Molybdenum oxynitride rotating target material, preparation method thereof and solar cell

Through the combination of nano-MoO2 powder and micro-MoO2 powder, MoN powder, Mo powder and spray granulation technology, the problem of difficult control of the element content of molybdenum oxide films is solved, and the stability of solar cells and the photogenerated carrier separation effect are improved. Extends the battery life.

CN118835205BActive Publication Date: 2024-11-26SHENZHEN APG MATERIAL TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411314638.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-20
Publication Date
2024-11-26
Estimated Expiration
2044-09-20

AI Technical Summary

Technical Problem

The existing preparation methods for molybdenum oxide films are difficult to accurately control the content of each element in the molybdenum oxide films, which affects the quality and stability of solar cell products.

Method used

NanoMoO2 powder is prepared into nanomoO2 slurry and mixed with micromoO2 powder, MoN powder and Mo powder. After isostatic molding, calcining, ball milling and spray granulation, it forms a rotating target of molybdenum nitrogen oxide to accurately regulate N and O. The stoichiometric ratio to Mo improves the stability and performance of the coating.

Benefits of technology

The precise control of the proportion of each element in the rotary target of molybdenum oxide is achieved, the stability of the coating and the photogenerated carrier separation effect are improved, and the service life of solar cells is extended.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118835205B_ABST
    Figure CN118835205B_ABST
Patent Text Reader

Abstract

The present application relates to the technical field of target material preparation, and provides a molybdenum oxynitride rotary target material and a preparation method thereof and a solar cell, including: mixing nano MoO2 slurry and micron MoO2 powder, MoN powder, and Mo powder, isostatically pressing, and then crushing and sieving to obtain a mixed powder; calcining the mixed powder to obtain a calcined powder; ball milling the calcined powder, a binder, a dispersant, and water to obtain a mixed slurry; spraying the mixed slurry to obtain a granulated powder; degreasing the granulated powder, and then sieving to obtain a spray powder; spraying the spray powder onto a back tube, and then machining to obtain a molybdenum oxynitride rotary target material. The preparation method of the molybdenum oxynitride rotary target material provided by the present application, because the nano MoO2 powder and the micron MoO2 powder, MoN powder, and Mo powder are formed, crushed, calcined, and then granulated and sprayed, the composition of the obtained target material is closer to the raw material ratio, the organization is more uniform, and the density is higher.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of target material preparation, and in particular relates to a molybdenum oxynitride rotating target material, a preparation method thereof, and a solar cell. Background Art

[0002] MoO x It has the advantages of being non-toxic and having a high work function, and is widely used as a hole-selective contact layer material for perovskite solar cells and crystalline silicon heterojunction solar cells. However, its work function is greatly affected by the water and oxygen environment, and it easily reacts with adjacent metal layers, causing the stability of the battery to gradually decrease after a period of use. In contrast, molybdenum oxynitride has more stable chemical properties and better conductivity, and can be used as a potential application material for hole-selective contact layers.

[0003] At present, the preparation process of molybdenum oxynitride film mainly uses molybdenum target as sputtering target, high-purity argon as working gas, nitrogen and oxygen as reaction gas, and adjusts the content of each element in the molybdenum oxynitride film by controlling the ratio of the three gases. However, it is very difficult to accurately control the ratio of reaction gas in the cavity, which not only makes it difficult to accurately control the content of each element in the molybdenum oxynitride film, but also affects the sputtering reaction rate, making the entire reaction process more complicated and difficult to control, thereby affecting the quality of solar cell products. In addition, if a molybdenum oxynitride film with a high oxygen content or a high nitrogen content is to be prepared, a large amount of oxygen or nitrogen needs to be introduced, which is easy to affect the smooth progress of coating, and it is even more difficult to accurately control the content of each element in the molybdenum oxynitride film. Summary of the invention

[0004] The purpose of the present application is to provide a molybdenum oxynitride rotating target material, a preparation method thereof and a solar cell, aiming to solve the problem that it is difficult to accurately control the content of each element in the molybdenum oxynitride film in the existing preparation method of the molybdenum oxynitride film.

[0005] In order to achieve the above application purpose, the technical solution adopted in this application is as follows:

[0006] In a first aspect, the present application provides a method for preparing a molybdenum oxynitride rotary target, comprising the following steps:

[0007] Nano-MoO 2 Powder is prepared into nano MoO 2 Slurry;

[0008] The nano MoO 2 Slurry and micronized MoO 2 powder, MoN powder and Mo powder are mixed to obtain a mixed material;

[0009] isostatically pressing the mixed material, and then crushing and sieving to obtain mixed powder;

[0010] calcining the mixed powder to obtain calcined powder;

[0011] The calcined powder, binder, dispersant and water are mixed by ball milling to obtain a mixed slurry;

[0012] The mixed slurry is spray-granulated to obtain granulated powder;

[0013] Degreasing the granulated powder and then sieving it to obtain spray powder;

[0014] The spray powder is sprayed onto a back tube by using a plasma spraying device, and then the molybdenum oxynitride rotary target is obtained by machining.

[0015] In a second aspect, the present application provides a molybdenum oxynitride rotary target, including a molybdenum oxynitride rotary target prepared by the method for preparing the molybdenum oxynitride rotary target provided in the present application;

[0016] Wherein, the atomic ratio of N, O and Mo in the molybdenum oxynitride rotating target is (10-19) / (30-40) / (41-60).

[0017] In a third aspect, the present application provides a solar cell, which comprises a molybdenum oxynitride thin film obtained by sputtering the molybdenum oxynitride rotating target provided by the present application.

[0018] Compared with the prior art, this application has the following beneficial effects:

[0019] (1) Nano-MoO 2 The slurry plays a bonding role, promoting the micron MoO 2 The mixture of powder, MoN powder and Mo powder is molded to make micron MoO 2 The powder, MoN powder and Mo powder are more closely combined in the physical space, so that the micron MoO 2 The powder, MoN powder and Mo powder are more likely to contact and form a sintering neck, so that the atoms can migrate to the sintering neck area by diffusion to form a more compact calcined powder, which can prevent the calcined powder from MoO2 in the subsequent ball milling process. 2 , MoN and Mo are dispersed, thus preventing the granulation process from forming "hollow" granulated powder, so that high fluidity, high uniformity and high density granulated powder can be formed, thereby improving the density of the target material;

[0020] (2) Directly converting MoO 2 Compared with the conventional method of ball-milling powder, MoN powder and Mo powder to form a slurry, and then spraying granulation, the present invention uses nano MoO 2 The slurry as a binder combined with calcination can solve the problem of MoO 2The large density difference between MoN powder and Mo powder easily causes the slurry to be delaminated, so the obtained slurry is more uniform and stable, thus making MoO 2 , MoN and Mo are evenly distributed in each granulated powder, so that the powder can maintain a relatively consistent flying state during the subsequent spraying process, making the composition of the molybdenum oxynitride rotating target obtained by spraying closer to the raw material ratio and the organizational uniformity is better;

[0021] (3) The added Mo powder can, on the one hand, precisely control the stoichiometric ratio of N, O and Mo in the molybdenum oxynitride rotating target, adjust the target coating work function to match the silicon valence band, and make it more effective in extracting holes and blocking electrons, thus making it more suitable as a hole-selective contact layer material; on the other hand, it can also improve the deposition rate of the spray powder and improve the utilization rate of raw materials;

[0022] (4) The spraying process does not require long-term high-temperature sintering, effectively preventing MoO 2 Volatilization makes the composition of the target material prepared by the present application closer to the raw material ratio, so that the ratio of each element in the molybdenum oxynitride rotating target can be accurately controlled, so that its coating can give full play to the dual advantages of molybdenum oxide film and molybdenum nitride film, so that it can remain stable for a long time in a water and oxygen environment, and have good ability to extract holes and block electrons, so that the photogenerated carrier separation effect is good and the battery efficiency is high. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0024] Figure 1 is a process flow chart of a method for preparing a molybdenum oxynitride rotary target provided in an embodiment of the present application;

[0025] Figure 2 This is a physical picture of the molybdenum oxynitride rotating target provided in the embodiment of the present application. DETAILED DESCRIPTION

[0026] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present application more clearly understood, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.

[0027] A first aspect of an embodiment of the present application provides a method for preparing a molybdenum oxynitride rotary target, comprising the following steps:

[0028] S01: Nano-MoO 2 Powder is prepared into nano MoO 2 Slurry;

[0029] S02: Nano-MoO 2 Slurry and micronized MoO 2 powder, MoN powder and Mo powder are mixed to obtain a mixed material;

[0030] S03: isostatically pressing the mixed material, and then crushing and sieving to obtain mixed powder;

[0031] S04: calcining the mixed powder to obtain calcined powder;

[0032] S05: ball-milling the calcined powder, the binder, the dispersant and water to obtain a mixed slurry;

[0033] S06: spray granulating the mixed slurry to obtain granulated powder;

[0034] S07: Degreasing the granulated powder and then sieving it to obtain spray powder;

[0035] S08: Spraying the spray powder onto the back tube by using a plasma spraying device, and then machining to obtain a molybdenum oxynitride rotary target.

[0036] In the above step S01, nano MoO 2 Powder is prepared into nano MoO 2 The slurry step includes: adding nano MoO 2 The powder was added to water and ball-milled to obtain nano MoO 2 Slurry.

[0037] In the above step S02, nano MoO 2 Powder, micron MoO 2 The powder, MoN powder and Mo powder satisfy the atomic ratio of N, O and Mo of (10-19) / (30-40) / (41-60), so that the atomic ratio of N, O and Mo in the prepared molybdenum oxynitride rotating target can meet (10-19) / (30-40) / (41-60), which can not only make the molybdenum oxynitride rotating target coating remain stable for a long time in a water and oxygen environment, but also have good effects of extracting holes and blocking electrons; at the same time, the Mo powder content is also helpful to improve the deposition rate of the spray powder, thereby improving the utilization rate of raw materials.

[0038] In the embodiment, nano MoO 2 Nano MoO 2 Powder, micron MoO 2 The total weight of MoO powder, MoN powder and Mo powder is 2-7%. 2 The content range of powder can be well2 Powder, MoN powder and Mo powder are bonded to form by static pressure, which can ensure low cost.

[0039] In practical applications, the ratio of each element in the molybdenum oxynitride rotating target material to be prepared as required, as well as the nano MoO 2 The powder ratio can be converted to obtain nano MoO 2 Powder, micron MoO 2 The mass ratio of Mo powder, MoN powder and Mo powder.

[0040] In the embodiment, micron MoO 2 The particle sizes of powder, MoN powder and Mo powder are 1~2μm, 1~2μm and 4~6μm respectively. This powder particle size range is conducive to MoO 2 The powder and MoN powder are filled into the gaps of Mo powder, so that the powder has a higher packing density in the natural state, which is helpful for static pressure molding and makes the powder more tightly combined in the physical space. 2 Powder, MoN powder and Mo powder are more likely to contact to form a sintering neck, so that atoms can migrate to the sintering neck area by diffusion to form a more compact and uniform calcined powder.

[0041] In practical applications, you can directly purchase micron MoO with particle sizes of 1~2μm, 1~2μm, and 4~6μm. 2 Powder, MoN powder, Mo powder. Of course, in order to reduce costs, you can also buy MoO powder with larger particle size. 2 Powder, MoN powder, Mo powder, such as 10~20μm, by crushing, MoO 2 The particle sizes of Ag powder, MoN powder and Mo powder are 1~2μm, 1~2μm and 4~6μm respectively.

[0042] In the above step S03, due to the presence of micron MoO 2 The powder, MoN powder and Mo powder are relatively loosely stacked, so the mixed material is subjected to isostatic pressing to make the powders more tightly combined in the physical space, and then crushed and sieved, such as through a 60-100 mesh sieve, to obtain a mixed powder. Among them, the particle size of the mixed powder is 150-250μm, which can ensure that the micron MoO 2 The powder, MoN powder and Mo powder are tightly bonded together, which can ensure that the mixed powder has a higher sintering activity, and is conducive to atomic diffusion and migration during calcination to form a more compact calcined powder.

[0043] In the above step S04, the mixed powder is placed in a protective atmosphere of argon gas, a pressure of 0.01-0.05 MPa, and a temperature of 1000-1300°C for sealed calcination for 4-6 hours. If the calcination temperature is too low and the time is too short, it is difficult to form nano MoO2 Powder, micron MoO 2 The calcination of powder, MoN powder and Mo powder to form dense and uniform calcined powder is not conducive to the subsequent ball milling mixing to form a uniform and stable slurry, which will affect the final target material composition, uniformity and density; if the calcination temperature is too high and the time is too long, it is easy to cause MoO 2 The powder volatilization will affect the ratio of each element in the final molybdenum oxynitride rotating target, causing the atomic ratio of the target to deviate from the raw material ratio; therefore, the calcination conditions of this embodiment are conducive to the nano MoO 2 Powder, micron MoO 2 Powder, MoN powder, and Mo powder are calcined to form a dense, uniform solid solution, which can also prevent MoO 2 The powder is volatilized, so that the ratio of each element in the final molybdenum oxynitride rotary target is closer to the ratio of the raw materials and the density is higher.

[0044] In the above step S05, due to the nano MoO 2 Slurry, micron MoO 2 After the powder, MoN powder and Mo powder are calcined, these materials are pre-sintered and combined together to make the particles grow. Therefore, by ball milling the calcined powder, binder, dispersant and water, the calcined powder can be broken up to facilitate spray granulation, and the solid particles after ball milling can be evenly distributed with MoO 2 , MoN and Mo, thereby forming a granulated powder with uniform structure and high fluidity, which is beneficial to improving the structural uniformity of the target material.

[0045] In the embodiment, the amount of binder added is nano MoO 2 Powder, micron MoO 2 The amount of dispersant added is 0.5~1% of the total mass of nano MoO 2 Powder, micron MoO 2 The total mass of Mo powder, MoN powder and Mo powder is 0.5~1%.

[0046] In an embodiment, the binder is selected from polyvinyl alcohol; and the dispersant is selected from polyethylene glycol.

[0047] In the embodiment, the solid content of the slurry is 60-70%.

[0048] In the above step S06, the inlet temperature of the spray granulation is 200-250°C, and the outlet temperature is 80-100°C.

[0049] In the above step S07, the step of degreasing the granulated powder includes: placing the granulated powder in a vacuum sintering furnace, evacuating the vacuum to 10 -2 Pa, then heat to 400~600℃ and keep warm for 6~18h.

[0050] In the embodiment, the fluidity of the spray powder is 50-60 s / 50g.

[0051] In the above step S08, the plasma spraying equipment includes a back tube and a spray gun, and the distance from the spray gun to the central axis of the back tube is 90~120mm. If the distance between the spray gun and the central axis of the back tube is too long, the speed of the particles will be reduced, the kinetic energy will be reduced, and the bonding strength between the coatings and the coating and the back tube will be reduced, which will eventually affect the density and strength of the target material obtained by spraying; if the distance between the spray gun and the central axis of the back tube is too short, the speed of the particles will be too large, which will easily cause powder splashing and reduce the deposition rate of the spray powder. Therefore, within the scope of this embodiment, the spray powder has a high deposition rate, high target density and high mechanical strength. The moving speed of the spray gun is 20~80mm / min. This moving speed range allows the spray powder to be sprayed more evenly on the back tube, and the spray coating will not be too thick in some areas, thereby affecting the bonding strength between the coatings and the coating and the back tube. The powder feeding amount is 60~300g / min. This powder feeding amount range can ensure a higher spraying efficiency while also facilitating the spray powder to be evenly sprayed onto the back tube to form a uniform and dense target material.

[0052] In the embodiment, the rotation speed of the back tube is 200-300 r / min. In this rotation speed range, the spray powder is sprayed on the back tube more evenly, and the coating is not too thick in some areas, thereby affecting the bonding strength between the coatings and between the coating and the back tube. The temperature of the back tube surface is 50-90°C.

[0053] Therefore, the method for preparing the molybdenum oxynitride rotating target provided in the embodiment of the present application comprises adding nano MoO 2 Nano MoO powder 2 The slurry plays a bonding role, promoting the micron MoO 2 The mixture of powder, MoN powder and Mo powder is molded to make micron MoO 2 The powder, MoN powder and Mo powder are more closely combined in the physical space, so that the micron MoO 2 The powder, MoN powder and Mo powder are more likely to contact and form a sintering neck, so that the atoms can migrate to the sintering neck area by diffusion to form a more compact calcined powder, which can prevent the calcined powder from MoO 2 , MoN and Mo are dispersed, so that the solid particles after ball milling are evenly distributed with MoO 2, MoN and Mo, to avoid the formation of "hollow" granulated powder by spray granulation, so that the obtained granulated powder has better fluidity, more uniform and denser organizational structure. Therefore, the granulated powder can maintain a relatively consistent flying state during the spraying process after degreasing, so that the ratio of each element in the obtained molybdenum oxynitride rotating target is closer to the raw material ratio, with better organizational uniformity and higher density. Secondly, the added Mo powder can not only accurately control the stoichiometric ratio of N, O and Mo in the molybdenum oxynitride rotating target, and adjust the target coating work function to match the silicon valence band, so that it can better extract holes and block electrons, making it more suitable as a hole selection contact layer material, but also improve the deposition rate of the spray powder and improve the utilization rate of raw materials. In addition, the spraying process does not require high-temperature sintering, which effectively prevents MoO 2 Volatilization, so the composition of the prepared target material is closer to the raw material ratio.

[0054] A second aspect of the embodiments of the present application provides a molybdenum oxynitride rotary target, including a molybdenum oxynitride rotary target prepared by the method for preparing the molybdenum oxynitride rotary target provided in the above embodiments;

[0055] Among them, the atomic ratio of N, O and Mo in the molybdenum oxynitride rotating target is (10~19) / (30~40) / (41~60).

[0056] The molybdenum oxynitride rotary target provided in the embodiment of the present application includes the molybdenum oxynitride rotary target prepared by the preparation method of the molybdenum oxynitride rotary target provided in the present application, so the ratio of each element in the target is closer to the raw material ratio, the organizational uniformity is better, and the density is higher. Therefore, the ratio of N, O and Mo in the molybdenum oxynitride rotary target coating can also be precisely controlled, and the dual advantages of molybdenum oxide film (good hole extraction and electron blocking effects, but poor stability in water and oxygen environments) and molybdenum nitride film (good stability in water and oxygen environments, but poor hole extraction and electron blocking effects) can be fully utilized. It can not only maintain stability for a long time in a water and oxygen environment, but also has better hole extraction and electron blocking capabilities, so the photogenerated carrier separation effect is good.

[0057] A third aspect of the present application provides a solar cell, which comprises a molybdenum oxynitride thin film obtained by sputtering the molybdenum oxynitride rotating target provided by the present application.

[0058] The solar cell provided in the embodiment of the present application can remain stable for a long time and extend its service life because it contains the molybdenum oxynitride thin film obtained by sputtering the molybdenum oxynitride rotating target provided in the present application.

[0059] The following describes the invention in conjunction with specific embodiments.

[0060] Example 1

[0061] This embodiment provides a method for preparing a molybdenum oxynitride rotary target, comprising the following steps:

[0062] S11: According to the atomic ratio of N, O and Mo is 15 / 35 / 50, nano MoO 2 Nano MoO 2 Powder, micron MoO 2 5% of the total mass of powder, MoN powder and Mo powder, weigh an appropriate amount of nano MoO 2 Powder (D50=100nm), micron MoO 2 powder (D50=1.5μm), MoN powder (D50=1.4μm) and Mo powder (D50=5.2μm);

[0063] S12: Nano-MoO 2 The powder was added into water and mixed evenly by ball milling to form nano MoO 2 slurry; using a power mixing device to mix nano MoO 2 Slurry and micronized MoO 2 powder, MoN powder and Mo powder are uniformly mixed to obtain a mixture;

[0064] S13: isostatically pressing the mixture, crushing it, and passing it through a 60-mesh sieve and a 100-mesh sieve to obtain a mixed powder;

[0065] S14: placing the mixed material in an atmosphere sintering furnace, and sealing and calcining the mixed material for 5 hours under the conditions of argon gas as a protective atmosphere, a pressure of 0.03 MPa, and a temperature of 1200° C. to obtain calcined powder;

[0066] S15: The calcined powder, polyethylene glycol and water are mixed by ball milling, and then polyvinyl alcohol is added and mixed evenly to obtain a mixed slurry; the amount of polyethylene glycol added is 2 Powder, micron MoO 2 The amount of polyvinyl alcohol added is 0.7% of the total mass of nano-MoO 2 Powder, micron MoO 2 0.7% of the total mass of Mo powder, MoN powder and Mo powder;

[0067] S16: introducing the mixed slurry into a centrifugal spray granulator with an inlet temperature of 225° C. and an outlet temperature of 90° C. to form granulated powder;

[0068] S17: Place the granulated powder in a vacuum sintering furnace and evacuate to 5×10 -2 Pa, then heated to 500°C, degreased for 12 h, and sieved to obtain spray powder;

[0069] S18: The treated back tube is installed on the frame, and the frame drives the back tube to rotate and move axially. The spray gun is installed 100mm above the central axis of the back tube. The rotation speed of the back tube is set to 250r / min, the moving speed of the spray gun is 50mm / min, the powder feeding amount is 200g / min, and the powder feeding gas and the working gas are both inert gases. During the spraying process, water is passed into the back tube to make the temperature of the back tube surface 80℃, and a molybdenum oxynitride rotating target is obtained.

[0070] Example 2

[0071] This embodiment provides a method for preparing a molybdenum oxynitride rotary target, which is different from Embodiment 1 in that in step S14, the temperature is 1000° C. and the calcination is 6 hours.

[0072] Example 3

[0073] This embodiment provides a method for preparing a molybdenum oxynitride rotary target, which is different from Embodiment 1 in that in step S14, the temperature is 1300° C. and the calcination is 4 hours.

[0074] Example 4

[0075] This embodiment provides a method for preparing a molybdenum oxynitride rotary target, which is different from Embodiment 1 in that:

[0076] In step S11, according to the atomic ratio of N, O and Mo being 15 / 35 / 50, nano MoO 2 Nano MoO 2 Powder, micron MoO 2 2% of the total mass of powder, MoN powder and Mo powder, weigh an appropriate amount of nano MoO 2 Powder (D50=100nm), micron MoO 2 powder (D50=1.1μm), MoN powder (D50=1.0μm) and Mo powder (D50=4.2μm).

[0077] Example 5

[0078] This embodiment provides a method for preparing a molybdenum oxynitride rotary target, which is different from Embodiment 1 in that:

[0079] In step S11, according to the atomic ratio of N, O and Mo being 15 / 35 / 50, nano MoO 2 Nano MoO 2 Powder, micron MoO 2 7% of the total mass of powder, MoN powder and Mo powder, weigh an appropriate amount of nano MoO 2 Powder (D50=100nm), micron MoO 2powder (D50=2.0μm), MoN powder (D50=2.1μm) and Mo powder (D50=6.0μm).

[0080] Example 6

[0081] This embodiment provides a method for preparing a molybdenum oxynitride rotary target, which is different from Embodiment 1 in that:

[0082] In step S11, the atomic ratio of N, O and Mo is 10 / 30 / 60.

[0083] Example 7

[0084] This embodiment provides a method for preparing a molybdenum oxynitride rotary target, which is different from Embodiment 1 in that:

[0085] In step S11, the atomic ratio of N, O and Mo is 19 / 40 / 41.

[0086] Comparative Example 1

[0087] This comparative example provides a method for preparing a molybdenum oxynitride rotary target, which is different from Example 1 in that:

[0088] No addition of nano MoO 2 pink;

[0089] In step S11, according to the atomic ratio of N, O and Mo being 15 / 35 / 50, an appropriate amount of micron MoO 2 powder (D50=1.5μm), MoN powder (D50=1.4μm) and Mo powder (D50=5.2μm);

[0090] Steps S12 and S13 are replaced by: adding micron MoO 2 The Mo powder, MoN powder and Mo powder are uniformly mixed to obtain a mixed powder.

[0091] Comparative Example 2

[0092] This comparative example provides a method for preparing a molybdenum oxynitride rotary target, comprising the following steps:

[0093] S1: According to the atomic ratio of N, O and Mo being 15 / 35 / 50, weigh an appropriate amount of micron MoO 2 powder (D50 = 1.1 μm), MoN powder (D50 = 1.0 μm) and Mo powder (D50 = 4.2 μm), and then the micron MoO 2 Powder, MoN powder, Mo powder, polyethylene glycol and water are ball-milled and mixed, and then polyvinyl alcohol is added and ball-milled to mix evenly to obtain a slurry; the amount of polyethylene glycol added is micron MoO 2The total weight of MoO powder, MoN powder and Mo powder is 0.7%, and the amount of polyvinyl alcohol added is micron MoO 2 0.7% of the total mass of Mo powder, MoN powder and Mo powder;

[0094] S2: introducing the slurry into a centrifugal spray granulator with an inlet temperature of 225°C and an outlet temperature of 90°C to form granulated powder;

[0095] S3: Place the granulated powder in a vacuum sintering furnace and evacuate to 5×10 -2 Pa, then heated to 500°C, degreased for 12 h, and sieved to obtain spray powder;

[0096] S4: The treated back tube is installed on the frame, and the frame drives the back tube to rotate and move axially. The spray gun is installed 100mm above the central axis of the back tube. The rotation speed of the back tube is set to 250r / min, the moving speed of the spray gun is 50mm / min, the powder feeding amount is 200g / min, and the powder feeding gas and the working gas are both inert gases. During the spraying process, water is passed into the back tube to make the temperature of the back tube surface 80℃. Spraying is performed for 6h to obtain a molybdenum oxynitride rotating target.

[0097] Comparative Example 3

[0098] This comparative example provides a method for preparing a molybdenum oxynitride rotary target, which is different from Example 1 in that:

[0099] No Mo powder added;

[0100] In step S11, the atomic ratio of N, O and Mo is 23.75 / 35 / 41.25, and the nano MoO 2 Nano MoO 2 Powder, micron MoO 2 5% of the total mass of MoO powder and MoN powder, weigh an appropriate amount of nano MoO 2 Powder (D50=100nm), micron MoO 2 powder (D50=1.5μm) and MoN powder (D50=1.4μm).

[0101] Comparative Example 4

[0102] This comparative example provides a method for preparing a molybdenum oxynitride rotary target, which is different from Example 1 in that in step S14, the temperature is 1400° C. and the calcination is 3 h.

[0103] Comparative Example 5

[0104] This comparative example provides a method for preparing a molybdenum oxynitride rotary target, comprising the following steps:

[0105] S1: According to the atomic ratio of N, O and Mo being 15 / 35 / 50, weigh an appropriate amount of micron MoO 2 powder (D50 = 1.1 μm), MoN powder (D50 = 1.0 μm) and Mo powder (D50 = 4.2 μm), and then the micron MoO 2 Powder, MoN powder, Mo powder, polyethylene glycol and water are ball-milled and mixed, and then polyvinyl alcohol is added and ball-milled to mix evenly to obtain a slurry; the amount of polyethylene glycol added is micron MoO 2 The total weight of MoO powder, MoN powder and Mo powder is 0.7%, and the amount of polyvinyl alcohol added is micron MoO 2 0.7% of the total mass of Mo powder, MoN powder and Mo powder;

[0106] S2: introducing the slurry into a centrifugal spray granulator with an inlet temperature of 225°C and an outlet temperature of 90°C to form granulated powder;

[0107] S3: isostatically pressing the granulated powder to form a green body;

[0108] S4: Place the green body in a vacuum sintering furnace and evacuate to 10 -2 Pa, then heated to 500 ° C, degreased for 12 hours, and then sintered at 1400 ° C for 24 hours, and naturally cooled to obtain a molybdenum oxynitride rotary target.

[0109] Comparative Example 6

[0110] This embodiment provides a method for preparing a molybdenum oxynitride rotary target, comprising the following steps:

[0111] In step S11, an appropriate amount of nano MoO 2 Powder (D50=100nm), micron MoO 2 powder (D50=1.5μm), MoN powder (D50=1.5μm) and Mo powder (D50=1.5μm).

[0112] Related performance test analysis:

[0113] 1. Figure 1 The actual picture of the molybdenum oxynitride rotary target provided in Example 1, from Figure 1 It can be seen that the molybdenum oxynitride rotary target has good organizational uniformity.

[0114] 2. The O and N contents of the molybdenum oxynitride rotary targets prepared in Examples 1 to 7 and Comparative Examples 1 to 6 were respectively tested using an oxygen and nitrogen analyzer, and the Mo contents of the molybdenum oxynitride rotary targets prepared in Examples 1 to 7 and Comparative Examples 1 to 6 were respectively tested using ICP (inductively coupled plasma testing), and the atomic ratios of N, O, and Mo in the targets were obtained by combining them;

[0115] 3. The actual density of the molybdenum oxynitride rotary targets prepared in Examples 1 to 7 and Comparative Examples 1 to 6 was tested by the Archimedes density test method, and the relative density was calculated based on the theoretical density;

[0116] 4. The flowability of the granulated powders prepared in Examples 1 to 7 and Comparative Examples 1 to 6 was tested using a Hall flow meter;

[0117] The test results are shown in Table 1 below:

[0118] Table 1

[0119]

[0120] It can be seen from Table 1 that the fluidity of the granulated powder provided in Example 1 is significantly better than that in Comparative Examples 1, 2, and 5, indicating that the present invention improves the performance of the granulated powder by adding nano-MoO 2 Slurry and MoO 2 The powder fluidity can be improved by mixing MoN powder and Mo powder, pressing and sintering them, then ball milling and granulating them.

[0121] The atomic ratio of N, O, and Mo in the molybdenum oxynitride rotary targets prepared in Examples 1 to 7 of the present application is close to the atomic ratio of N, O, and Mo in the raw materials, and the relative density is above 94.2%.

[0122] However, in Comparative Example 1 (without adding nano MoO 2 The atomic ratio of N, O, and Mo in the molybdenum oxynitride rotary target prepared by using the molybdenum oxynitride powder is obviously biased towards the atomic ratio of N, O, and Mo in the raw material, and the relative density is obviously lower than that in Example 1, indicating that the nano MoO 2 The slurry can play a bonding role, promote the molding of the mixture, and make the micron MoO 2 The powder, MoN powder and Mo powder are more tightly combined in physical space, so that the powders are more likely to contact and form a sintering neck during the calcination process, so that the atoms can migrate to the sintering neck area by diffusion to form a more compact calcined powder, avoiding the formation of "hollow" granulated powder by spray granulation, and making the obtained granulated powder have better fluidity, more uniform and denser organizational structure, thereby ensuring that a relatively consistent flight state can be maintained during the spraying process. Therefore, the ratio of each element in the target material is closer to the raw material ratio and the density is higher.

[0123] Comparative Example 2 (without adding nano MoO 2 The atomic ratio of N, O, and Mo in the molybdenum oxynitride rotary target prepared by adding nano MoO 2 Slurry and micron MoO 2The calcined powder with uniform and dense structure can be formed by mixing, molding, crushing and sintering the powder, MoN powder and Mo powder. When it is mixed with the binder, dispersant and water ball mill, the slurry stratification caused by the density difference of each powder can be avoided, so that the slurry is stable, the granulated powder is dense and uniform, and a relatively consistent flight state can be maintained during the spraying process. Therefore, the target material composition is closer to the raw material ratio and the density is higher.

[0124] The atomic ratio of N, O, and Mo in the molybdenum oxynitride rotary target prepared in Comparative Example 3 (without adding Mo powder) deviates significantly from the atomic ratio of N, O, and Mo in the raw material, indicating that the addition of Mo powder in the embodiment of the present application helps the target composition to be closer to the raw material ratio.

[0125] The atomic ratio of N, O, and Mo in the molybdenum oxynitride rotary target prepared in Comparative Example 4 (high calcination temperature) is significantly different from the atomic ratio of N, O, and Mo in the raw material, indicating that the calcination temperature and time of the embodiment of the present application, that is, calcination at a temperature range of 1000-1300°C for 4-6h, can well prevent MoO 2 The powder volatilizes, making the composition of the prepared target material closer to the raw material ratio.

[0126] The atomic ratio of N, O, and Mo in the molybdenum oxynitride rotary target prepared in Comparative Example 5 (high temperature sintering) is significantly different from that in the raw material, and the relative density is significantly lower than that in Example 1, indicating that the present embodiment adopts a spraying process without long-term high temperature sintering, which can effectively prevent MoO 2 Volatilization, so the target material composition is closer to the raw material ratio and the relative density is higher.

[0127] The relative density of the molybdenum oxynitride rotary target prepared in Comparative Example 6 (the particle size of each powder raw material is the same) is significantly lower than that in Example 1, indicating that the present invention uses MoO 2 The particle size of MoO 2 MoN powder is filled into the gaps of Mo powder, so that the powder has a higher packing density in the natural state, which is helpful for static pressure molding, making the powder more tightly combined in the physical space, and it is easier to contact and form a sintering neck during the calcination process, so that the calcined powder formed is more compact, which helps to improve the density of the target material.

[0128] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application should be included in the protection scope of the present application.

Claims

1. A method for preparing a molybdenum oxynitride rotary target, characterized in that: The following steps are involved: The nano MoO2 powder is prepared into nano MoO2 slurry; The nano-MoO2 slurry is mixed with micron MoO2 powder, MoN powder and Mo powder to obtain a mixture; The mixed material is isostatically pressed, crushed and sieved to obtain a mixed powder, wherein the particle size of the mixed powder is 150-250 μm; The mixed powder is placed in a protective atmosphere of argon gas, a pressure of 0.01-0.05 MPa, and a temperature of 1000-1300° C. and sealed and calcined for 4-6 hours to obtain calcined powder; The calcined powder, binder, dispersant and water are mixed by ball milling to obtain a mixed slurry; The mixed slurry is spray-granulated to obtain granulated powder; Degreasing the granulated powder and then sieving it to obtain spray powder; The spray powder is sprayed onto a back tube by using a plasma spraying device, and then machined to obtain a molybdenum oxynitride rotary target; Wherein, the nano MoO2 powder, micron MoO2 powder, MoN powder and Mo powder satisfy the atomic ratio of N, O and Mo of (10-19) / (30-40) / (41-60); The nano MoO2 powder accounts for 2-7% of the total mass of the nano MoO2 powder, micron MoO2 powder, MoN powder and Mo powder; The particle sizes of the micron MoO2 powder, MoN powder and Mo powder are 1-2 μm, 1-2 μm and 4-6 μm respectively.

2. The preparation method according to claim 1, characterized in that The step of degreasing the granulated powder comprises: placing the granulated powder in a vacuum sintering furnace, evacuating the furnace to 10 -2 Pa, then heat to 400~600℃ and keep warm for 6~18h.

3. The preparation method according to claim 2, characterized in that The fluidity of the spray powder is 50-60 s / 50g.

4. The preparation method according to claim 1, characterized in that The plasma spraying equipment comprises a back tube and a spray gun, the distance between the spray gun and the central axis of the back tube is 90-120 mm, the moving speed of the spray gun is 20-80 mm / min, and the powder feeding amount is 60-300 g / min.

5. The preparation method according to claim 4, characterized in that The rotation speed of the back tube is 200-300 r / min, and the temperature of the surface of the back tube is 50-90° C.

6. The preparation method according to any one of claims 1 to 5, characterized in that: The amount of the binder added is 0.5-1% of the total mass of the nano MoO2 powder, micron MoO2 powder, MoN powder and Mo powder; And / or, the added amount of the dispersant is 0.5-1% of the total mass of the nano MoO2 powder, micron MoO2 powder, MoN powder and Mo powder; And / or, the binder is selected from polyvinyl alcohol; And / or, the dispersant is selected from polyethylene glycol.

7. A molybdenum oxynitride rotary target, characterized in that: A molybdenum oxynitride rotary target material obtained by the method for preparing a molybdenum oxynitride rotary target material according to any one of claims 1 to 6; Wherein, the atomic ratio of N, O and Mo in the molybdenum oxynitride rotating target is (10-19) / (30-40) / (41-60).

8. A solar cell, characterized in that: The solar cell comprises a molybdenum oxynitride thin film obtained by sputtering the molybdenum oxynitride rotating target material according to claim 7.