High temperature resistant hydroxy acrylic resin and preparation process
By introducing isocyanate groups and naphthalene ring structures on the surface of the aramid fiber and reacting with hydroxyacrylic resin, the problem of insufficient compatibility and high-temperature performance between the aramid fiber and the resin is solved, and the hardness and wear resistance of the resin are significantly improved. and high temperature resistance.
Patent Information
- Application Number
- CN202411297415.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-18
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-09-18
AI Technical Summary
Traditional hydroxyacrylic resins have shortcomings in high-temperature properties and mechanical strength, which limits their application in high-performance coatings and composite materials, and the compatibility of aramid fibers with hydroxyacrylic resins is poor.
Isocyanate is introduced into the surface of aramid fiber through oxygen plasma treatment and multi-step reaction process, and reacts with hydroxyacrylic resin to enhance its interface performance. Isocyanate modified aramid fiber is added to improve the hardness and wear resistance of the resin, and at the same time, naphthalene is introduced The ring structure improves high temperature resistance.
The compatibility and mechanical properties of aramid fiber and hydroxyacrylic resin are significantly improved, the wear resistance and high temperature resistance of the resin are enhanced, and the thermal decomposition temperature and high temperature mass residual rate are improved.
Smart Images

Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of acrylic resins, in particular to a high temperature resistant hydroxy acrylic resin and a preparation process. Background Art
[0002] Acrylic resin is a common polymer material with important applications in coatings, inks, photocurable resins, etc. Acrylic resin is usually polymerized from monomers such as acrylates. By adding hydroxyethyl acrylate, styrene, fluorine-containing monomers, etc. during the polymerization process, hydroxy acrylates, styrene-acrylic resins, fluorine-containing acrylic resins, etc. with excellent performance can be obtained. Among them, hydroxy acrylates have good curing properties, high weather resistance and yellowing resistance, and are widely used. However, traditional hydroxy acrylates have disadvantages such as low strength and poor high temperature resistance, which limit their practical applications in high-performance coatings, composite materials, etc.
[0003] Adding fibers, such as glass fibers, carbon fibers, cellulose nanofibers, etc., to acrylic resin can achieve enhanced modification of acrylic resin. Aramid fiber is a polyaromatic amide synthetic fiber with the advantages of good chemical stability, high mechanical strength, high modulus, and strong high temperature resistance. It is widely used in polymer resin materials. The key is to modify the surface of aramid fiber and improve its compatibility with the resin matrix. The Chinese patent with authorization announcement number CN105908483B discloses a method for surface grafting modification of aramid fiber, in which the aramid fiber is subjected to low-temperature plasma surface treatment and then grafted with glyoxal and chitosan. After modification, the bonding force between the aramid fiber and the matrix resin is greatly improved, and the tensile strength and other properties of the resin material are enhanced. This patent does not improve the wear resistance and high temperature resistance of the matrix resin material. Summary of the invention
[0004] The invention solves the problem of poor compatibility between aramid fiber and hydroxy acrylic resin, and simultaneously improves the high temperature resistance and mechanical strength of the hydroxy acrylic resin.
[0005] The technical scheme of the present invention is: a preparation process of a high temperature resistant hydroxy acrylic resin, the preparation process comprising: adding 1-12 parts by weight of isocyanate modified aramid fiber to toluene and butyl acetate solvent, ultrasonically dispersing, then adding 100 parts by weight of hydroxy acrylic resin, 0.5-0.7 parts by weight of defoamer, 0.3-0.5 parts by weight of wetting and leveling agent, shearing and dispersing, to obtain a high temperature resistant hydroxy acrylic resin;
[0006] The preparation process of the isocyanate modified aramid fiber is as follows:
[0007] Step (1), washing the aramid fiber with deionized water and acetone in sequence, and placing it in a reaction chamber of a cold plasma treatment instrument after drying, controlling the vacuum degree to 20-40 Pa, and setting the power to 200-300 W; introducing oxygen at a flow rate of 20-50 mL / min, and performing oxygen plasma treatment for 5-10 min to obtain oxidatively modified aramid fiber;
[0008] Step (2), adding the oxidatively modified aramid fiber to thionyl chloride, heating to 60-70° C., stirring for reaction for 3-5 hours, filtering, washing with acetone, and drying to obtain acyl chloride modified aramid fiber;
[0009] Step (3), adding the acylation-modified aramid fiber to dichloromethane, ultrasonically dispersing, then adding 1,5-naphthalenediamine and triethylamine, stirring and reacting at 20-30° C. for 12-18 hours, filtering, washing with dichloromethane, and drying to obtain the naphthylamine-modified aramid fiber;
[0010] Step (4), add the naphthylamine modified aramid fiber to toluene, disperse it by ultrasonication, then add hexamethylene diisocyanate, raise the temperature to 60-75°C, stir and react for 12-24h, filter, wash with toluene, and dry to obtain isocyanate modified aramid fiber. The preparation reaction route is as follows:
[0011] ;
[0012] Furthermore, in step (2), the mass ratio of the oxidatively modified aramid fiber to thionyl chloride is 1:(40-50).
[0013] Furthermore, in the step (3), the mass ratio of the chlorinated modified aramid fiber, 1,5-naphthalenediamine, and triethylamine is 1:(4-15):(2.6-10).
[0014] Furthermore, in the step (4), the mass ratio of the naphthylamine-modified aramid fiber to hexamethylene diisocyanate is 1:(3.2-12).
[0015] The high temperature resistant hydroxy acrylic resin obtained by the preparation process described in any one of the above items.
[0016] The beneficial effects of the present invention are as follows: the aramid fiber is treated with oxygen plasma to introduce carboxyl groups on the surface, and then treated with thionyl chloride to remove acyl chloride groups, and then reacted with 1,5-naphthalenediamine to obtain naphthylamine-modified aramid fiber, and finally the introduced amino group reacted with hexamethylene diisocyanate to obtain isocyanate-modified aramid fiber, thereby realizing the introduction of active isocyanate groups and naphthalene ring structures on the surface of the aramid fiber.
[0017] The present invention adds isocyanate-modified aramid fiber to the hydroxy acrylic resin. During the curing process, the isocyanate group reacts with the hydroxyl group of the hydroxy acrylic resin. Through chemical bonding, the interface performance between the aramid fiber and the hydroxy acrylic resin is enhanced, the compatibility of the two is better, the dispersibility of the aramid fiber in the acrylic resin is improved, and the aramid fiber significantly improves the hardness, wear resistance and tensile properties of the hydroxy acrylic resin.
[0018] The aramid fiber of the present invention has strong high temperature resistance in itself, and at the same time, a naphthalene ring structure resistant to thermal decomposition is introduced on its surface. After reacting with the hydroxy acrylic resin, the naphthalene ring structure is introduced into the acrylic resin, which further improves its high temperature resistance and has a higher thermal decomposition temperature and high temperature mass residual rate. DETAILED DESCRIPTION
[0019] The embodiments of the present invention will be described in detail below with reference to examples, but those skilled in the art will appreciate that the following examples are only used to illustrate the present invention and should not be construed as limiting the scope of the present invention.
[0020] Embodiment 1: The preparation process of the high temperature resistant hydroxy acrylic resin comprises the following steps:
[0021] (1) The short-cut aramid fiber (length 3 mm) was washed with deionized water and acetone in turn, and after drying, it was placed in the reaction chamber of the cold plasma treatment instrument, the vacuum degree was controlled to 40 Pa, and the power was set to 300 W; oxygen was introduced at a flow rate of 40 mL / min, and oxygen plasma treatment was performed for 8 minutes to obtain oxidatively modified aramid fiber;
[0022] (2) Add 10 g of oxidatively modified aramid fiber to 100 mL of thionyl chloride, heat to 60 ° C, stir and react for 4 h, filter, wash with acetone, and dry to obtain acyl chloride modified aramid fiber;
[0023] (3) Add 5 g of acylation-modified aramid fiber to 500 mL of dichloromethane, disperse by ultrasonication, then add 75 g of 1,5-naphthalenediamine and 50 g of triethylamine, stir and react at 30 °C for 12 h, filter, wash with dichloromethane, and dry to obtain naphthylamine-modified aramid fiber;
[0024] (4) Add 5 g of naphthylamine-modified aramid fiber to 500 mL of toluene, disperse by ultrasonication, then add 60 g of hexamethylene diisocyanate, heat to 70 °C, stir and react for 24 h, filter, wash with toluene, and dry to obtain isocyanate-modified aramid fiber;
[0025] (5) Add 5 g of isocyanate-modified aramid fiber to 300 mL of toluene and 200 mL of butyl acetate solvent, disperse by ultrasonic, then add 500 g of hydroxyl acrylic resin Hongan HU8620, 2.5 g of defoaming agent Dow Corning AFE-1247, and 1.7 g of wetting and leveling agent Lencolo 3245, and disperse by shear to obtain a high temperature resistant hydroxyl acrylic resin.
[0026] Embodiment 2: The preparation process of the high temperature resistant hydroxy acrylic resin comprises the following steps:
[0027] (1) The short-cut aramid fiber (length 3 mm) was washed with deionized water and acetone in turn, and after drying, it was placed in the reaction chamber of the cold plasma treatment instrument, the vacuum degree was controlled to 20 Pa, and the power was set to 200 W; oxygen was introduced at a flow rate of 20 mL / min, and oxygen plasma treatment was performed for 10 min to obtain oxidatively modified aramid fiber;
[0028] (2) Add 10 g of oxidatively modified aramid fiber to 80 mL of thionyl chloride, heat to 60 °C, stir and react for 5 h, filter, wash with acetone, and dry to obtain acyl chloride modified aramid fiber;
[0029] (3) Add 5 g of acylation-modified aramid fiber to 400 mL of dichloromethane, disperse by ultrasonication, then add 48 g of 1,5-naphthalenediamine and 32 g of triethylamine, stir and react at 20 °C for 18 h, filter, wash with dichloromethane, and dry to obtain naphthylamine-modified aramid fiber;
[0030] (4) Add 5 g of naphthylamine-modified aramid fiber to 400 mL of toluene, disperse by ultrasonication, then add 35 g of hexamethylene diisocyanate, heat to 60 °C, stir and react for 24 h, filter, wash with toluene, and dry to obtain isocyanate-modified aramid fiber;
[0031] (5) Add 30 g of isocyanate modified aramid fiber to 300 mL of toluene and 200 mL of butyl acetate solvent, disperse by ultrasonic, then add 500 g of hydroxyl acrylic resin Hongan HU8620, 2.5 g of defoaming agent Dow Corning AFE-1247, and 2.5 g of wetting and leveling agent Lencolo 3245, and disperse by shear to obtain a high temperature resistant hydroxyl acrylic resin.
[0032] Embodiment 3: The preparation process of the high temperature resistant hydroxy acrylic resin comprises the following steps:
[0033] (1) The short-cut aramid fiber (length 3 mm) was washed with deionized water and acetone in turn, and after drying, it was placed in the reaction chamber of the cold plasma treatment instrument, the vacuum degree was controlled to 30 Pa, and the power was set to 300 W; oxygen was introduced at a flow rate of 50 mL / min, and oxygen plasma treatment was performed for 5 minutes to obtain oxidatively modified aramid fiber;
[0034] (2) Add 10 g of oxidatively modified aramid fiber to 80 mL of thionyl chloride, heat to 70 °C, stir and react for 3 h, filter, wash with acetone, and dry to obtain acyl chloride modified aramid fiber;
[0035] (3) Add 5 g of acyl chloride modified aramid fiber to 350 mL of dichloromethane, disperse by ultrasonication, then add 20 g of 1,5-naphthalenediamine and 13 g of triethylamine, stir and react at 25 °C for 12 h, filter, wash with dichloromethane, and dry to obtain naphthylamine modified aramid fiber;
[0036] (4) Add 5 g of naphthylamine-modified aramid fiber to 300 mL of toluene, disperse by ultrasonication, then add 16 g of hexamethylene diisocyanate, heat to 75 °C, stir and react for 12 h, filter, wash with toluene, and dry to obtain isocyanate-modified aramid fiber;
[0037] (5) Add 60 g of isocyanate-modified aramid fiber to 300 mL of toluene and 200 mL of butyl acetate solvent, disperse by ultrasonic, then add 500 g of hydroxyl acrylic resin Hongan HU8620, 3.5 g of defoaming agent Dow Corning AFE-1247, and 1.5 g of wetting and leveling agent Lencolo 3245, and disperse by shear to obtain a high temperature resistant hydroxyl acrylic resin.
[0038] Comparative Example 1: A process for preparing a high temperature resistant hydroxy acrylic resin, comprising the following steps:
[0039] (1) Add 500 g of hydroxyl acrylic resin Hongan HU8620, 2.5 g of defoaming agent Dow Corning AFE-1247, and 1.7 g of wetting and leveling agent Lencolo 3245 to 300 mL of toluene and 200 mL of butyl acetate solvent, and shear and disperse to obtain a high temperature resistant hydroxyl acrylic resin.
[0040] Comparative Example 2: A process for preparing a high temperature resistant hydroxy acrylic resin, comprising the following steps:
[0041] (1) Add 5 g of short-cut aramid fiber (length 3 mm) to 300 mL of toluene and 200 mL of butyl acetate solvent, disperse by ultrasonic, then add 500 g of hydroxyl acrylic resin Hongan HU8620, 2.5 g of defoaming agent Dow Corning AFE-1247, and 1.7 g of wetting and leveling agent Lencolo 3245, and disperse by shear to obtain a high temperature resistant hydroxyl acrylic resin.
[0042] Comparative Example 3: A process for preparing a high temperature resistant hydroxy acrylic resin, comprising the following steps:
[0043] (1) Add 5 g of oxidized modified aramid fiber to 300 mL of toluene and 200 mL of butyl acetate solvent, disperse by ultrasonic, then add 500 g of hydroxyl acrylic resin Hongan HU8620, 2.5 g of defoaming agent Dow Corning AFE-1247, and 1.7 g of wetting and leveling agent Lencolo 3245, and disperse by shear to obtain a high temperature resistant hydroxyl acrylic resin.
[0044] Comparative Example 4: A process for preparing a high temperature resistant hydroxy acrylic resin, comprising the following steps:
[0045] (1) Add 5 g of naphthylamine-modified aramid fiber to 300 mL of toluene and 200 mL of butyl acetate solvent, disperse by ultrasonic, then add 500 g of hydroxyl acrylic resin Hongan HU8620, 2.5 g of defoaming agent Dow Corning AFE-1247, and 1.7 g of wetting and leveling agent Lencolo 3245, and disperse by shear to obtain a high temperature resistant hydroxyl acrylic resin.
[0046] The high temperature resistant hydroxyl acrylic resin was cured at 80°C for 6 hours to form a paint film.
[0047] The wear resistance of the paint film was tested in an abrasion tester according to GB / T 1768-2006 standard, with a grinding wheel load of 1000g, a rotation speed of 200r / min, and a revolution of 1000r, and the mass loss before and after wear was measured.
[0048] The hardness of the paint film is measured by the pencil method in accordance with GB / T 6739-2022.
[0049] The tensile properties of the high temperature resistant hydroxyl acrylic resin cured film were tested according to GB / T 1040.1-2018 standard using an electronic tensile testing machine at a tensile rate of 50 mm / min. The test results are shown in Table 1.
[0050] Table 1: Test results of various embodiments and comparative examples
[0051]
[0052] The thermal properties of the film were tested in a thermogravimetric analyzer under a nitrogen atmosphere by heating the temperature to 800°C at a heating rate of 10°C / min.
[0053] The test results are shown in Table 2.
[0054] Table 2: Test results of various embodiments and comparative examples
[0055]
[0056] As can be seen from the above table, the mass wear of the hydroxy acrylic resin film of Example 1-Example 3 is only 22.0-36.5mg, the hardness reaches 4-5H, the tensile strength of the film reaches 9.7-15.5MPa, and the elongation at break reaches 479.6-565.3, which has excellent wear resistance, hardness and tensile properties. At the same time, the 5% mass loss temperature reaches 298.5-312.4℃, and the 5% mass loss temperature reaches 351.0-362.9℃, which has excellent high temperature resistance. Mainly, naphthylamine-modified aramid fiber is added, and aramid fiber has the advantages of high strength, strong high temperature resistance, excellent wear resistance, etc., and isocyanate groups are introduced on the surface. During the curing process, the isocyanate groups react with the hydroxyl groups of the hydroxy acrylic resin, and the interface performance between the aramid fiber and the hydroxy acrylic resin is enhanced through chemical bonding, and the compatibility of the two is better, which improves the dispersibility of the aramid fiber in the acrylic resin, so that the aramid fiber significantly improves the hardness, wear resistance and tensile properties of the hydroxy acrylic resin. In addition, aramid fiber itself has strong high temperature resistance. At the same time, a naphthalene ring structure that resists thermal decomposition is introduced on its surface. After reacting with hydroxy acrylic resin, the naphthalene ring structure is introduced into the acrylic resin, which further improves its high temperature resistance and has a higher thermal decomposition temperature and high temperature mass residue rate.
[0057] In Comparative Example 1, no naphthylamine-modified aramid fiber was added, and the hardness, abrasion resistance and tensile properties of the hydroxy acrylic resin were relatively low, and the thermal decomposition temperature was low, and the high temperature resistance was relatively poor.
[0058] The main difference between Comparative Example 2 and Example 1 is that ordinary unmodified aramid fiber is added. Due to the poor compatibility between aramid fiber and hydroxy acrylic resin, the dispersion of aramid fiber in the resin matrix is not good, the reinforcement effect on acrylic resin is not good, the hardness, wear resistance and tensile properties are low, the thermal decomposition temperature is low, and the high temperature resistance is poor.
[0059] The main difference between Comparative Example 3 and Example 1 is that oxidatively modified aramid fiber is added. The aramid fiber is treated with oxygen plasma and contains groups such as carboxyl groups on its surface, which improves the interface performance and compatibility with the hydroxy acrylic resin, which is beneficial to enhancing the mechanical properties such as hardness of the acrylic resin, as well as the thermal decomposition temperature.
[0060] The main difference between Comparative Example 4 and Example 1 is that after adding naphthylamine-modified aramid fiber and introducing organic functional groups on the surface of the aramid fiber, the interfacial performance and compatibility with the hydroxy acrylic resin are further improved, and its mechanical properties such as hardness and thermal decomposition temperature are significantly improved. However, the negative aramid fiber does not contain isocyanate groups and cannot react with the hydroxy acrylic resin. The interfacial performance between the two is lower than that in Example 1, resulting in the reinforcement effect of the aramid fiber being weaker than that in Example 1.
[0061] It can be understood that the above specific description of the present invention is only used to illustrate the present invention and is not limited to the technical solutions described in the embodiments of the present invention. Those skilled in the art should understand that the present invention can still be modified or replaced by equivalents to achieve the same technical effects; as long as the use requirements are met, they are within the protection scope of the present invention.
Claims
1. Preparation process of high temperature resistant hydroxy acrylic resin, It is characterized in that The preparation process comprises: adding 1-12 parts by weight of isocyanate-modified aramid fiber to toluene and butyl acetate solvents, performing ultrasonic dispersion, and then adding 100 parts by weight of hydroxy acrylic resin, 0.5-0.7 parts by weight of defoamer, and 0.3-0.5 parts by weight of wetting and leveling agent, performing shear dispersion, and obtaining a high temperature resistant hydroxy acrylic resin; The preparation process of the isocyanate modified aramid fiber is as follows: Step (1), washing the aramid fiber with deionized water and acetone in sequence, placing the fiber in a reaction chamber of a cold plasma treatment apparatus after drying, introducing oxygen, and performing oxygen plasma treatment to obtain an oxidatively modified aramid fiber; Step (2), adding the oxidatively modified aramid fiber to thionyl chloride, stirring for reaction, filtering, washing, and drying to obtain acyl chloride modified aramid fiber; Step (3), adding the acylation-modified aramid fiber into dichloromethane, ultrasonically dispersing, then adding 1,5-naphthalenediamine and triethylamine, stirring for reaction, filtering, washing, and drying to obtain the naphthylamine-modified aramid fiber; Step (4), adding the naphthylamine modified aramid fiber into toluene, ultrasonically dispersing, then adding hexamethylene diisocyanate, stirring for reaction, filtering, washing, and drying to obtain isocyanate modified aramid fiber.
2. The preparation process of the high temperature resistant hydroxy acrylic resin according to claim 1, It is characterized in that In the step (1), the vacuum degree in the reaction chamber is 20-40 Pa; the power is set to 200-300 W, the flow rate of oxygen is 20-50 mL / min, and the oxygen plasma treatment time is 5-10 min.
3. The preparation process of the high temperature resistant hydroxy acrylic resin according to claim 1, It is characterized in that In the step (2), the mass ratio of the oxidatively modified aramid fiber to thionyl chloride is 1:(40-50).
4. The preparation process of the high temperature resistant hydroxy acrylic resin according to claim 1, It is characterized in that The reaction temperature in step (2) is 60-70° C. and the reaction time is 3-5 h.
5. The preparation process of the high temperature resistant hydroxy acrylic resin according to claim 1, It is characterized in that In the step (3), the mass ratio of the chlorinated modified aramid fiber, 1,5-naphthalenediamine, and triethylamine is 1:(4-15):(2.6-10).
6. The preparation process of the high temperature resistant hydroxy acrylic resin according to claim 1, It is characterized in that The reaction temperature in step (3) is 20-30°C and the reaction time is 12-18h.
7. The preparation process of the high temperature resistant hydroxy acrylic resin according to claim 1, It is characterized in that In the step (4), the mass ratio of naphthylamine-modified aramid fiber to hexamethylene diisocyanate is 1:(3.2-12).
8. The preparation process of the high temperature resistant hydroxy acrylic resin according to claim 1, It is characterized in that The reaction temperature in step (4) is 60-75°C and the reaction time is 12-24h.
9. The high temperature resistant hydroxy acrylic resin obtained by the preparation process according to any one of claims 1 to 8.