of the constituent consisting of the free carbon component is removed from the constituent of the refractory as 100% by volume, the refractory particles having a particle size exceeding 0.3 mm account for more than 5% by volume, and the refractory particles having a particle size of less than 0.045 mm account for more than 5% by volume and less than 40% by volume, Among the refractory particles in the refractory, at least around the coarse particles of the largest particle size, there is a substantially continuous void layer similar in shape to the coarse particles, and in the substantially continuous void layer, the total thickness of the void layer existing at the interface between the matrix structure containing carbon at both ends and the coarse particles is 0.3% or more and 3.0% or less relative to the particle size of the coarse particles, Furthermore, the apparent porosity is 16% or less, and the maximum thermal expansion coefficient up to 1500° C. is 0.6% or less.
[0009] According to another aspect of the present invention, there is provided a refractory component for continuous casting, wherein the refractory for continuous casting of the present invention is disposed partially or entirely on a portion in contact with molten steel.
[0010] According to the present invention, the corrosion resistance and thermal shock resistance of zirconia-carbon continuous casting refractory and refractory parts can be improved, thereby achieving excellent durability even in a use environment where the refractory is used without preheating. BRIEF DESCRIPTION OF THE DRAWINGS
[0011] Figure 1 Schematic diagrams showing the structure of refractory particles and their surroundings as aggregates in the refractory of the present invention, (a) is a case where there is a void layer with a shape similar to the particle outline around the refractory particles and the particles are approximately located in the center (a typical example of the present invention), and (b) is a case where there is a void layer with a shape similar to the particle outline around the refractory particles and the particles are located on either side of the inner wall surface of the void layer (an example of the distribution produced when preparing a sample for microscopic observation). Figure 2 This is a cross-sectional view showing an example of an immersion nozzle which is one aspect of a refractory component to which the refractory of the present invention is applied. Figure 3 This is a cross-sectional view showing another example of an immersion nozzle which is one aspect of a refractory component to which the refractory of the present invention is applied. Figure 4 This is an example of a continuous casting facility for steel and is an explanatory diagram showing an example of installation of refractory parts for continuous casting. Figure 5 This is a cross-sectional view showing an example of a long nozzle which is one form of a refractory component to which the refractory of the present invention is applied. Figure 6This is a cross-sectional view showing an example of a lower nozzle which is one aspect of a refractory component to which the refractory of the present invention is applied. Figure 7 This is a cross-sectional view showing another example of a long nozzle which is one aspect of a refractory component to which the refractory of the present invention is applied. Figure 8 This is a cross-sectional view showing an example of a long stopper rod which is one aspect of a refractory component to which the refractory of the present invention is applied. Explanation of symbols 20-Material for main body; 21-Refractory of the present invention; 22-Difficult-to-adhere material; 22G-Refractory for ventilation; 22S-Space (gas passage, pressure storage chamber); A-Upper nozzle; B-Sliding nozzle plate; C-Lower nozzle; D-Long nozzle; E-Long plug rod; F-Immersion nozzle; G-Refractory for lining. DETAILED DESCRIPTION
[0012] As mentioned above, in order to solve the above-mentioned problems, it is important to realize the densification of refractory and control the pore morphology inside refractory at the same time.Therefore, the present inventors take the following refractory organization as the target, that is, in the matrix organization (hereinafter referred to as "carbonaceous matrix") containing 3-dimensional continuous carbon, there are refractory particles with a particle size exceeding 0.3mm as aggregate in a discontinuous manner, and at the same time, among these refractory particles, there is a refractory organization of a roughly continuous void layer similar to the shape of the coarse particles at least around the coarse particles of the maximum particle size.That is, by adopting such a refractory organization, the thermal expansion of the coarse particles that have a greater contribution to the thermal expansion of the refractory can be absorbed by the roughly continuous void layer around the particles, and the result can obtain the effect of making the thermal expansion of the coarse particles disappear in appearance.That is, in the heating process, during the period when there is a void layer around the coarse particles, the thermal expansion amount of the refractory is mainly based on the thermal expansion amount of the 3-dimensional continuous carbonaceous matrix part, thereby reducing the thermal expansion of the refractory. And, in the present invention, by limiting the volume ratio of the refractory particles (hereinafter referred to as "coarse-grained refractory particles") with a particle size exceeding 0.3mm and the refractory particles (hereinafter referred to as "micro-particle refractory particles") with a particle size below 0.045mm, the densification of the refractory can be achieved, and the control of the pore morphology inside the refractory as described above can be achieved, thereby the improvement of the corrosion resistance and thermal shock resistance of the refractory and refractory parts used for continuous casting can be achieved. Specific description is given below.
[0013] The refractory of the present invention contains a free carbon component of more than 8% by mass and less than 16% by mass. Here, "free carbon component" refers to a carbon component consisting of a carbon component monomer other than compounds such as carbides such as B4C and SiC, except for inevitable impurities, and refers to amorphous or quasi-crystalline such as graphite generated by various organic binders, pitch, tar, and carbon black by being heated, and in addition, all carbon components present in the refractory organization in a particle shape (including fibrous shape) or a shape or structure that is present in the refractory organization in a continuous or discontinuous state without forming a specific shape. When the content of free carbon component is less than 8% by mass, 3-dimensional continuous carbonaceous matrix will not be formed in refractory structure, and enough low expansion effect cannot be obtained. In addition, when the content of free carbon component is less than 8% by mass, formability decreases, and the compactness of refractory is impaired, and its result can cause corrosion resistance to decrease. On the other hand, when it exceeds 16% by mass, the damage of carbonaceous matrix caused by molten steel, slag, etc. can become fierce, and the melting loss amount of refractory can be increased and corrosion resistance can be decreased. The content of preferably free carbon component is more than 10% by mass and less than 14% by mass.
[0014] In the refractory of the present invention, the main component of the remainder other than the free carbon component is a zirconium oxide component, and the content of other components other than the free carbon component and the zirconium oxide component (hereinafter referred to as "other components") is less than 5% by mass. That is, the refractory of the present invention includes a zirconium oxide component exceeding 79% by mass and below 92% by mass. In this way, since the refractory of the present invention includes at least 79% by mass of the zirconium oxide component, from the viewpoint of the basic composition, it also has higher corrosion resistance.
[0015] As mentioned above, the refractory of the present invention can include other components in the range of less than 5% by mass in total. Specifically, as other components, it can include one or more than two components selected from magnesium oxide components, silicon carbide components, boron carbide components and zirconium boride components. The magnesium oxide component reacts with the free carbon components in the refractory during heating, and the reaction product can inhibit the invasion of molten steel into the refractory, which can improve the corrosion resistance. In addition, silicon carbide components, boron carbide components and zirconium boride components can inhibit the oxidation of the free carbon components in the refractory. In order to obtain these effects, as other components, the refractory of the present invention can include one or more than two components selected from magnesium oxide components, silicon carbide components, boron carbide components and zirconium boride components in the range of less than 5% by mass in total. Because when the content of these other components is more than 5% by mass, the content of zirconium oxide components will be relatively reduced, so sufficient corrosion resistance will not be obtained.
[0016] Here, the zirconium oxide raw material as the zirconium oxide component source contains stabilizing components such as CaO, MgO, and Y2O3, but in the refractory of the present invention, the content of the zirconium oxide component also contains the content of stabilizing components such as CaO, MgO, and Y2O3. In other words, the content of stabilizing components such as CaO, MgO, and Y2O3 contained in the zirconium oxide raw material is not included in the content of the above-mentioned other components.
[0017] In the refractory of the present invention, the content of each of the above-mentioned components can be basically determined by ICP emission spectrometry. In addition, although it is impossible to distinguish between the stabilizing components such as CaO, MgO, and Y2O3 contained in the zirconium oxide raw material and the above-mentioned other components in the ICP emission spectrometry, since the content of the stabilizing components such as CaO, MgO, and Y2O3 contained in the zirconium oxide raw material can be determined in advance, the content of the other components can be determined by subtracting the content of the stabilizing components such as CaO, MgO, and Y2O3 contained in the zirconium oxide raw material from the value determined by the ICP emission spectrometry.
[0018] Next, one of the characteristics of the present invention, that is, the particle size composition (volume ratio) of the refractory particles in the refractory will be described. In the present invention, the particle size composition (volume ratio) of the refractory particles in the refractory is characterized in that, when the portion of the constituent composed of free carbon components is removed from the constituent of the refractory as 100 volume %, the coarse-grained refractory particles are more than 5 volume %, and the fine-grained refractory particles are more than 5 volume % and less than 40 volume %. Since when the coarse refractory particles are less than 5% by volume, the volume ratio of the refractory particles of the microparticles or the medium particles described later will increase relatively, so the number of refractory particles in the refractory will increase. As a result, the refractory structure in which the refractory particles are continuously present will become high expansion. Therefore, the thermal shock resistance will decrease. Although the upper limit of the volume ratio of the coarse refractory particles is not particularly limited, from the viewpoint of stably ensuring the necessary characteristics such as the strength and corrosion resistance required as the refractory for continuous casting, for example, it can be less than 60% by volume. The volume ratio of the coarse refractory particles is preferably more than 10% by volume, more preferably less than 60% by volume. In addition, although the upper limit of the particle size of the coarse refractory particles is not particularly limited, from the viewpoint of stably ensuring the necessary characteristics such as the strength and corrosion resistance required as the refractory for continuous casting, it is preferably less than 3mm, more preferably less than 1mm. That is, as coarse-grained refractory particles, in addition to particle sizes exceeding 0.3 mm and being less than 1 mm, the refractory of the present invention may also include particle sizes exceeding 1 mm and being less than 3 mm, but the volume proportion of the particle sizes exceeding 1 mm and being less than 3 mm is preferably 15 volume % or less, when the portion other than the constituent material consisting of free carbon components removed from the constituent material of the refractory is taken as 100 volume %, and more preferably 0 volume %, i.e., refractory particles having a particle size exceeding 1 mm and being less than 3 mm are not included.
[0019] In addition, when the volume ratio of the refractory particles of the microparticles is less than 5 volume %, it is impossible to obtain enough corrosion resistance. On the other hand, because when the volume ratio of the refractory particles of the microparticles exceeds 40 volume %, the number of the refractory particles in the refractory will increase, so the refractory structure in which the refractory particles are continuously present will become high expansion. Therefore, thermal shock resistance will decline. In addition, when the volume ratio of the refractory particles of the microparticles exceeds 40 volume %, the formability will decline, and the compactness of the refractory will be impaired, and the result will cause the corrosion resistance to decline. The volume ratio of the refractory particles of the preferred microparticles is more than 10 volume % and less than 30 volume %. In addition, in the refractory of the present invention, the refractory particles of the microparticles are basically present in the carbonaceous matrix.
[0020] Above, although the volume ratio of the refractory particles of coarse grain (particle diameter exceeds 0.3mm) and microparticle (particle diameter 0.045mm or less) is described, refractory of the present invention suitably comprises the refractory particles of medium grain (particle diameter exceeds 0.045mm and is 0.3mm or less).Its volume ratio is, when the part of the constituent consisting of free carbon component is removed from the constituent of refractory as 100% by volume, the remainder of the volume ratio of the refractory particles of coarse grain and the volume ratio of the refractory particles of microparticle, specifically, is preferably below 90% by volume, more preferably above 25% by volume and below 85% by volume.
[0021] Here, in the present invention, the particle size of refractory particles refers to the size of the mesh when the refractory particles are screened with a sieve. For example, refractory particles with a particle size of less than 0.045 mm refer to refractory particles that pass through a sieve with a mesh of 0.045 mm, and refractory particles with a particle size exceeding 0.3 mm refer to refractory particles that do not pass through a sieve with a mesh of 0.3 mm.
[0022] Next, the organization of the refractory of the present invention is described in detail. As described above, the basic organizational form of the refractory of the present invention is the following refractory organization, in a 3-dimensional continuous carbonaceous matrix, there are refractory particles with a particle size of more than 0.3mm as aggregates in a discontinuous manner, and at the same time, among these refractory particles, there is a refractory organization of a roughly continuous void layer similar to the shape of the coarse particles at least around the coarse particles of the maximum particle size. Specifically, in the roughly continuous void layer, the total thickness of the void layer on the interface between the carbonaceous matrix at both ends and the coarse particles is, relative to the particle size of the coarse particles, a refractory organization of more than 0.3% and less than 3.0%.
[0023] Here, the term "substantially continuous void layer" means that, under cross-sectional observation of a microscope around the refractory particles as aggregate, the voids have an enlarged shape that is substantially similar to the shape of the particle cross-sectional shape, and the particles are present inside the voids like a bell ball (see Figure 1 (a)). That is, there is no structure in which a structure such as carbon that hinders the thermal expansion of the refractory particles exists in the void layer, and the void layer is not uniform or does not have voids, and there are random portions where the refractory particles are in direct contact with each other or the refractory particles and the carbonaceous matrix. In addition, in the refractory of the present invention, a void layer exists in the whole surrounding of the refractory particles as aggregate, that is, in a "continuous state", but when the void layer is verified by microscopic observation, it can be said that the refractory particles exist in a floating manner without being fixed in the space, so when the sample is made from the refractory, a part of the surface of the refractory particles may also be generated that is in contact with other refractory particles and the carbonaceous matrix around them (refer to Figure 1 (b)). Therefore, considering the actual situation in the verification, the expression "substantially continuous" is used. In fact, although there is a void layer around the refractory particles as a whole, for example, when verifying the sample under microscope observation, even if there is a part that contacts other refractory particles or carbonaceous matrix, the part is not in a state of "bonding or bonding" to the extent that the refractory particles are fixed. That is, through such a "substantially continuous void layer", the thermal expansion of the refractory particles can be absorbed, thereby achieving low expansion of the refractory.
[0024] From the viewpoint of reducing the thermal expansion of refractory, the thickness of the interstitial layer around the refractory particles is as thick as possible, and preferably there is the interstitial layer around all refractory particles as aggregate. However, since the interstitial layer around the refractory particles can become the reason for the strength reduction of the refractory, it is necessary to obtain the balance of thermal expansion and strength, damage, etc. while adjusting the thickness of the interstitial layer.
[0025] The ratio of the void layer thickness to the particle size (void layer thickness rate of each particle: MS value (micro space value)) is that the larger the particle, the smaller its ratio is, and the smaller the particle, the larger its ratio is. Therefore, the MS value of the coarse particle with the maximum particle size among the specific refractory particles refers to the lower limit value of the void layer thickness rate of each particle in the refractory structure being specified, and the heat shock resistance of the general refractory can be evaluated.
[0026] Here, the MS value refers to the ratio of the thickness L of the void layer between the coarse particle and the carbonaceous matrix (the total thickness of the void layer on both sides of the particle is taken as L) to the coarse particle diameter D, and can be obtained by the following formula. MS value = (L / D) × 100 (%)
[0027] Specifically, in the present invention, the MS value (%) is calculated by the following method. In the microscopic organization observation of refractory, 10 coarse particles are selected in the order of the size of the particle diameter, and in the face of each particle, the largest circle that contacts with its outline and is enclosed is outlined, and an arbitrary line through the center is drawn. And, based on this line, 3 lines of 45 ° spacing through the center of the above-mentioned circle are drawn again, and a total of 4 lines are drawn for each particle. Thereafter, on the above-mentioned lines of the particle, the length between the contour points at the two ends of the particle is used as D1, D2, D3, D4, and the total of the interstitial layer thickness of the particle interface present on each line at both ends is measured as L1, L2, L3, L4 respectively. Use the numerical value obtained by these 4 lines, calculate MS1, MS2, MS3, MS4 calculated by the above formula respectively, and calculate the average value of these numerical values as the interstitial layer thickness rate of 1 coarse particle, i.e., MS value. Utilize the above-mentioned method to calculate the MS values of 10 coarse particles selected in advance respectively, and average them as the MS value of this refractory organization.
[0028] In addition, the reason for evaluating the MS value of the refractory structure by using the coarse particles of the maximum particle size, i.e., 10 coarse particles selected in the order of the size of the particle size in the microscopic organization observation of the refractory, is that the larger the particle size, the greater the change in volume and length caused by its expansion, and the greater the impact on the thermal shock resistance of the refractory. Therefore, as an index for adjusting and evaluating the MS value of thermal shock resistance, it is necessary to calculate the coarse particles of the maximum particle size in the refractory structure. In addition, from the same viewpoint, in the present invention, the above-mentioned "roughly continuous void layer" needs to be present at least around the coarse particles of the maximum particle size, i.e., 10 coarse particles selected in the order of large to small particle size in the microscopic organization observation of the refractory.
[0029] The inventors have confirmed that, in a refractory containing a free carbon component of more than 8% by mass and less than 16% by mass, the main component of the remainder is a zirconium oxide component, there is a low expansion effect, and the thickness of the void layer around the refractory particles that can be balanced in terms of strength, corrosion resistance and wear resistance is, based on the MS value calculated for the coarse particles of the maximum particle size, more than 0.3% and less than 3.0%. That is, when the above-mentioned MS value is less than 0.3%, sufficient low expansion effect cannot be obtained. In addition, when the above-mentioned MS value exceeds 3.0%, the strength decreases, and the corrosion resistance and wear resistance also decrease. Thus, in the present invention, by forming the following refractory structure, that is, among the refractory particles in the refractory, there is a roughly continuous void layer similar to the shape of the coarse particles at least around the coarse particles of the maximum particle size, and in the roughly continuous void layer, the total thickness of the void layer on the interface between the carbon-containing matrix structure at both ends and the coarse particles is a refractory structure of not less than 0.3% and not more than 3.0% relative to the particle size of the coarse particles, thereby being able to provide a refractory that can significantly improve thermal shock resistance and achieve a balance in strength, corrosion resistance and wear resistance.
[0030] The MS value control method is to form a substantially continuous void layer having a shape similar to that of at least the largest coarse particles among the refractory particles in the refractory and to control the thickness of the void layer, for example, as follows. Although the control of MS value is synonymous with the control of thermal expansion coefficient, due to the fact that in the process of heat treatment, the larger the refractory particles (coarse particles), the larger the thermal expansion amount, and the more significant the thermal expansion difference with the carbonaceous matrix, the more easily a substantially continuous void layer (hereinafter also referred to as "MS") similar to its shape is generated around the coarse particles, and the smaller the refractory particles, the smaller the thermal expansion amount becomes, and it is difficult to generate a clear MS. Therefore, by controlling the particle size composition (volume ratio) of the refractory particles in the refractory, it is possible to achieve the control of MS value, that is, the control of thermal expansion coefficient. In the present invention, when the part of the constituent composed of free carbon components is removed as 100% by volume, by making the refractory particles with a particle size exceeding 0.3mm be more than 5% by volume, making the refractory particles with a particle size of less than 0.045mm be more than 5% by volume and less than 40% by volume, it is possible to achieve low expansion and its control. For example, when lower expansion is desired, the generation of MS can be promoted by reducing the volume ratio of refractory particles with a particle size of less than 0.045 mm within the above-mentioned particle size composition (volume ratio) to cut off the continuity of the refractory particles in the refractory structure, and increasing the volume ratio of refractory particles with a particle size exceeding 0.3 mm.
[0031] By combining the above-mentioned constitution (chemical composition, granularity constitution (volume ratio) of refractory particles and refractory organization), the refractory of the present invention can stably coexist with a compactness of an apparent porosity of less than 16% and a low expansion property of less than 0.6% of the maximum thermal expansion coefficient up to 1500°C. Thus, the corrosion resistance and thermal shock resistance of the refractory and refractory parts for continuous casting can be improved, and excellent durability can be exerted even in an environment of use in which the refractory and refractory parts are used without preheating.
[0032] Here, in the present invention, the chemical composition, refractory structure, apparent porosity, thermal expansion coefficient, etc. of the refractory are basically evaluated for the sample "after heating in a non-oxidizing atmosphere at 1000°C". The reason is to achieve the removal of components such as moisture, organic matter, water and matter, carbon oxides, etc. in the refractory, and to stabilize the chemical composition of the refractory by carbonization of the organic binder component to improve the analysis accuracy. From this point of view, the heating time is set to the period until the weight change caused by heating disappears. However, when the refractory has been heat-treated at a temperature above 1000°C in the manufacturing process, or when it has been heat-treated at a temperature above 800°C according to the type of volatile components, the chemical composition, refractory structure, apparent porosity, thermal expansion coefficient, etc. can be evaluated in the product state after its production.
[0033] In addition, the refractory of the present invention can also include carbon fiber in the carbonaceous matrix. Carbon fiber can fill the defective parts such as cracks produced by the shrinkage of the carbonaceous matrix, and the shrinkage of the carbonaceous matrix is caused by the carbonization of the organic binder component during the heating of the refractory. Thus, the densification and strengthening of the carbonaceous matrix can be achieved, and the strength of the refractory is improved. From the viewpoint of giving full play to the strength improvement effect of this refractory, the aspect ratio of the preferred carbon fiber is more than 15 and less than 200, and preferably its content is less than 5% by mass.
[0034] Similar to the preparation of samples in Examples described below, the refractory of the present invention can be prepared by the same method as the method for preparing a general zirconia-carbonaceous refractory. For example, a binder is added to a raw material mixture including zirconium oxide raw material, graphite, etc., and the kneaded clay is adjusted to a state suitable for forming. The clay is then formed using CIP (Cold Isostatic Pressing), dried at a temperature below about 300°C, and then heat treated in a non-oxidizing atmosphere at about 800°C to about 1200°C.
[0035] Next, a refractory component for continuous casting using the refractory of the present invention will be described. Figure 2 In FIG. 1 , a submerged nozzle, which is one form of a refractory component for continuous casting, is shown in longitudinal section. exist Figure 2 In (a), an example of applying the refractory material 21 of the present invention to an immersion nozzle of a powder line is shown. Figure 2 (a) shows an example of a cylindrical shape, but the nozzle such as the immersion nozzle of the refractory material to which the present invention is applied is not limited to such a cylindrical shape, for example, Figure 2 The shapes of the nozzles shown in (b) are flat, elliptical, funnel-shaped (funnel-shaped with a larger diameter at the top) and other shapes, which are mainly used for casting thin plates, and can be applied to nozzles of various shapes. In addition, Figure 2 (c) shows that there is Figure 2 (a) is an example of an immersion nozzle having the function of blowing gas into molten steel from a part of the inner hole portion (inner hole wall surface) of the immersion nozzle. In this example, a highly permeable refractory (hereinafter referred to as "ventilation refractory") 20G is arranged on a part of the inner hole portion. The material of the ventilation refractory 20G can be a general alumina-graphite ventilation refractory. In addition, it can also be a material that can improve the porosity and permeability while maintaining the refractory composition of the present invention. In addition, Figure 2 The symbol 20S in (c) is a space, which is the passage of gas and also the gas pressure storage chamber. Figure 2 The symbol 20 in the figure is the material for the main body. Figure 3 and Figures 5 to 8 The same is true in Chinese.
[0036] exist Figure 3 In the figure, there is shown an example of an immersion nozzle in which a refractory 21 of the present invention is arranged on a part or the whole of the part in contact with molten steel, and a layer composed of a refractory (difficult to adhere material 22) composed of a composition different from the refractory 21 of the present invention is arranged inside the refractory 21, thereby forming a plurality of layers, and the plurality of layers form an integral structure in a state of direct contact with each other. In the production of such a nozzle composed of multiple layers, it is only necessary to separate a gap for clay injection at a position of a specified thickness in the radial direction from the surface in contact with molten steel in the target area in the CIP forming mold based on the above-mentioned production method, fill the inside (core rod side) with clay for refractory different from the refractory of the present invention, and fill the back side with clay for refractory of the present invention. Thereafter, before forming, it is only necessary to remove the clamp such as the plate used for separation and perform press forming.
[0037] Examples of nozzles for continuous casting of refractory materials to which the present invention can be applied or suitably include, in addition to immersion nozzles, pouring nozzles (including upper nozzles, open nozzles, etc.), intermediate nozzles, and flow rate control nozzles (especially inner holes, etc.). exist Figure 4 In the figure, there is shown an example of the structure of a continuous casting device for steel, and on the left side of the same figure, there is shown an example in which a nozzle portion serving as a flow path for molten steel when discharging molten steel from a molten steel container is a structure composed of a plurality of nozzles, and in the structure, an immersion nozzle F is an externally mounted example. The refractory material 21 of the present invention can be applied not only to the immersion nozzle F, but also to a part or the whole of the portion in contact with molten steel of various nozzles such as an upper nozzle A, a sliding nozzle plate B, a lower nozzle C, and a long nozzle D of such a structure composed of a plurality of nozzles for continuous casting. In addition, it can also be applied to a so-called inserted immersion nozzle ( Figure 4 The right side of the nozzle is not immersed in the molten steel, and the so-called open nozzle is not immersed in the molten steel. In addition, it can also be used as a stopper rod E located above the nozzle part to control the flow rate of the molten steel or open and close it, or a refractory G for lining the molten steel container.
[0038] exist Figure 5 and Figure 6 In FIG. 1 , there is shown an example in which a long nozzle and a lower nozzle are provided with a refractory material 21 of the present invention on a part or the whole of the part in contact with molten steel. Figure 5 and Figure 6 In the embodiment, either or both of the inner refractory layer and the back side refractory layer may be the refractory 21 of the present invention. In addition, Figure 7In the example of a long nozzle for forming a powder line using the refractory material 21 of the present invention, is shown. Figure 7 In the embodiment, if the refractory 21 of the present invention is also arranged on the part other than the powder line, it can be an immersion nozzle in which the refractory of the present invention is arranged as a single layer in the entire area of the part in contact with the molten steel, from the surface in contact with the molten steel to the back side. In the case of a nozzle with a single-layer structure, the danger of fracturing, etc. can be reduced, and a simple method can also be used in the production. In the production of such a nozzle with a single-layer structure, it is only necessary to fill the refractory of the present invention with clay as a single layer in the target area in the CIP forming mold based on the above-mentioned production method.
[0039] exist Figure 8 , there is shown an example of a long stopper rod in which the refractory material 21 of the present invention is arranged on a part or the whole of the part in contact with the molten steel. Figure 8 In the embodiment, either or both of the tip end portion and the base end portion other than the tip end portion of the long stopper rod may be the refractory 21 of the present invention. Example
[0040] The raw material coordination and evaluation result of the embodiment of the present invention and comparative example are shown in the following table 1~table 6. In addition, in each table, "the volume ratio of refractory particles" is the volume ratio calculated based on the raw material coordination, but also maintains this volume ratio in the refractory of making. That is, the "volume ratio of refractory particles" represented in each table is identical with the volume ratio of the refractory particles of each particle size when the part of the constituent consisting of the free carbon component is removed from the constituent of the refractory as 100% by volume.
[0041] An organic binder, namely a phenolic resin, is added to the raw material mix of each example shown in each table, and the kneaded clay is adjusted to a state suitable for forming. After the clay is formed by CIP, it is cured and dried at 300°C, and then heat-treated at 1000°C in a non-oxidizing atmosphere to obtain a refractory of each example.
[0042] The chemical composition of the obtained refractory was analyzed, the structural state was observed, and the refractory was subjected to evaluation tests. The chemical composition analysis was carried out according to the method of Japanese Industrial Standard JIS R2216. In the observation of the structural state, after the resin was impregnated into the refractory structure, a mirror surface was polished by mechanical grinding, and the MS value was obtained by the above-mentioned method under microscope observation, and the continuity of the void layer was observed. As evaluations of the refractory, the apparent porosity, the maximum thermal expansion coefficient up to 1500° C., the corrosion resistance, and the thermal shock resistance were evaluated, and a comprehensive evaluation was performed based on these evaluation results.
[0043] The apparent porosity is measured according to the method of Japanese Industrial Standard JIS R2205. The thermal expansion coefficient was measured up to 1500°C according to the method of Japanese Industrial Standard JIS R2207-3, and the maximum thermal expansion coefficient up to 1500°C was evaluated.
[0044] The corrosion resistance is evaluated by immersing the prism sample (20×20×180mm) of the refractory of each example in a crucible in which about 30mm of synthetic slag with a CaO / SiO2 mass ratio adjusted to 1.0 floats on the surface of low-carbon steel melted at 1550°C for 60 minutes. After being lifted up, the melting loss at the interface of the molten steel-molten slag is measured, and the degree is compared. Specifically, the melting loss of the refractory of each example is converted into a melting loss index with the melting loss of Comparative Example 1 as 100, and the situation where the melting loss index is less than 100 is recognized as the effect of solving the problem. More specifically, the situation where the melting loss index is less than 94 is evaluated as 0 (excellent), the situation where it exceeds 94 and is less than 100 is evaluated as △ (good), and the situation where it is more than 100 is evaluated as × (poor).
[0045] The evaluation of heat shock resistance is carried out by injecting molten iron at 1600°C into the inner hole of the sample at room temperature using a cylindrical sample (outer diameter / inner diameter (inner bore diameter) / height = 130 / 55 / 300mm), and applying heat shock to the refractory of the sample. After the test, the horizontal section is cut at 50mm intervals and checked for cracks. Then, the situation where no cracks are observed is evaluated as ○ (excellent), the situation where microcracks are confirmed is evaluated as △ (good), and the situation where cracks are confirmed is evaluated as × (poor).
[0046] The comprehensive evaluation was that the case where the MS value in the organizational state was within the range of the present invention (0.3% to 3.0%), the continuity of the void layer was approximately continuous, the apparent porosity was within the range of the present invention (16% to 1500°C), and the maximum thermal expansion coefficient to 1500°C was within the range of the present invention (0.6% to 0), the corrosion resistance was evaluated as 0, and the thermal shock resistance was evaluated as 0 was evaluated as ○ (excellent). The case where the MS value in the organizational state was within the range of the present invention (0.3% to 3.0%), the continuity of the void layer was approximately continuous, the apparent porosity was within the range of the present invention (16% to 1500°C), and the maximum thermal expansion coefficient to 1500°C was within the range of the present invention (0.6% to 0), and either the corrosion resistance or the thermal shock resistance was evaluated as △ was evaluated as △ (good). The case where the continuity of the void layer in the organizational state was partially continuous, the apparent porosity exceeded 16%, the maximum thermal expansion coefficient to 1500°C exceeded 0.6%, and the corrosion resistance was evaluated as × or the thermal shock resistance was evaluated as × was evaluated as × (poor).
[0047] (Table 1)
[0048] In Table 1, Examples 1 to 5 are examples in which the content of the free carbon component (hereinafter referred to as "FC") in the refractory is different, but within the scope of the present invention, the apparent porosity is low and the corrosion resistance is also excellent, and the thermal shock resistance is also excellent, and the comprehensive evaluation is ○ (excellent) or △ (good), and good results can be obtained. Among them, the comprehensive evaluation of Examples 2 to 4 in which the content of FC is within the preferred range of 10 mass % or more and 14 mass % or less is ○ (excellent), and particularly good results can be obtained. In contrast, Comparative Example 1 is an example in which the FC content is lower than the lower limit of the present invention, and a three-dimensional continuous carbonaceous matrix is not formed in the refractory structure, and the continuity of the void layer around the coarse particles is damaged and becomes "partially continuous". Therefore, a sufficient low expansion effect is not obtained, and high expansion is obtained, and the thermal shock resistance decreases. In addition, due to the problem of formability, a dense refractory cannot be obtained, and the corrosion resistance also decreases. On the other hand, Comparative Example 2 is an example in which the FC content exceeds the upper limit of the present invention, and the corrosion resistance decreases.
[0049] (Table 2)
[0050] In Table 2, embodiment 6, embodiment 3 and embodiment 7 to embodiment 9 are different examples of the volume ratio of coarse-grained refractory particles, but within the scope of the present invention, comprehensive evaluation is ○ (excellent) or △ (good), and good results can be obtained. In addition, embodiment 6 is an example that the volume ratio of coarse-grained refractory particles is the lower limit of the present invention, i.e., 5 volume %, if compared with other embodiments of more than 10 volume % with the volume ratio of coarse-grained refractory particles, it becomes high expansion, resulting in a variation in thermal shock resistance. In addition, embodiment 6 is compared with other embodiments, and apparent porosity also increases, resulting in a variation in corrosion resistance. On the other hand, Comparative Example 3 is an example in which the volume ratio of coarse-grained refractory particles is lower than the lower limit of the present invention, and as a result, the number of refractory particles in the refractory increases, becoming a refractory structure in which refractory particles continuously exist, and becoming a refractory structure in which the continuity of the void layer is "roughly continuous" but the MS value is lower than the lower limit of the present invention. Therefore, it becomes high expansion, and thermal shock resistance decreases.
[0051] (Table 3)
[0052] In Table 3, embodiment 10, embodiment 11, embodiment 3, embodiment 12 to embodiment 14 are different examples of the volume ratio of the refractory particles of microparticles, but within the scope of the present invention, the comprehensive evaluation is ○ (excellent) or △ (good), and good results can be obtained. Wherein, the comprehensive evaluation of embodiment 11, embodiment 3, embodiment 12 and embodiment 13 in the preferred range of more than 10 mass % and less than 30 mass % of the volume ratio of the refractory particles of microparticles is ○ (excellent), and particularly good results can be obtained. On the contrary, Comparative Example 4 is an example in which the volume ratio of the refractory particles of microparticles is lower than the lower limit of the present invention, and the corrosion resistance decreases. On the other hand, Comparative Example 5 is an example in which the volume ratio of the refractory particles of microparticles exceeds the upper limit of the present invention, and the number of the refractory particles in the refractory increases as a result, and becomes a refractory structure in which the refractory particles continuously exist, and becomes a refractory structure in which the continuity of the void layer is "roughly continuous" but the MS value is lower than the lower limit of the present invention. Therefore, it becomes high expansion, and the thermal shock resistance decreases. In addition, due to the problem of formability, it is impossible to obtain a dense refractory, and the corrosion resistance also decreases.
[0053] (Table 4)
[0054] In Table 4, Examples 3 and 15 to 18 are examples in which the types of zirconium oxide raw materials are different. The zirconium oxide raw materials used in each example are as follows. Example 3: 4 mass % CaO partially stabilized zirconia (the same applies to the examples in Tables 1 to 3, and Tables 5 and 6 described later) Example 15: 6 mass% CaO partially stabilized zirconia Example 16: 6 mass% MgO partially stabilized zirconia Example 17: 8 mass% Y2O3 partially stabilized zirconia Example 18: 100 mass% of the zirconium oxide raw material contains 90 mass% of 4 mass% CaO partially stabilized zirconium oxide and 10 mass% of unstabilized zirconium oxide. As described above, in the refractory of the present invention, the content of the zirconium oxide component also includes the content of stabilizing components such as CaO, MgO, and Y2O3. In each table, the content of the stabilizing component is added to the zirconium oxide component (ZrO2). Embodiment 3 and Embodiment 15 to Embodiment 18 are all within the scope of the present invention, and the comprehensive evaluation is ○ (excellent) or △ (good), and good results can be obtained. In addition, although Examples 15 and 16 contain CaO and MgO in the zirconium oxide component (ZrO2), the amount of ZrO2 is reduced after CaO and MgO are removed, so the corrosion resistance is △ (good). Since Y2O3 in Example 17 has high corrosion resistance, the corrosion resistance is 0 (excellent).
[0055] (Table 5)
[0056] Each embodiment shown in Table 5 is an example containing carbon fiber, but within the scope of the present invention, the comprehensive evaluation is ○ (excellent) or △ (good), and good results can be obtained. Among them, the comprehensive evaluation of Example 19 in which the aspect ratio of the carbon fiber is 15 to 200 and the content of the carbon fiber is limited to 5% by mass or less is ○ (excellent), and particularly good results can be obtained.
[0057] (Table 6)
[0058] In Table 6, Examples 21 to 23 are examples containing "other components", but the content (total) thereof is less than 5% by mass, which is within the range of the present invention, and good results can be obtained. On the contrary, the content (total) of other components of Comparative Examples 6 to Comparative Examples 12 is more than 5% by mass, and the corrosion resistance decreases. In addition, in Comparative Example 8 comprising more than 5% by mass of B4C components as other components, since more B2O3 components (liquid phase components) are generated from B4C components during the heating process, the liquid phase components will invade the void layer around the refractory particles, and therefore the continuity of the void layer will be damaged and become "partially continuous". Therefore, it will become high expansion, and the thermal shock resistance will decrease. In addition, in Comparative Example 11 comprising more than 5% by mass of B4C components and MgO components as other components, since liquid phase components will also be generated during the heating process, and the liquid phase components will invade the void layer around the refractory particles, the continuity of the void layer will be damaged and become "partially continuous". Therefore, it will become high expansion, and the thermal shock resistance will decrease. In Comparative Example 12, the sintering of the entire structure is promoted by the reaction of the B2O3 component generated from the ZrB2 component and the MgO component, so that the elastic modulus increases and the thermal shock resistance decreases. In Table 6, "additive" refers to a boron component source, and the amount added is indicated as the amount added as an external addition relative to 100% by mass of the raw materials other than the "additive".
Claims
1. A refractory for continuous casting, comprising 8 mass % or more and 16 mass % or less of free carbon, the remainder of which is mainly composed of zirconium oxide, and the total content of the free carbon and other components other than the zirconium oxide is less than 5 mass %, characterized in that: When the portion of the constituent consisting of the free carbon component is removed from the constituent of the refractory as 100% by volume, the refractory particles having a particle size exceeding 0.3 mm account for more than 5% by volume, and the refractory particles having a particle size of less than 0.045 mm account for more than 5% by volume and less than 40% by volume, Among the refractory particles in the refractory, at least around the coarse particles of the largest particle size, there is a substantially continuous void layer similar in shape to the coarse particles, and in the substantially continuous void layer, the total thickness of the void layer existing at the interface between the matrix structure containing carbon at both ends and the coarse particles is 0.3% or more and 3.0% or less relative to the particle size of the coarse particles, Furthermore, the apparent porosity is 16% or less, and the maximum thermal expansion coefficient up to 1500° C. is 0.6% or less.
2. The refractory for continuous casting according to claim 1, characterized in that: The refractory particles having a particle size exceeding 0.3 mm account for 10% by volume or more, and the refractory particles having a particle size of 0.045 mm or less account for 10% by volume or more and 30% by volume or less.
3. The refractory for continuous casting according to claim 1 or 2, characterized in that: The matrix structure contains carbon fibers having an aspect ratio of 15 to 200, and the content of the carbon fibers is 5% by mass or less.
4. The refractory for continuous casting according to any one of claims 1 to 3, characterized in that: The other components are one or more selected from the group consisting of a magnesium oxide component, a silicon carbide component, a boron carbide component, and a zirconium boride component.
5. A refractory component for continuous casting, characterized in that: The refractory for continuous casting according to any one of claims 1 to 4 is arranged on a part or the whole of a portion in contact with molten steel.
Citation Information
Patent Citations
Zirconia-carbon-containing refractory and method for producing same
CN101970375A
Zirconia-carbon-containing refractory and immersion nozzle disposed with the refractory