Polarizing film and image display device

By directly joining the polarizing film and the resin film, the adhesive layer is avoided, which solves the problems of stress accumulation and uneven interference in the adhesive layer, improves the stability and adhesive force of the polarizing film in high temperature environments, and ensures polarization Efficient performance of the membrane.

CN118786372APending Publication Date: 2024-10-15NITTO DENKO CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380024695.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-30
Filing Date
2023-03-20
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

When the existing polarizing film and the transparent protective film are bonded through the adhesive layer, stress accumulation and uneven interference are prone to occur, resulting in weak adhesion and visually identifiable uneven light interference, especially in high-temperature heating environments. Significantly.

Method used

The polarizing film and the resin film are directly bonded to avoid the adhesive layer, and the thickness of the polarizing film is less than 20 μm. The thickness of the resin film is thicker than the polarizing film. The bonding strength is improved through ultraviolet irradiation and volatile medium drying to ensure that before and after the heating test Suppress interference unevenness.

Benefits of technology

It effectively suppresses the interference unevenness of the polarizing film, improves the adhesive force, enhances humidification reliability, avoids stress accumulation and dichroic material diffusion in the adhesive layer, and improves the stability of the polarizing film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005019920290000101
    Figure BDA0005019920290000101
Patent Text Reader

Abstract

The present invention relates to a polarizing film in which a polarizing film and a resin film are directly bonded together without having an adhesive layer interposed therebetween, and the thickness of the polarizing film is 20 [mu] m or less and is thicker than the thickness of the resin film. The polarizing film can suppress interference unevenness before and after a heating test.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a polarizing film and an image display device. Background Art

[0002] In the past, as polarizing films used in various image display devices such as liquid crystal display devices and organic EL display devices, polyvinyl alcohol films that have been dyed (containing dichroic substances such as iodine and dichroic dyes) have been used because they have both high transmittance and high polarization degree. The polarizing film can be manufactured by subjecting the polyvinyl alcohol film to various treatments such as swelling, dyeing, cross-linking, and stretching in a bath, followed by washing and drying. In addition, the polarizing film is usually used in the form of a polarizing film (polarizer) having a transparent protective film such as triacetyl cellulose bonded to one or both sides with an adhesive.

[0003] In addition, as the above-mentioned polarizing film (polarizing plate), there are also known polarizing films in which a polarizing film and a transparent protective film are directly bonded together without an adhesive layer or a pressure-sensitive adhesive layer (Patent Documents 1 to 4).

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: International Publication No. 2005 / 085918

[0007] Patent Document 2: Japanese Patent Application Publication No. 2002-303725

[0008] Patent Document 3: Japanese Patent Application Publication No. 2002-303726

[0009] Patent Document 4: Japanese Patent Application Publication No. 2002-303727 Summary of the invention

[0010] Problems to be solved by the invention

[0011] There is a strong demand for thin filming for polarizing films and polarizing membranes. When the polarizing film and the transparent protective film are bonded together via an adhesive layer as described above, the adhesive layer is prone to accumulate stress when the adhesive is cured, and stress and strain are easily generated at the interface. In particular, when a transparent protective film thinner than the polarizing film is bonded using an adhesive, the occurrence of strain is likely to become significant, and there is a problem of significant visual recognition of uneven interference of light. In addition, for the polarizing film obtained by the manufacturing method specifically disclosed in Patent Document 1, there is a hidden danger of uneven interference caused by the relationship between the thickness of the polarizing film and the transparent protective film, and then there is a problem of weak adhesion between the polarizing film and the transparent protective film. In addition, the polarizing film obtained by the manufacturing method specifically disclosed in Patent Documents 2-4 requires a crimping process at a high temperature of 135°C, so there are problems in the visual recognition of uneven interference after exposure to a heated environment.

[0012] In view of the above circumstances, an object of the present invention is to provide a polarizing film capable of suppressing interference unevenness before and after a heating test.

[0013] Another object of the present invention is to provide an image display device including the above-mentioned polarizing film.

[0014] Solutions to the problem

[0015] That is, the present invention relates to a polarizing film in which a polarizing film and a resin film are directly bonded together without an adhesive layer or a pressure-sensitive adhesive layer, and the thickness of the polarizing film is 20 μm or less and is thicker than the thickness of the resin film.

[0016] Furthermore, the present invention relates to an image display device having the above-mentioned polarizing film.

[0017] Effects of the Invention

[0018] The details of the mechanism of action of the effect of the polarizing film of the present invention can be estimated as follows. It should be noted that the interpretation of the present invention is not limited to this mechanism of action.

[0019] In the polarizing film of the present invention, the polarizing film and the resin film are directly joined together without an adhesive layer or an adhesive layer. The thickness of the polarizing film is less than 20 μm and is thicker than the thickness of the resin film. Therefore, light interference will not occur in the adhesive layer, and it is not easy to generate fine strain on the surface of the resin film / polarizing film due to the shrinkage of the adhesive. Therefore, the interference unevenness of the polarizing film can be suppressed before and after the heating test.

[0020] In addition, the polarizing film of the present invention can directly bond the polarizing film and the transparent protective film without an adhesive layer or an adhesive layer, so that diffusion of dichroic substances such as iodine into the adhesive layer or the adhesive layer can be suppressed, and thus the humidification reliability is excellent. DETAILED DESCRIPTION

[0021] <Polarizing film>

[0022] The polarizing film of the present invention is formed by directly bonding a polarizing film and a resin film without an adhesive layer or a pressure-sensitive adhesive layer, and the thickness of the polarizing film is 20 μm or less and is thicker than the thickness of the resin film.

[0023] <Polarizing film>

[0024] The polarizing film is formed by adsorbing and aligning a dichroic substance such as iodine or a dichroic dye in a polyvinyl alcohol film. From the viewpoint of initial polarization performance of the polarizing film, the polarizing film is preferably an iodine-based polarizing film containing iodine as the dichroic substance.

[0025] The polyvinyl alcohol (PVA) film can be used without particular limitation. The polyvinyl alcohol (PVA) film has light transmittance in the visible light region and disperses and adsorbs dichroic substances such as iodine and dichroic dyes. As the material of the polyvinyl alcohol film, polyvinyl alcohol or its derivatives can be cited. As the derivatives of the polyvinyl alcohol, for example, polyvinyl formal, polyvinyl acetal; olefins such as ethylene and propylene; derivatives modified with unsaturated carboxylic acids such as acrylic acid, methacrylic acid, crotonic acid and their alkyl esters, acrylamide, etc. The average polymerization degree of the polyvinyl alcohol is preferably about 100 to 10,000, more preferably about 1,000 to 10,000, and further preferably about 1,500 to 4,500. In addition, the saponification degree of the polyvinyl alcohol is preferably about 80 to 100 mol%, more preferably about 95 mol% to 99.95 mol. It should be noted that the average polymerization degree and the saponification degree can be obtained according to JIS K 6726.

[0026] The polarizing film can be obtained by a conventional method for producing a polarizing film, for example, by subjecting the polyvinyl alcohol film to any swelling step and washing step, and at least to a dyeing step, a crosslinking step, and a stretching step.

[0027] From the viewpoint of improving the initial polarization degree of the polarizing film, the thickness of the polarizing film is preferably 1 μm or more, more preferably 2 μm or more, and from the viewpoint of preventing the warping of the panel, it is preferably 15 μm or less, more preferably 10 μm or less, and further preferably 8 μm or less. In particular, in order to obtain a polarizing film having a thickness of about 8 μm or less, the following method for producing a thin polarizing film can be used, in which a laminate comprising a polyvinyl alcohol resin layer formed on a thermoplastic resin substrate is used as the polyvinyl alcohol film.

[0028] A polarizing film (thin polarizing film) can be obtained by an existing method for manufacturing a polarizing film, for example, by implementing a process of preparing a laminate by forming a polyvinyl alcohol resin layer (PVA resin layer) containing a polyvinyl alcohol resin (PVA resin) on one side of a long thermoplastic resin substrate; while transporting the obtained laminate in the length direction, performing an optional insolubilization treatment process, a cross-linking treatment process and a cleaning treatment process on the above-mentioned laminate; and at least performing an auxiliary stretching treatment process in a gas atmosphere, a dyeing treatment process and a stretching treatment process in an aqueous solution to obtain the laminate.

[0029] <Resin film>

[0030] The resin film is not particularly limited as long as it is thinner than the polarizing film. For example, an organic base material such as a transparent protective film or a retardation film that has been used for a polarizing film may be used.

[0031] From the above viewpoints, the ratio of the thickness of the polarizing film to the thickness of the resin film (thickness of the polarizing film / thickness of the resin film) is preferably greater than 1.2, more preferably greater than 1.5, and further preferably greater than 2.0. In addition, from the viewpoint of thinning / curling suppression of the polarizing film, it is preferably less than 10.0, more preferably less than 5.0, and further preferably less than 3.0.

[0032] The thickness of the resin film can be appropriately determined, but is generally preferably 0.5 μm or more, more preferably 1 μm or more, and even more preferably 2 μm or more from the viewpoint of strength, handling properties such as ease of handling, and the like.

[0033] As materials constituting the above-mentioned transparent protective film, for example, cellulose ester resins, polycarbonate resins, (meth) acrylic resins, cyclic polyolefin resins, polyester resins, etc. As the above-mentioned phase difference film, for example, birefringent films formed by unidirectional or bidirectional stretching of polymer raw materials, oriented films of liquid crystal polymers, phase difference plates formed by supporting the oriented layers of liquid crystal polymers with films, etc. In addition, one or more hard coating layers, anti-reflection layers, anti-adhesion layers, diffusion layers, or anti-glare layers, etc., can be provided on the above-mentioned transparent protective film and the above-mentioned phase difference film; optical layers used in the formation of image display devices, such as reflective plates, semi-transmissive plates, phase difference plates (including 1 / 2, 1 / 4, etc. wave plates), and viewing angle compensation films.

[0034] When the resin film is bonded to both surfaces of the polarizing film, the resin films on both surfaces may be the same or different.

[0035] The resin film may contain any appropriate additives such as an ultraviolet absorber, an antioxidant, a lubricant, a plasticizer, a release agent, an anti-coloring agent, a flame retardant, an antistatic agent, a pigment, and a colorant.

[0036] <Method for producing polarizing film>

[0037] The method of directly joining the polarizing film and the resin film without an adhesive layer or an adhesive layer can be cited as follows: a method of crimping, a method of laminating by irradiating energy rays such as ultraviolet rays and electron beams, etc., and in particular, from the viewpoint of suppressing the interference unevenness of the polarizing film and improving the adhesion, it is preferred to irradiate the bonding surface of the resin film and the polarizing film with ultraviolet light and perform surface treatment, and then laminating via a volatile medium, and drying the volatile medium. By the presence of the volatile medium, it is possible to fit closely to the bonding surface without mixing with bubbles, etc., and further, by drying the volatile medium, the adhesion of the bonding surface (interface) is significantly improved. As ultraviolet light, for example, the wavelength is preferably 250-100nm, more preferably 200-100nm, wherein, from the viewpoint of mass production, a wavelength of 172nm using a xenon excimer lamp (excimer UV) is particularly preferred.

[0038] In addition, from the viewpoint of processing capacity, the illuminance of the ultraviolet light is preferably 1 mW / cm 2 More preferably, 50 mW / cm 2 In addition, from the viewpoint of adhesiveness, the accumulated light intensity is preferably 1 mJ / cm 2 More preferably, 50 mJ / cm 2 From the viewpoint of film damage, 5000 mJ / cm 2 Less than, more preferably 2000mJ / cm 2 In addition, the temperature during ultraviolet irradiation is not particularly limited. From the perspective of stabilization of surface modification, it is preferably about 0 to 50°C, more preferably about 10 to 40°C. In the production of polarizing films, room temperature is convenient. In addition, as for the atmosphere during ultraviolet irradiation, the oxygen concentration can be 21% or less. From the perspective of treatment efficiency, the oxygen concentration is preferably 7.0% or less.

[0039] The volatile medium is not particularly limited, but is preferably a solvent such as water, ethanol, toluene, cyclohexane, or acetone from the viewpoint of drying efficiency, and more preferably water from the viewpoint of environment.

[0040] The heating temperature may be any temperature that can properly dry the volatile medium. For example, when the volatile medium is water, the heating temperature is preferably about 40 to 80° C., and more preferably about 50 to 70° C. In addition, the drying time is affected by the temperature of the polarizing film, and therefore cannot be generalized. The drying time is preferably about 1 minute to 60 minutes, and more preferably about 3 to 15 minutes. The drying step may be performed only once, or may be performed multiple times as needed.

[0041] The above-mentioned bonding can be performed by a roll laminator or the like.

[0042] The bonding interface between the polarizing film and the resin film may include a modified layer or a high elastic layer resulting from treatment during bonding.

[0043] In the above-mentioned polarizing film, the adhesion (peel strength) between the above-mentioned resin film and the above-mentioned polarizing film is preferably 0.5N / 15mm or more, more preferably 1.0N / 15mm or more, and further preferably 1.5N / 15mm or more in the peel strength measurement under the conditions of peeling angle 90° and peeling speed 1000mm / min.

[0044] The polarizing film can be applied to an image display device. Representative examples of image display devices include liquid crystal display devices and organic electroluminescent (EL) display devices. The image display device can adopt a well-known structure in the industry, so a detailed description is omitted.

[0045] Example

[0046] Hereinafter, the present invention will be described in more detail with reference to Examples, but the present invention is not limited to these Examples.

[0047] <Example 1>

[0048] <Production of polarizing film>

[0049] A laminated body having a 9 μm thick PVA layer formed on an amorphous PET substrate was subjected to auxiliary stretching in a gas atmosphere at a stretching temperature of 130°C to produce a stretched laminated body, and then the stretched laminated body was dyed to produce a colored laminated body, and further, the colored laminated body was stretched in boric acid water at a stretching temperature of 65 degrees to produce an optical film laminated body including a 5 μm thick polarizing film stretched integrally with the amorphous PET substrate in a manner that the total stretching ratio reached 5.94 times. By such two-step stretching, an optical film laminated body including a polarizing film with a thickness of 5 μm was obtained, in which the PVA molecules of the PVA layer formed on the amorphous PET substrate were highly oriented, and the iodine adsorbed by dyeing was highly oriented in one direction in the form of a polyiodide ion complex.

[0050] <Production of polarizing film>

[0051] In a nitrogen-substituted atmosphere having an oxygen concentration of about 2.5%, the polarizing film surface of the optical film laminate including the polarizing film obtained above, and a cycloolefin resin film with a thickness of 3 μm as a resin film (the cycloolefin resin film with a release liner obtained as follows: after adding 10 g of a cycloolefin polymer (COP) film (trade name "ZEONOR FILM ZF14") to 90 g of a 2:3 mixed solvent of 2,4-trichlorobenzene and toluene to prepare a COP solution, the prepared COP solution was applied on a PET film (release liner) using a wire bar coater #13, and then dried in an oven at 60°C for 3 minutes, thereby laminating a COP film with a thickness of 3 μm on the release liner.) were irradiated with excimer UV light (wavelength 172 nm, peak illuminance 75 mW / cm 2 、Accumulated light quantity 450mJ / cm 2 ) and surface modification was performed. Next, water was applied to the surface modified surface of each film, and before the water dried, the polarizing film and the resin film were bonded together using a laminator, and then dried in an oven at 60°C for 5 minutes and 30 seconds to obtain a polarizing film in which the polarizing film and the resin film were directly bonded.

[0052] <Evaluation of interference unevenness>

[0053] After peeling off the PET substrate and the release liner of the polarizing film formed by directly bonding the above-mentioned polarizing film and the transparent protective film, the polarizing film surface was adhered to a black acrylic plate via a transparent adhesive. The test piece thus obtained was observed for interference unevenness with the naked eye in a dark room under a desk lamp (three-wavelength fluorescent tube) and evaluated according to the following criteria.

[0054] ◎: No interference unevenness was visually recognized.

[0055] ○: Although a small amount of interference unevenness is visually recognized, it is at a level that does not cause a problem in practical use.

[0056] ×: Interference unevenness is clearly visually recognized.

[0057] <Evaluation of interference unevenness after heating test>

[0058] The test pieces were left in an environment at 85° C. for 240 hours, and then the interference unevenness was visually observed in a dark room under a desk lamp (three-wavelength fluorescent lamp), and evaluated based on the following criteria.

[0059] ◎: No interference unevenness was visually recognized.

[0060] ○: Although a small amount of interference unevenness is visually recognized, it is at a level that does not cause a problem in practical use.

[0061] ×: Interference unevenness is clearly visually recognized.

[0062] <Evaluation of Adhesion (Peel Strength)>

[0063] The PET substrate of the polarizing film formed by directly bonding the above-mentioned polarizing film and the transparent protective film was peeled off, and a double-sided tape (No. 500, manufactured by Nitto Denko Corporation) was attached to the peeling surface. Furthermore, a size of 200 mm parallel to the stretching direction of the polarizing film and 15 mm in the orthogonal direction was cut out, and a cut was made between the polarizing film and the transparent protective film with a cutter, and then the peeling film of the double-sided tape was peeled off, and the adhesive surface was attached to the glass plate. The polarizing film and the transparent protective film were peeled off along the 90-degree direction at a peeling speed of 1000 mm / min using an angle-variable adhesive / film peeling analysis device (VPA-2, manufactured by Kyowa Interface Chemical Co., Ltd.), and the peeling strength (N / 15mm) was measured.

[0064] <Evaluation of humidification reliability>

[0065] After peeling off the PET substrate and the release liner of the above-mentioned polarizing film, the polarizing film side was bonded to the side of the alkali-free glass with a thickness of 0.7 mm via an adhesive layer (thickness 20 μm), and the polarizing film obtained in this way (sample for evaluation of humidification durability test) was prepared. The transmittance Ts of the obtained polarizing film was measured using an ultraviolet visible spectrophotometer (V-7100 manufactured by JASCO Corporation), and the single transmittance Ts, parallel transmittance Tp, and orthogonal transmittance Tc were set as Ts, Tp, and Tc of the polarizing film, respectively. Their Ts, Tp, and Tc are the Y values ​​obtained by measuring the 2-degree field of view (C light source) of JIS Z8701 and correcting the visibility. After being exposed to an environment of 60°C and 95%RH for 120 hours, the transmittance Ts of the polarizing film after exposure was also measured by the same method, and the transmittance change ΔT (%) = | (transmittance Ts (%) before exposure) - (transmittance Ts (%) after exposure) |. The smaller the transmittance change ΔT(%) is, the better the durability in a hot and humid environment is judged to be. ΔT(%) is preferably 0.4 or less, and more preferably 0.3 or less.

[0066] <Example 2>

[0067] <Production of polarizing film>

[0068] A polyvinyl alcohol film with an average degree of polymerization of 2400 and a saponification degree of 99.9 mol% and a thickness of 45 μm was immersed in warm water at 30°C for 60 seconds to swell. Next, it was immersed in an aqueous solution of 0.3% iodine / potassium iodide (weight ratio = 1 / 7), and the film was dyed while being stretched to 2.6 times. Then, it was stretched in a 4 wt% boric acid aqueous solution at 65°C so that the total stretching ratio reached 6 times. After stretching, it was dried in an oven at 55°C for 1 minute to obtain a PVA-type polarizing film. The thickness of the polarizing film is 18 μm and the moisture content is 15 wt%.

[0069] <Production of polarizing film>

[0070] As the resin film, a cycloolefin resin film with a thickness of 13 μm (manufactured by Japan Zeon Co., Ltd., ZF14) was used. In addition, a polarizing film with a thickness of 18 μm produced by the above operation was used. Except for this, the same operation as in Example 1 was performed to obtain a polarizing film in which the polarizing film and the resin film were directly bonded.

[0071] <Comparative Example 1>

[0072] As a resin film, a 3 μm thick cycloolefin resin film (a cycloolefin resin film with a release liner obtained as follows: 10 g of a cycloolefin polymer (COP) film (trade name "ZEONOR Film ZF14") was added to 90 g of a 2:3 mixed solvent of 2,4-trichlorobenzene and toluene to prepare a COP solution, and then the prepared COP solution was applied to a PET film (release liner) using a wire bar coater #13, and then dried in an oven at 60°C for 3 minutes, thereby laminating a 3 μm thick COP film on the release liner.) was coated with the following active energy ray-curable adhesive using a wire bar coater, and the polarizing film surface of the optical film laminate including a polarizing film with a thickness of 5 μm obtained in Example 1 was laminated using a laminator. In this state, active energy rays were irradiated from the resin film side to cure the adhesive, and a polarizing film having a resin film bonded to the polarizing film via an active energy ray adhesive was obtained.

[0073] [Active energy ray-curable adhesive]

[0074] 2-Hydroxyethylacrylamide (manufactured by KJ Chemical Co., Ltd., trade name: HEAA) 16.5 parts by weight, 4-vinylphenylboronic acid (manufactured by Tokyo Chemical Industry Co., Ltd.) 1 part by weight, 2-hydroxy-3-phenoxypropyl acrylate (manufactured by Toagosei Co., Ltd., trade name: Aronix M-5700) 30.5 parts by weight, 1,9-nonanediol diacrylate (manufactured by Kyoeisha Chemical Co., Ltd., trade name: LIGHT ACRYLATE 1,9ND-A) 25 parts by weight, hydroxypivalic acid diacrylate (manufactured by Kyoeisha Chemical Co., Ltd., trade name: LIGHT ACRYLATE HPP-A) 13 parts by weight, an oligomer obtained by polymerizing a (meth)acrylate (manufactured by Toagosei Co., Ltd., trade name: ARFON UP-1190) 15 parts by weight, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropane-1-one (IGM 3 parts by weight of 2,4-diethylthioxanthone (manufactured by Nippon Kayaku Co., Ltd., trade name: KAYACURE-DETX-S)

[0075] [Active energy rays]

[0076] Visible light (gallium-encapsulated metal halide lamp) was used as active energy ray. Irradiation device: Light HAMMER 10 manufactured by Heraeus. Valve: V valve. Peak illuminance: 800 mW / cm 2 , cumulative exposure 800 / mJ / cm 2 (Wavelength: 380 to 440 nm) The illuminance of visible light was measured using a Sola-Check system manufactured by Solatell.

[0077] <Comparative Example 2>

[0078] A 13 μm thick cycloolefin resin film (ZF14 manufactured by Zeon Co., Ltd.) was laminated at 145° C. on one side of a 30 μm thick polarizing film (polyvinyl alcohol film) using a roll laminator to obtain a polarizing film in which the polarizing film and the resin film were directly bonded.

[0079] <Comparative Example 3>

[0080] <Production of polarizing film>

[0081] A polyvinyl alcohol film with an average degree of polymerization of 2400 and a saponification degree of 99.9 mol% and a thickness of 45 μm was immersed in warm water at 30°C for 60 seconds to swell. Next, it was immersed in an aqueous solution of 0.3% iodine / potassium iodide (weight ratio = 1 / 7), and the film was dyed while being stretched to 2.6 times. Then, it was stretched in a 4 wt% boric acid aqueous solution at 65°C so that the total stretching ratio reached 6 times. After stretching, it was dried in an oven at 55°C for 1 minute to obtain a PVA-type polarizing film. The thickness of the polarizing film is 18 μm and the moisture content is 15 wt%.

[0082] <Production of polarizing film>

[0083] As the resin film, a cycloolefin resin film with a thickness of 13 μm (manufactured by Japan Zeon Co., Ltd., ZF14) was used. In addition, a polarizing film with a thickness of 18 μm produced by the above operation was used. Except for this, the same operation as in Comparative Example 1 was performed to obtain a polarizing film in which a resin film was bonded to the polarizing film via an active energy ray adhesive.

[0084] The same evaluation as in Example 1 was performed using the polarizing films obtained in the above-mentioned respective Examples and Comparative Examples. The results are shown in Table 1.

[0085]

Claims

1. A polarizing film, in, The polarizing film and the resin film are directly bonded together without an adhesive layer or a bonding agent layer. The polarizing film has a thickness of 20 μm or less and is thicker than the resin film.

2. The polarizing film according to claim 1, in, The ratio of the thickness of the polarizing film to the thickness of the resin film (thickness of the polarizing film / thickness of the resin film) is 1.2 to 10.

0. 3 . An image display device comprising the polarizing film according to claim 1 .