A method for preparing a 1100°C resistant, low-cost, high-strength aerogel composite material
By combining small-particle silicon sol and large-particle silicon sol with mullite fiber, the problem of failure of high-temperature lightweight insulation materials for spacecraft at high temperatures is solved, and low cost, high strength and low heat are achieved Preparation of conductivity aerogel composite materials, suitable for thermal protection of spacecraft.
Patent Information
- Application Number
- CN202411276198.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-12
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-09-12
AI Technical Summary
The high-temperature and lightweight insulation materials for existing spacecraft fail at high temperatures. The high-temperature thermal conductivity of silica aerogels is high and the mechanical properties are poor, and the preparation process is complex and costly.
The mixture of small-particle silicon sol and large-particle silicon sol is used as the silicon source, combined with mullite fibers, and aerogel composite materials are prepared through a multi-step impregnation and calcination process to form a low-high-temperature thermal conductivity and high mechanical properties. Material.
The prepared aerogel composite material can maintain excellent high-temperature resistance and mechanical properties at a high temperature of 1100°C, with low thermal conductivity at high temperatures, no cracking on the surface, simple process and low cost.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of thermal insulation materials, and in particular to a method for preparing a 1100° C. resistant, low-cost, high-strength aerogel composite material. Background Art
[0002] With the rapid development of science and technology, hypersonic aircraft have become a hot topic for research and development in various countries around the world. In order to ensure the safety performance of the aircraft, the surface of the aircraft must be thermally protected. At the same time, the load of the aircraft should be kept as unchanged as possible. Therefore, there is an increasingly clear demand for high-temperature resistant and lightweight thermal insulation materials for aerospace vehicles.
[0003] At present, the commonly used high-temperature resistant lightweight insulation material for aerospace vehicles is silica aerogel, which has low high-temperature thermal conductivity and can effectively inhibit heat transfer, but its long-term use temperature is 650-800°C, which is difficult to meet the use requirements at high temperatures. In order to improve the high-temperature resistance of silica aerogel, the most commonly used method is to dope the silica aerogel with high-temperature resistant components, metal oxides, to obtain doped silica aerogel, but the high-temperature thermal conductivity of doped silica aerogel is higher than that of silica aerogel, and its mechanical properties are poor.
[0004] In order to solve the above problems, the failure mechanism of silica aerogel at high temperature was analyzed. It was found that at high temperature, the silica particles in the silica aerogel will fuse, which will cause the aerogel matrix to shrink and cause the internal pore structure of the silica aerogel to collapse. After further experiments, it was found that when using small-particle silica sol as a silicon source to prepare silica aerogel, the skeleton of the prepared silica aerogel is formed by the agglomeration of small-particle silica. Since there are more contact points between small-particle silica, there is obvious agglomeration between small-particle silica, which will improve the mechanical properties of silica aerogel. However, macropores are prone to appear in the prepared silica aerogel, resulting in a higher high-temperature thermal conductivity of silica aerogel. At the same time, aerogels with smaller particle sizes are more likely to melt at high temperatures and have poor heat resistance. When using large-particle silica sol as a silicon source to prepare silica aerogel, the skeleton of silica aerogel is formed by large-particle silica interconnected, and the prepared silica aerogel has less macropores and can still maintain a good aerogel network structure at high temperatures. Therefore, the high-temperature thermal conductivity of silica aerogel is lower. However, due to the fewer contact points between large-particle silica and the lower degree of agglomeration between large-particle silica, the mechanical properties of silica aerogel will be reduced.
[0005] Therefore, in view of the above failure mechanism and experimental findings, the inventors tried to mix an appropriate proportion of small-particle silica sol and large-particle silica sol as a silicon source, and added mullite fiber to prepare an aerogel composite material. The large-particle silica and the small-particle silica are combined to form the skeleton of the silica aerogel, which can strengthen the aerogel network skeleton, reduce the macropore content in the aerogel composite material, improve the high temperature resistance and mechanical properties of the aerogel composite material, and reduce the high-temperature thermal conductivity of the aerogel composite material; and utilize the excellent high temperature resistance and mechanical properties of mullite fiber to further improve the high temperature resistance and mechanical properties of the aerogel composite material, and the process is simple and the cost is low.
[0006] However, when preparing aerogel composite materials by the above method, the following problems still exist: first, after mixing small-particle silica sol and large-particle silica sol, small-particle silica is easy to agglomerate, resulting in uneven mixing during the mixing process, further resulting in the appearance of large pores in the prepared aerogel composite material, thereby increasing the high-temperature thermal conductivity of the aerogel composite material; second, there is a problem of poor interface compatibility between mullite fiber and silica aerogel, which not only increases the high-temperature thermal conductivity of the aerogel composite material, but also causes the aerogel composite material to crack; third, small-particle silica sol will block some of the pores formed by large-particle silica sol, thereby further increasing the high-temperature thermal conductivity of the aerogel composite material. Summary of the invention
[0007] In view of the shortcomings of the prior art, the present invention provides a method for preparing a low-cost and high-strength aerogel composite material resistant to 1100°C. The cost is low, and the prepared aerogel composite material has excellent high-temperature resistance and mechanical properties, low high-temperature thermal conductivity, and no surface cracks.
[0008] In order to solve the above technical problems, the technical solution adopted by the present invention is as follows:
[0009] A method for preparing a 1100°C resistant, low-cost, high-strength aerogel composite material, comprising the following steps: preparing filler, pretreatment, primary impregnation, secondary impregnation;
[0010] The preparation of filler comprises the following steps: preparation of nano carbon, calcination, hydroxylation, and surface coating;
[0011] The method for preparing nano-carbon comprises mixing glucose, sodium polyacrylate and deionized water, stirring at 40-60° C. for 40-60 min to obtain a mixed solution; transferring the mixed solution into a hydrothermal synthesis kettle, sealing the mixture, transferring the hydrothermal synthesis kettle into an oven, heating the oven to 180-190° C., standing for 14-16 h, filtering, washing the filter residue with deionized water for 3-4 times, transferring the mixture into a vacuum oven, adjusting the temperature of the vacuum oven to 60-70° C., standing for 8-9 h, transferring the mixture into a grinder and grinding the mixture into a particle size of 35-40 nm to obtain nano-carbon;
[0012] In the preparation of nanocarbon, the mass volume ratio of glucose, sodium polyacrylate and deionized water is 80-85g:0.35-0.4g:270-300mL;
[0013] The heating rate when the temperature rises to 180-190°C is 5-6°C / min;
[0014] The number average molecular weight of the sodium polyacrylate is 10000;
[0015] The calcination is to transfer the nanocarbon into a tube furnace, heat the tube furnace to 700-750° C. in a nitrogen atmosphere, and stand for 3-3.5 hours to obtain porous nanocarbon;
[0016] During the calcination, the heating rate when the temperature is raised to 700-750°C is 7-8°C / min;
[0017] The hydroxylation comprises mixing the porous nano-carbon and the nitric acid aqueous solution, stirring for 10-11 hours at 20-35° C., transferring the mixture into a centrifuge, adjusting the centrifugal speed of the centrifuge to 7000-8000 rpm, centrifuging for 8-10 minutes, taking the precipitate, washing it with deionized water for 5-7 times, transferring the mixture into a vacuum oven, adjusting the temperature of the vacuum oven to 60-70° C., and standing for 13-15 hours to obtain the hydroxylated porous nano-carbon;
[0018] In the hydroxylation, the mass volume ratio of the porous nanocarbon and the nitric acid aqueous solution is 100-110 g:650-700 mL;
[0019] The concentration of the nitric acid aqueous solution is 5 mol / L;
[0020] The surface coating comprises mixing hydroxylated porous nanocarbon, sodium dodecyl sulfate and deionized water, stirring at 20-35° C. for 18-20 hours, transferring to a centrifuge, adjusting the centrifugal speed of the centrifuge to 7000-8000 rpm, centrifuging for 8-10 minutes, taking a precipitate, washing it with deionized water for 5-7 times, transferring to a vacuum oven, adjusting the temperature of the vacuum oven to 60-70° C., and standing for 13-15 hours to obtain a filler;
[0021] In the surface coating, the mass volume ratio of hydroxylated porous nanocarbon, sodium dodecyl sulfate and deionized water is 10-12g:6-7g:550-600mL;
[0022] The pretreatment is composed of the following steps: primary pretreatment, secondary pretreatment;
[0023] The primary pretreatment comprises mixing γ-aminopropyltriethoxysilane, anhydrous ethanol and deionized water, stirring at 40-50° C. for 1-1.5 hours to obtain a primary pretreatment solution; completely immersing the mullite fiber felt in the primary pretreatment solution at 40-50° C. for 7-8 hours, then taking it out and transferring it to a vacuum oven, adjusting the temperature of the vacuum oven to 80-90° C., and standing it for 8-10 hours to obtain a primary pretreated mullite fiber felt;
[0024] In the primary pretreatment, the volume ratio of γ-aminopropyltriethoxysilane, anhydrous ethanol and deionized water is 200-220:1800-1900:100-150;
[0025] The secondary pretreatment comprises mixing γ-glycidyloxypropyl trimethoxysilane, γ-methacryloxypropyl trimethoxysilane and deionized water, adjusting the pH to 2-2.5 under nitrogen protection, stirring at 60-65° C. for 4-5 hours, transferring to a vacuum oven, adjusting the temperature of the vacuum oven to 70-80° C., and standing for 6-7 hours to obtain a hyperbranched polysiloxane; mixing the hyperbranched polysiloxane and anhydrous ethanol, stirring at 60-65° C. for 20-30 minutes to obtain a secondary pretreatment liquid; completely immersing the primary pretreated mullite fiber felt in the secondary pretreatment liquid, completely immersing at 60-65° C. for 4-5 hours, then taking it out and transferring it to a vacuum oven, adjusting the temperature of the vacuum oven to 80-90° C., and standing for 10-12 hours to obtain a pretreated mullite fiber felt;
[0026] In the secondary pretreatment, the volume ratio of γ-glycidyloxypropyltrimethoxysilane, γ-methacryloxypropyltrimethoxysilane and deionized water is 1250-1300:1300-1400:240-270;
[0027] The volume ratio of hyperbranched polysiloxane to anhydrous ethanol is 1000-1200:300-350;
[0028] The volume ratio of γ-aminopropyltriethoxysilane in the primary pretreatment to γ-glycidyloxypropyltrimethoxysilane in the secondary pretreatment is 200-220:1250-1300;
[0029] The primary impregnation comprises mixing small-particle silica sol, large-particle silica sol, filler, ammonium chloride, γ-aminopropyltriethoxysilane, citric acid and anhydrous ethanol, and stirring at 20-35° C. for 30-40 minutes to obtain a primary impregnation liquid; placing the pretreated mullite fiber felt into a mold, and then adding the primary impregnation liquid to ensure that the pretreated mullite fiber felt can be completely immersed in the primary impregnation liquid, performing vacuum impregnation, and then taking it out and transferring it to an oven for gelation, and then taking it out and completely immersing it in an aging liquid for aging, and then transferring it to a high-pressure reactor for supercritical drying, and transferring it to a tubular furnace for primary calcination and secondary calcination to obtain a primary impregnation mullite fiber felt;
[0030] In the one-time impregnation, the mass volume ratio of small-particle silica sol, large-particle silica sol, filler, ammonium chloride, γ-aminopropyltriethoxysilane, citric acid, and anhydrous ethanol is 250-260 mL: 87-90 mL: 10-12 g: 0.2-0.25 g: 0.5-0.6 mL: 14-16 g: 1700-1800 mL;
[0031] The small-particle size of the silica sol is 15-20 nm, the mass content of silicon dioxide is 10%, and the pH is 8.5-9.5;
[0032] The large-particle silica sol has a particle size of 25-50 nm, a mass content of silicon dioxide of 30%, and a pH of 8.5-9.5;
[0033] The vacuum pressure of the vacuum impregnation is -0.095MPa to -0.1MPa, and the time is 40-60min;
[0034] The gelation temperature is 50-55°C and the time is 2-10h;
[0035] The aging liquid is anhydrous ethanol;
[0036] The aging temperature is 50-55°C and the aging time is 48-96h;
[0037] During the aging process, the aging liquid is replaced twice every 24 hours;
[0038] The temperature of the high-pressure reactor in the supercritical drying is 270-280°C, the pressure is 7-9MPa, and the heat and pressure holding time is 1-2h;
[0039] The primary calcination temperature is 800-850°C and the time is 2-2.5h;
[0040] The temperature of the secondary calcination is 950-1000°C and the time is 1-1.5h;
[0041] The secondary impregnation comprises mixing small-particle silica sol, ammonium chloride, γ-aminopropyltriethoxysilane, sodium dodecylsulfonate, citric acid and anhydrous ethanol, and stirring at 20-35° C. for 30-40 minutes to obtain a secondary impregnation solution; placing the primary impregnated mullite fiber felt into a mold, transferring the mold into a vacuum tank, and then adding the secondary impregnation solution to ensure that the primary impregnated mullite fiber felt can be completely immersed in the secondary impregnation solution for vacuum impregnation, and then taking it out and transferring it into an oven for gelation to obtain a secondary impregnated mullite fiber felt; completely immersing the secondary impregnated mullite fiber felt in an aging solution for aging; then transferring it into a high-pressure reactor for supercritical drying, and transferring it into a tubular furnace for calcination to obtain a 1100° C. resistant, low-cost, and high-strength aerogel composite material;
[0042] In the secondary impregnation, the mass volume ratio of small-particle silica sol, ammonium chloride, γ-aminopropyltriethoxysilane, sodium dodecylsulfonate, citric acid, and anhydrous ethanol is 350-400mL: 0.15-0.2g: 0.3-0.4mL: 6-7g: 11-12g: 1300-1500mL;
[0043] The small-particle size of the silica sol is 15-20 nm, the mass content of silicon dioxide is 10%, and the pH is 8.5-9.5;
[0044] The vacuum impregnation has a vacuum pressure of -0.095 MPa to -0.1 MPa and a time of 80-90 min;
[0045] The gelation temperature is 50-55°C and the time is 2-10h;
[0046] The aging temperature is 50-55°C and the aging time is 48-96h;
[0047] During the aging process, the aging liquid is replaced twice every 24 hours;
[0048] The supercritical drying temperature is 270-280°C, the pressure is 7-9MPa, and the heat and pressure holding time is 1-2h;
[0049] The calcination temperature is adjusted to 800-850°C and the time is 3-4h;
[0050] The aging liquid is anhydrous ethanol.
[0051] Compared with the prior art, the present invention has the following beneficial effects:
[0052] (1) The preparation method of the aerogel composite material of the present invention has simple process and low cost;
[0053] (2) The aerogel composite material prepared by the present invention has excellent high temperature resistance and can withstand high temperatures of 1100°C;
[0054] (3) The aerogel composite material prepared by the present invention has excellent mechanical properties, and the compressive strength at 3% compression is 0.17-0.20MPa;
[0055] (4) The aerogel composite material prepared by the present invention has low high-temperature thermal conductivity, and the thermal conductivity coefficient at 1000°C is 0.08-0.09 W / m·K;
[0056] (5) The aerogel composite material prepared by the present invention has no cracks on the surface. DETAILED DESCRIPTION
[0057] In order to have a clearer understanding of the technical features, purposes and effects of the present invention, the specific implementation methods of the present invention are now described.
[0058] Example 1
[0059] A method for preparing a 1100°C resistant, low-cost, high-strength aerogel composite material, specifically comprising:
[0060] 1. Preparation of filler:
[0061] (1) Preparation of nanocarbon: 80 g of glucose, 0.35 g of sodium polyacrylate and 270 mL of deionized water were mixed and stirred at 40 °C for 40 min to obtain a mixed solution; the mixed solution was transferred into a hydrothermal synthesis kettle, which was sealed, and then the hydrothermal synthesis kettle was transferred into an oven, which was heated to 180 °C at a heating rate of 5 °C / min, and the mixture was allowed to stand for 14 h, filtered, and the filter residue was washed three times with deionized water, transferred into a vacuum oven, and the temperature of the vacuum oven was adjusted to 60 °C, and the mixture was allowed to stand for 8 h, and then transferred into a grinder and ground to a particle size of 35 nm to obtain nanocarbon;
[0062] The number average molecular weight of the sodium polyacrylate is 10000;
[0063] (2) Calcination: The nanocarbon was transferred into a tubular furnace, and the temperature of the tubular furnace was raised to 700°C at a heating rate of 7°C / min in a nitrogen atmosphere, and the mixture was allowed to stand for 3 h to obtain porous nanocarbon.
[0064] (3) Hydroxylation: 100 g of porous nanocarbon and 650 mL of 5 mol / L nitric acid aqueous solution were mixed, stirred at 20 °C for 10 h, transferred to a centrifuge, the centrifugal speed of the centrifuge was adjusted to 7000 rpm, centrifuged for 8 min, the precipitate was taken, washed with deionized water 5 times, transferred to a vacuum oven, the temperature of the vacuum oven was adjusted to 60 °C, and allowed to stand for 13 h to obtain hydroxylated porous nanocarbon;
[0065] (4) Surface coating: 10 g of hydroxylated porous nanocarbon, 6 g of sodium dodecyl sulfate, and 550 mL of deionized water were mixed, stirred at 20 °C for 18 h, transferred to a centrifuge, and the centrifugal speed of the centrifuge was adjusted to 7000 rpm. The centrifuge was centrifuged for 8 min. The precipitate was taken and washed with deionized water for 5 times. The precipitate was transferred to a vacuum oven, and the temperature of the vacuum oven was adjusted to 60 °C. The mixture was allowed to stand for 13 h to obtain a filler.
[0066] 2. Preprocessing:
[0067] (1) Primary pretreatment: 200 mL of γ-aminopropyltriethoxysilane, 1800 mL of anhydrous ethanol and 100 mL of deionized water were mixed and stirred at 40°C for 1 h to obtain a primary pretreatment solution; the mullite fiber felt was completely immersed in the primary pretreatment solution at 40°C for 7 h, then taken out and transferred to a vacuum oven, the temperature of the vacuum oven was adjusted to 80°C, and allowed to stand for 8 h to obtain a primary pretreated mullite fiber felt;
[0068] (2) Secondary pretreatment: 1250 mL of γ-glycidyloxypropyl trimethoxysilane, 1300 mL of γ-methacryloxypropyl trimethoxysilane and 240 mL of deionized water were mixed, and the pH was adjusted to 2 under nitrogen protection. The mixture was stirred at 60°C for 4 h, and then placed in a vacuum oven. The temperature of the vacuum oven was adjusted to 70°C, and the mixture was allowed to stand for 6 h to obtain hyperbranched polysiloxane. 1000 mL of hyperbranched polysiloxane and 300 mL of anhydrous ethanol were mixed, and the mixture was stirred at 60°C for 20 min to obtain a secondary pretreatment solution. The primary pretreated mullite fiber felt was completely immersed in the secondary pretreatment solution, and the mixture was completely immersed at 60°C for 4 h, and then taken out and placed in a vacuum oven. The temperature of the vacuum oven was adjusted to 80°C, and the mixture was allowed to stand for 10 h to obtain a pretreated mullite fiber felt.
[0069] 3. Primary impregnation: Mix 250mL small-particle silica sol, 87mL large-particle silica sol, 10g filler, 0.2g ammonium chloride, 0.5mL γ-aminopropyltriethoxysilane, 14g citric acid, and 1700-1800mL anhydrous ethanol, and stir at 20°C for 30min to obtain a primary impregnation solution; put the pretreated mullite fiber felt into the mold, transfer the mold into a vacuum tank, evacuate to a vacuum pressure of -0.095MPa, and then add the primary impregnation solution to ensure that the pretreated mullite fiber felt can be completely immersed in the primary impregnation solution. At a vacuum pressure of -0.095MPa, a, and then take it out and transfer it to an oven for gelation, adjust the temperature of the oven to 50°C, take it out again after 2 hours and completely immerse it in the aging liquid, and age it for 48 hours at a temperature of 50°C. During the aging process, the aging liquid is replaced twice every 24 hours, and then it is transferred to a high-pressure reactor for supercritical drying, and the temperature of the high-pressure reactor is adjusted to 270°C, the pressure is adjusted to 7MPa, and the heat and pressure are maintained for 1 hour, and then it is transferred to a tubular furnace, and the temperature of the tubular furnace is adjusted to 800°C, and it is allowed to stand for 2 hours, and then the temperature of the tubular furnace is adjusted to 950°C, and it is allowed to stand for 1 hour to obtain a once-impregnated mullite fiber felt;
[0070] The small-particle size of the silica sol is 15 nm, the mass content of silicon dioxide is 10%, and the pH is 8.5;
[0071] The large-particle silica sol has a particle size of 25 nm, a mass content of silicon dioxide of 30%, and a pH of 8.5;
[0072] The aging liquid is anhydrous ethanol;
[0073] 4. Secondary impregnation: 350mL small-particle silica sol, 0.15g ammonium chloride, 0.3mL γ-aminopropyl triethoxysilane, 6g sodium dodecyl sulfate, 11g citric acid, and 1300mL anhydrous ethanol were mixed and stirred at 20°C for 30min to obtain a secondary impregnation solution; the primary impregnated mullite fiber felt was loaded into a mold, the mold was transferred to a vacuum tank, and the vacuum was evacuated to a vacuum pressure of -0.095MPa, and then the secondary impregnation solution was added to ensure that the primary impregnated mullite fiber felt could be completely immersed in the secondary impregnation solution, and the mixture was allowed to stand for 80min under a vacuum pressure of -0.095MPa. in, then take it out and transfer it to an oven for gelation, adjust the temperature of the oven to 50°C, and after 2 hours, obtain a secondary impregnated mullite fiber felt; completely immerse the secondary impregnated mullite fiber felt in the aging liquid, age it at a temperature of 50°C for 48 hours, and replace the aging liquid twice every 24 hours during the aging process; then transfer it to a high-pressure reactor for supercritical drying, adjust the temperature of the high-pressure reactor to 270°C, adjust the pressure to 7MPa, keep the temperature and pressure for 1 hour, transfer it to a tubular furnace, adjust the temperature of the tubular furnace to 800°C, and let it stand for 3 hours to obtain a low-cost and high-strength aerogel composite material resistant to 1100°C;
[0074] The small-particle size of the silica sol is 15 nm, the mass content of silicon dioxide is 10%, and the pH is 8.5;
[0075] The aging liquid is anhydrous ethanol.
[0076] Example 2
[0077] A method for preparing a 1100°C resistant, low-cost, high-strength aerogel composite material, specifically comprising:
[0078] 1. Preparation of filler:
[0079] (1) Preparation of nanocarbon: 82 g of glucose, 0.38 g of sodium polyacrylate, and 280 mL of deionized water were mixed and stirred at 50 °C for 50 min to obtain a mixed solution; the mixed solution was transferred into a hydrothermal synthesis kettle, which was sealed, and then the hydrothermal synthesis kettle was transferred into an oven, which was heated to 185 °C at a heating rate of 5 °C / min, and the mixture was allowed to stand for 15 h, filtered, and the filter residue was washed three times with deionized water, transferred into a vacuum oven, and the temperature of the vacuum oven was adjusted to 65 °C, and the mixture was allowed to stand for 8.5 h, and then transferred into a grinder and ground to a particle size of 40 nm to obtain nanocarbon;
[0080] The number average molecular weight of the sodium polyacrylate is 10000;
[0081] (2) Calcination: The nanocarbon was transferred into a tubular furnace, and the temperature was raised to 720°C at a heating rate of 7°C / min in a nitrogen atmosphere, and the mixture was allowed to stand for 3 h to obtain porous nanocarbon.
[0082] (3) Hydroxylation: 105 g of porous nanocarbon and 680 mL of 5 mol / L nitric acid aqueous solution were mixed, stirred at 30 °C for 10.5 h, transferred to a centrifuge, and the centrifugal speed of the centrifuge was adjusted to 7500 rpm. The centrifuge was centrifuged for 9 min, and the precipitate was taken and washed with deionized water for 6 times. The precipitate was transferred to a vacuum oven, and the temperature of the vacuum oven was adjusted to 65 °C. The mixture was allowed to stand for 14 h to obtain hydroxylated porous nanocarbon.
[0083] (4) Surface coating: 11 g of hydroxylated porous nanocarbon, 6.5 g of sodium dodecyl sulfate, and 580 mL of deionized water were mixed, stirred at 30 °C for 19 h, transferred to a centrifuge, and the centrifugal speed of the centrifuge was adjusted to 7500 rpm. The centrifuge was centrifuged for 9 min, and the precipitate was taken and washed with deionized water for 6 times. The precipitate was transferred to a vacuum oven, and the temperature of the vacuum oven was adjusted to 65 °C. The mixture was allowed to stand for 14 h to obtain a filler.
[0084] 2. Preprocessing:
[0085] (1) Primary pretreatment: 210 mL of γ-aminopropyltriethoxysilane, 1850 mL of anhydrous ethanol and 120 mL of deionized water were mixed and stirred at 45 °C for 1 h to obtain a primary pretreatment solution; the mullite fiber felt was completely immersed in the primary pretreatment solution at 45 °C for 7.5 h, then taken out and transferred to a vacuum oven, the temperature of the vacuum oven was adjusted to 85 °C, and allowed to stand for 9 h to obtain a primary pretreated mullite fiber felt;
[0086] (2) Secondary pretreatment: 1280 mL of γ-glycidyloxypropyl trimethoxysilane, 1350 mL of γ-methacryloxypropyl trimethoxysilane and 250 mL of deionized water were mixed, and the pH was adjusted to 2 under nitrogen protection. The mixture was stirred at 60°C for 4.5 h, and then placed in a vacuum oven. The temperature of the vacuum oven was adjusted to 75°C, and the mixture was allowed to stand for 6.5 h to obtain hyperbranched polysiloxane. 1100 mL of hyperbranched polysiloxane and 320 mL of anhydrous ethanol were mixed, and the mixture was stirred at 60°C for 25 min to obtain a secondary pretreatment solution. The primary pretreated mullite fiber felt was completely immersed in the secondary pretreatment solution, and the mixture was completely immersed at 60°C for 4.5 h, and then taken out and placed in a vacuum oven. The temperature of the vacuum oven was adjusted to 85°C, and the mixture was allowed to stand for 11 h to obtain a pretreated mullite fiber felt.
[0087] 3. Primary impregnation: Mix 255 mL of small-particle silica sol, 88 mL of large-particle silica sol, 11 g of filler, 0.22 g of ammonium chloride, 0.55 mL of γ-aminopropyltriethoxysilane, 15 g of citric acid, and 1750 mL of anhydrous ethanol, and stir at 30 ° C for 35 min to obtain a primary impregnation solution; put the pretreated mullite fiber felt into the mold, transfer the mold into a vacuum tank, evacuate to a vacuum pressure of -0.095 MPa, and then add the primary impregnation solution to ensure that the pretreated mullite fiber felt can be completely immersed in the primary impregnation solution. The fiber felt was placed under the conditions of 50 min, then taken out and transferred to an oven for gelation, the temperature of the oven was adjusted to 50°C, after 6 hours, taken out and completely immersed in the aging liquid, aged for 70 hours at a temperature of 50°C, the aging liquid was replaced twice every 24 hours during the aging process, and then transferred to a high-pressure reactor for supercritical drying, the temperature of the high-pressure reactor was adjusted to 275°C, the pressure was adjusted to 8MPa, the heat and pressure were maintained for 1.5 hours, and then transferred to a tubular furnace, the temperature of the tubular furnace was adjusted to 820°C, and it was placed for 2 hours, and then the temperature of the tubular furnace was adjusted to 980°C, and it was placed for 1 hour to obtain a once-impregnated mullite fiber felt;
[0088] The small-particle silica sol has a size of 20 nm, a mass content of silicon dioxide of 10%, and a pH of 9;
[0089] The large-particle silica sol has a particle size of 40 nm, a mass content of silicon dioxide of 30%, and a pH of 9;
[0090] The aging liquid is anhydrous ethanol;
[0091] 4. Secondary impregnation: 380mL small-particle silica sol, 0.17g ammonium chloride, 0.3mL γ-aminopropyl triethoxysilane, 6.5g sodium dodecyl sulfate, 11.5g citric acid, and 1400mL anhydrous ethanol were mixed and stirred at 30°C for 35min to obtain a secondary impregnation solution; the primary impregnated mullite fiber felt was loaded into a mold, the mold was transferred to a vacuum tank, and the vacuum was evacuated to a vacuum pressure of -0.095MPa, and then the secondary impregnation solution was added to ensure that the primary impregnated mullite fiber felt could be completely immersed in the secondary impregnation solution, and the mixture was allowed to stand for 85min under a vacuum pressure of -0.095MPa. in, then take it out and transfer it to an oven for gelation, adjust the temperature of the oven to 50°C, and after 6 hours, obtain a secondary impregnated mullite fiber felt; completely immerse the secondary impregnated mullite fiber felt in an aging solution, age it at a temperature of 50°C for 70 hours, and replace the aging solution twice every 24 hours during the aging process; then transfer it to a high-pressure reactor for supercritical drying, adjust the temperature of the high-pressure reactor to 275°C, adjust the pressure to 8MPa, keep the temperature and pressure for 1.5 hours, transfer it to a tubular furnace, adjust the temperature of the tubular furnace to 820°C, and let it stand for 3.5 hours to obtain a low-cost and high-strength aerogel composite material resistant to 1100°C;
[0092] The small-particle silica sol has a size of 20 nm, a mass content of silicon dioxide of 10%, and a pH of 9;
[0093] The aging liquid is anhydrous ethanol.
[0094] Example 3
[0095] A method for preparing a 1100°C resistant, low-cost, high-strength aerogel composite material, specifically comprising:
[0096] 1. Preparation of filler:
[0097] (1) Preparation of nanocarbon: 85 g of glucose, 0.4 g of sodium polyacrylate and 300 mL of deionized water were mixed and stirred at 60 °C for 60 min to obtain a mixed solution; the mixed solution was transferred into a hydrothermal synthesis kettle, sealed, and then the hydrothermal synthesis kettle was transferred into an oven, the oven was heated to 190 °C at a heating rate of 6 °C / min, the mixture was allowed to stand for 16 h, filtered, the filter residue was washed 4 times with deionized water, transferred into a vacuum oven, the temperature of the vacuum oven was adjusted to 70 °C, the mixture was allowed to stand for 9 h, and then the mixture was transferred into a grinder and ground to a particle size of 40 nm to obtain nanocarbon;
[0098] The number average molecular weight of the sodium polyacrylate is 10000;
[0099] (2) Calcination: The nanocarbon was transferred into a tubular furnace, and the temperature was raised to 750°C at a heating rate of 8°C / min in a nitrogen atmosphere, and the furnace was allowed to stand for 3.5 h to obtain porous nanocarbon.
[0100] (3) Hydroxylation: 110 g of porous nanocarbon and 700 mL of 5 mol / L nitric acid aqueous solution were mixed, stirred at 35 °C for 11 h, transferred to a centrifuge, the centrifugal speed of the centrifuge was adjusted to 8000 rpm, centrifuged for 10 min, the precipitate was taken, washed with deionized water 7 times, transferred to a vacuum oven, the temperature of the vacuum oven was adjusted to 70 °C, and allowed to stand for 15 h to obtain hydroxylated porous nanocarbon;
[0101] (4) Surface coating: 12 g of hydroxylated porous nanocarbon, 7 g of sodium dodecyl sulfate, and 600 mL of deionized water were mixed, stirred at 35 °C for 20 h, transferred to a centrifuge, and the centrifugal speed of the centrifuge was adjusted to 8000 rpm. The centrifuge was centrifuged for 10 min. The precipitate was taken and washed with deionized water for 7 times. The precipitate was transferred to a vacuum oven, and the temperature of the vacuum oven was adjusted to 70 °C. The mixture was allowed to stand for 15 h to obtain a filler.
[0102] 2. Preprocessing:
[0103] (1) Primary pretreatment: 220 mL of γ-aminopropyltriethoxysilane, 1900 mL of anhydrous ethanol, and 150 mL of deionized water were mixed, and stirred at 50°C for 1.5 h to obtain a primary pretreatment solution; the mullite fiber felt was completely immersed in the primary pretreatment solution at 50°C for 8 h, then taken out and transferred to a vacuum oven, the temperature of the vacuum oven was adjusted to 90°C, and allowed to stand for 10 h to obtain a primary pretreated mullite fiber felt;
[0104] (2) Secondary pretreatment: 1300 mL of γ-glycidyloxypropyl trimethoxysilane, 1400 mL of γ-methacryloxypropyl trimethoxysilane and 270 mL of deionized water were mixed, and the pH was adjusted to 2.5 under nitrogen protection. The mixture was stirred at 65°C for 5 h, and then placed in a vacuum oven. The temperature of the vacuum oven was adjusted to 80°C and the mixture was allowed to stand for 7 h to obtain hyperbranched polysiloxane. 1200 mL of hyperbranched polysiloxane and 350 mL of anhydrous ethanol were mixed, and the mixture was stirred at 65°C for 30 min to obtain a secondary pretreatment solution. The primary pretreated mullite fiber felt was completely immersed in the secondary pretreatment solution at 65°C for 5 h, and then taken out and placed in a vacuum oven. The temperature of the vacuum oven was adjusted to 90°C and the mixture was allowed to stand for 12 h to obtain a pretreated mullite fiber felt.
[0105] 3. Primary impregnation: Mix 260 mL of small-particle silica sol, 90 mL of large-particle silica sol, 12 g of filler, 0.25 g of ammonium chloride, 0.6 mL of γ-aminopropyltriethoxysilane, 16 g of citric acid, and 1800 mL of anhydrous ethanol, and stir at 35 ° C for 40 min to obtain a primary impregnation solution; put the pretreated mullite fiber felt into the mold, transfer the mold into a vacuum tank, evacuate to a vacuum pressure of -0.1 MPa, and then add the primary impregnation solution to ensure that the pretreated mullite fiber felt can be completely immersed in the primary impregnation solution, and let it stand at a vacuum pressure of -0.1 MPa. 60min, then take it out and transfer it to an oven for gelation, adjust the temperature of the oven to 55°C, after 10h, take it out again and completely immerse it in the aging liquid, age it at 55°C for 96h, replace the aging liquid twice every 24h during the aging process, then transfer it to a high-pressure reactor for supercritical drying, adjust the temperature of the high-pressure reactor to 280°C, adjust the pressure to 9MPa, keep the temperature and pressure for 2h, transfer it to a tubular furnace, adjust the temperature of the tubular furnace to 850°C, let it stand for 2.5h, then adjust the temperature of the tubular furnace to 1000°C, let it stand for 1.5h, and obtain a once-impregnated mullite fiber felt;
[0106] The small-particle size of the silica sol is 20 nm, the mass content of silicon dioxide is 10%, and the pH is 9.5;
[0107] The large-particle silica sol has a particle size of 50 nm, a mass content of silicon dioxide of 30%, and a pH of 9.5;
[0108] The aging liquid is anhydrous ethanol;
[0109] 4. Secondary impregnation: 400mL small-particle silica sol, 0.2g ammonium chloride, 0.4mL γ-aminopropyl triethoxysilane, 7g sodium dodecyl sulfate, 12g citric acid, and 1500mL anhydrous ethanol were mixed and stirred at 35°C for 40min to obtain a secondary impregnation solution; the primary impregnated mullite fiber felt was loaded into a mold, the mold was transferred into a vacuum tank, and the vacuum was evacuated to a vacuum pressure of -0.1MPa, and then the secondary impregnation solution was added to ensure that the primary impregnated mullite fiber felt could be completely immersed in the secondary impregnation solution, and the mixture was allowed to stand for 90min under a vacuum pressure of -0.1MPa. Then take it out and transfer it to an oven for gelation, adjust the temperature of the oven to 55°C, and after 10 hours, obtain a secondary impregnated mullite fiber felt; completely immerse the secondary impregnated mullite fiber felt in the aging liquid, age it at a temperature of 55°C for 96 hours, and replace the aging liquid twice every 24 hours during the aging process; then transfer it to a high-pressure reactor for supercritical drying, adjust the temperature of the high-pressure reactor to 280°C, adjust the pressure to 9MPa, keep the temperature and pressure for 2 hours, transfer it to a tubular furnace, adjust the temperature of the tubular furnace to 850°C, and let it stand for 4 hours to obtain a low-cost and high-strength aerogel composite material resistant to 1100°C;
[0110] The small-particle size of the silica sol is 20 nm, the mass content of silicon dioxide is 10%, and the pH is 9.5;
[0111] The aging liquid is anhydrous ethanol.
[0112] Comparative Example 1
[0113] On the basis of Example 2, the filler preparation step in step 1 is omitted, and in the first impregnation step in step 3, the addition of fillers is omitted in the preparation of the first impregnation solution, and the second impregnation step in step 4 is omitted.
[0114] Comparative Example 2
[0115] On the basis of Example 2, the second pretreatment step is omitted, and in the third impregnation step, a mullite fiber felt that has not undergone any pretreatment is used instead of the pretreated mullite fiber felt.
[0116] Performance Testing
[0117] The temperature resistance, thermal conductivity at 1000° C., and compressive strength of the aerogel composite materials of Examples 1-3 and Comparative Examples 1-2 were tested, and whether the surface had surface cracking problems was observed. The observation results are shown in Table 1:
[0118] Table 1
[0119]
[0120] It can be seen from the performance test results that by omitting the addition of fillers in the preparation of the primary impregnation liquid in a single impregnation and performing a secondary impregnation, the temperature resistance and compression strength of the aerogel composite material can be improved, and the thermal conductivity of the aerogel composite material at 1000°C can be reduced; by pretreating the mullite fiber felt, the temperature resistance and compression strength of the aerogel composite material can be improved, and the thermal conductivity of the aerogel composite material at 1000°C can be reduced, and the surface cracking problem of the aerogel composite material can be avoided.
[0121] When preparing the filler added in the preparation of the first impregnation solution, glucose is first reacted with sodium polyacrylate, with glucose as a carbon source and sodium polyacrylate as a porogen; then hydrothermal synthesis is performed to form nanocarbon; then calcination is performed to remove the sodium polyacrylate to form porous nanocarbon; then nitric acid is used for treatment to introduce hydroxyl and carboxyl groups, and finally an anionic surfactant is coated on the surface of the porous nanocarbon. The anionic surfactant can promote the dispersion of the porous nanocarbon and improve the dispersibility of the silica sol because the negative charge on its surface repels the negative charge on the surface of the silica sol; in one impregnation, Porous nanocarbon can promote the penetration of silica sol and strengthen the skeleton of silica aerogel. Then, during the calcination process, part of the porous nanocarbon burns to form unclosed large pores, and then small-particle silica sol is used to evenly fill the formed unclosed large pores. Then, after calcination and melting, closed small pores are formed, which avoids the appearance of large pores and improves the internal binding force of silica aerogel, thereby improving the strength of aerogel composite materials, reducing the thermal conductivity of aerogel composite materials at high temperatures, avoiding the cracking of aerogel composite materials, and improving the high temperature resistance of aerogel composite materials.
[0122] In the pretreatment stage, the mullite fiber felt is first treated with γ-aminopropyl triethoxysilane, and the γ-aminopropyl triethoxysilane reacts with the hydroxyl group on the surface of the mullite fiber felt to introduce amino groups, and then γ-glycidyloxypropyl trimethoxysilane and γ-methacryloxypropyl trimethoxysilane are added to react with the amino groups on the surface of the mullite fiber felt, and hyperbranched polysiloxane is introduced on the surface of the mullite fiber felt. In one impregnation, γ-aminopropyl triethoxysilane is first mixed with silica sol to introduce amino groups on the surface of the silica sol, and then the hyperbranched polysiloxane can bond with the amino groups on the surface of the silica sol to improve the binding ability of the mullite fiber felt and the silica sol. In addition, the hyperbranched chains in the hyperbranched polysiloxane can also play a role in fixing the silica sol. After calcination, the hyperbranched polysiloxane forms small holes on the surface of the mullite fiber felt, thereby improving the strength of the aerogel composite material, reducing the thermal conductivity of the aerogel composite material at high temperature, and avoiding the cracking of the aerogel composite material.
[0123] Unless otherwise specified, all percentages used in the present invention are by mass.
[0124] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a 1100°C resistant, low-cost, high-strength aerogel composite material, characterized in that: The method comprises the following steps: preparing filler, pretreatment, primary impregnation, secondary impregnation; The preparation of filler comprises the following steps: preparation of nano carbon, calcination, hydroxylation, and surface coating; In the preparation of nano-carbon, glucose, sodium polyacrylate and deionized water are mixed, and stirred at 40-60° C. to obtain a mixed solution; the mixed solution is transferred into a hydrothermal synthesis kettle, sealed, and then the hydrothermal synthesis kettle is allowed to stand at 180-190° C., filtered, washed, vacuum dried, and ground to obtain nano-carbon; The calcining is to calcine the nanocarbon at 700-750° C. in a nitrogen atmosphere to obtain porous nanocarbon; The hydroxylation comprises mixing the porous nanocarbon and an aqueous solution of nitric acid, stirring at 20-35° C., centrifuging, taking a precipitate, washing, and vacuum drying the precipitate to obtain the hydroxylated porous nanocarbon; The surface coating comprises mixing hydroxylated porous nanocarbon, sodium dodecyl sulfate and deionized water, stirring at 20-35° C., centrifuging, taking a precipitate, washing and vacuum drying the precipitate to obtain a filler; The pretreatment is composed of the following steps: primary pretreatment, secondary pretreatment; The primary pretreatment comprises mixing γ-aminopropyltriethoxysilane, anhydrous ethanol and deionized water, stirring at 40-50° C. to obtain a primary pretreatment solution; completely immersing the mullite fiber felt in the primary pretreatment solution at 40-50° C., and then vacuum drying to obtain a primary pretreated mullite fiber felt; The secondary pretreatment comprises mixing γ-glycidyloxypropyl trimethoxysilane, γ-methacryloxypropyl trimethoxysilane and deionized water, adjusting the pH to 2-2.5 under nitrogen protection, stirring at 60-65° C., and vacuum drying to obtain hyperbranched polysiloxane; mixing hyperbranched polysiloxane and anhydrous ethanol, stirring at 60-65° C. to obtain a secondary pretreatment liquid; and completely immersing the primary pretreated mullite fiber felt in the secondary pretreatment liquid, completely immersing at 60-65° C., and then vacuum drying to obtain a pretreated mullite fiber felt; The primary impregnation comprises mixing small-particle silica sol, large-particle silica sol, filler, ammonium chloride, γ-aminopropyltriethoxysilane, citric acid and anhydrous ethanol, and stirring at 20-35° C. to obtain a primary impregnation solution; completely immersing the pretreated mullite fiber felt in the primary impregnation solution, performing vacuum impregnation, and then performing gelation, and then completely immersing it in an aging solution for aging, and then performing supercritical drying, and then performing primary calcination and secondary calcination to obtain a primary impregnated mullite fiber felt; The secondary impregnation comprises mixing small-particle silica sol, ammonium chloride, γ-aminopropyltriethoxysilane, sodium dodecylsulfonate, citric acid and anhydrous ethanol, and stirring at 20-35° C. to obtain a secondary impregnation solution; completely immersing the primary impregnation mullite fiber felt in the secondary impregnation solution for vacuum impregnation, and then gelling to obtain a secondary impregnation mullite fiber felt; completely immersing the secondary impregnation mullite fiber felt in an aging solution for aging; and then supercritical drying and calcining to obtain a 1100° C. resistant, low-cost and high-strength aerogel composite material.
2. The method for preparing a 1100°C resistant, low-cost, high-strength aerogel composite material according to claim 1, characterized in that: In the preparation of nanocarbon, the mass volume ratio of glucose, sodium polyacrylate and deionized water is 80-85g:0.35-0.4g:270-300mL; The heating rate when the temperature rises to 180-190°C is 5-6°C / min; The particle size of the nanocarbon is 35-40nm.
3. The method for preparing a 1100°C resistant, low-cost, high-strength aerogel composite material according to claim 1, characterized in that: During the calcination, the heating rate when the temperature is raised to 700-750°C is 7-8°C / min.
4. The method for preparing a 1100°C resistant, low-cost, high-strength aerogel composite material according to claim 1, characterized in that: In the hydroxylation, the mass volume ratio of the porous nanocarbon and the nitric acid aqueous solution is 100-110 g:650-700 mL; The concentration of the nitric acid aqueous solution is 5 mol / L; In the surface coating, the mass volume ratio of hydroxylated porous nanocarbon, sodium dodecyl sulfate and deionized water is 10-12g:6-7g:550-600mL.
5. The method for preparing a 1100°C resistant, low-cost, high-strength aerogel composite material according to claim 1, characterized in that: In the primary pretreatment, the volume ratio of γ-aminopropyltriethoxysilane, anhydrous ethanol and deionized water is 200-220:1800-1900:100-150.
6. The method for preparing a 1100°C resistant, low-cost, high-strength aerogel composite material according to claim 1, characterized in that: In the secondary pretreatment, the volume ratio of γ-glycidyloxypropyltrimethoxysilane, γ-methacryloxypropyltrimethoxysilane and deionized water is 1250-1300:1300-1400:240-270; The volume ratio of hyperbranched polysiloxane to anhydrous ethanol is 1000-1200:300-350; The volume ratio of γ-aminopropyltriethoxysilane in the primary pretreatment to γ-glycidyloxypropyltrimethoxysilane in the secondary pretreatment is 200-220:1250-1300.
7. The method for preparing a 1100°C resistant, low-cost, high-strength aerogel composite material according to claim 1, characterized in that: In the one impregnation, the mass volume ratio of small-particle silica sol, large-particle silica sol, filler, ammonium chloride, γ-aminopropyltriethoxysilane, citric acid, and anhydrous ethanol is 250-260 mL: 87-90 mL: 10-12 g: 0.2-0.25 g: 0.5-0.6 mL: 14-16 g: 1700-1800 mL.
8. The method for preparing a 1100°C resistant, low-cost, high-strength aerogel composite material according to claim 1, characterized in that: In the first impregnation, the small-particle size of the silica sol is 15-20 nm, the mass content of silicon dioxide is 10%, and the pH is 8.5-9.5; The large-particle silica sol has a particle size of 25-50 nm, a mass content of silicon dioxide of 30%, and a pH of 8.5-9.5; The vacuum impregnation has a vacuum pressure of -0.095 MPa to -0.1 MPa and a time of 40-60 min; The gelation temperature is 50-55°C and the time is 2-10h; The aging liquid is anhydrous ethanol; The aging temperature is 50-55°C and the aging time is 48-96h; During the aging process, the aging liquid is replaced twice every 24 hours; The temperature of the high-pressure reactor in the supercritical drying is 270-280°C, the pressure is 7-9MPa, and the heat and pressure holding time is 1-2h; The primary calcination temperature is 800-850°C and the time is 2-2.5h; The temperature of the secondary calcination is 950-1000° C. and the time is 1-1.5 hours.
9. The method for preparing a 1100°C resistant, low-cost, high-strength aerogel composite material according to claim 1, characterized in that: In the secondary impregnation, the mass volume ratio of small-particle silica sol, ammonium chloride, γ-aminopropyltriethoxysilane, sodium dodecylsulfonate, citric acid, and anhydrous ethanol is 350-400mL: 0.15-0.2g: 0.3-0.4mL: 6-7g: 11-12g: 1300-1500mL.
10. The method for preparing a 1100°C resistant, low-cost, high-strength aerogel composite material according to claim 1, characterized in that: In the secondary impregnation, the small-particle size of the silica sol is 15-20 nm, the mass content of silicon dioxide is 10%, and the pH is 8.5-9.5; The vacuum impregnation has a vacuum pressure of -0.095 MPa to -0.1 MPa and a time of 80-90 min; The gelation temperature is 50-55°C and the time is 2-10h; The aging temperature is 50-55°C and the aging time is 48-96h; During the aging process, the aging liquid is replaced twice every 24 hours; The supercritical drying temperature is 270-280°C, the pressure is 7-9MPa, and the heat and pressure holding time is 1-2h; The calcination temperature is 800-850°C and the calcination time is 3-4h; The aging liquid is anhydrous ethanol.